Semiconductor device manufacturing method, substrate processing method, substrate processing device and recording medium

By supplying oxygen and hydrogen to the processing container during the film deposition process in semiconductor devices, the film inside the processing container is oxidized, thus solving the particle problem caused by film accumulation and improving productivity.

CN114318298BActive Publication Date: 2024-11-19KOKUSAI DENKI KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111082924.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-30
Filing Date
2021-09-15
Publication Date
2024-11-19
Estimated Expiration
2041-09-15

AI Technical Summary

Technical Problem

During the film deposition process in semiconductor devices, film accumulation in the processing container leads to particle generation, affecting productivity, and frequent cleaning reduces production efficiency.

Method used

By alternately or simultaneously supplying oxygen-containing gas and hydrogen-containing gas within the treatment container, the membrane inside the treatment container is oxidized to form an oxide film, reducing particle generation and extending the cleaning cycle.

Benefits of technology

It effectively suppressed the generation of particles on the inner membrane of the processing container, extended the cleaning cycle, and improved the productivity of film formation processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114318298B_ABST
    Figure CN114318298B_ABST
Patent Text Reader

Abstract

The present invention is a method for manufacturing a semiconductor device, a substrate processing method, a substrate processing device and a recording medium. By suppressing the generation of particles caused by a film formed in a processing container, the cleaning cycle is extended and the productivity of the film forming process is improved. The present invention has: (a) a process of carrying a substrate into a processing container, (b) a process of performing the following process in the processing container, that is, a process of forming a film on the substrate by alternating or simultaneously performing a process of supplying a raw material gas to the substrate from a first supply unit and a process of supplying a reaction gas to the substrate from a second supply unit for a predetermined number of times, (c) a process of carrying out the processed substrate from the processing container, and (d) a process of oxidizing at least a portion of the film formed in the processing container in (b) to convert it into an oxide film in a state where the processed substrate is carried out from the processing container, wherein in (d), an oxygen-containing gas and a hydrogen-containing gas are supplied to the processing container, and the hydrogen-containing gas is supplied to the first supply unit at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for manufacturing a semiconductor device, a substrate processing method, a substrate processing device, and a recording medium. Background Art

[0002] As one of the manufacturing processes of semiconductor devices, there is a film forming process for forming a film on a substrate in a processing container (for example, refer to Patent Document 1). When the film forming process is performed, a film is also formed in the processing container. Through repeated film forming processes, the film is accumulated in the processing container. If the accumulated film formed in the processing container exceeds the critical film thickness, cracking and film peeling will occur, and particles will be generated, which will become the cause of foreign matter contamination. Therefore, the processing container must be cleaned regularly to remove the accumulated film. However, the film forming process cannot be performed during the cleaning process. When the cleaning frequency is high, that is, when the cleaning cycle is short, the productivity of the film forming process will decrease.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2010-219308 Summary of the invention

[0006] Problems to be solved by the invention

[0007] The present disclosure aims to appropriately suppress the generation of particles caused by a film formed in a processing container, thereby extending a cleaning cycle and improving the productivity of a film forming process.

[0008] Solution to the problem

[0009] According to one embodiment of the present disclosure, there is provided a method for manufacturing a semiconductor device, comprising:

[0010] (a) a step of loading a substrate into a processing container,

[0011] (b) a process of performing the following process in the processing container, i.e., a process of forming a film on the substrate by alternately or simultaneously performing a process of supplying a raw material gas to the substrate from the first supply unit and a process of supplying a reaction gas to the substrate from the second supply unit a predetermined number of times,

[0012] (c) a step of removing the processed substrate from the processing container, and

[0013] (d) a step of oxidizing at least a portion of the film formed in the processing container in (b) to form an oxide film after the processed substrate is removed from the processing container;

[0014] In (d), the oxygen-containing gas and the hydrogen-containing gas are supplied into the processing container and the hydrogen-containing gas is supplied to the first supply unit at the same time.

[0015] Effects of the Invention

[0016] According to the present disclosure, by appropriately suppressing the generation of particles caused by a film formed in a processing container, it is possible to extend a cleaning cycle and improve the productivity of a film forming process. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic configuration diagram of a vertical processing furnace of a substrate processing apparatus that is preferably used in one embodiment of the present disclosure, and is a diagram showing a processing furnace 202 portion in a vertical cross-sectional view.

[0018] Figure 2 This is a schematic diagram of a vertical processing furnace of a substrate processing device suitable for use in one embodiment of the present disclosure. Figure 1 The AA line cross-sectional view shows a portion of the processing furnace 202 .

[0019] Figure 3 1 is a schematic diagram of the configuration of a controller 121 of a substrate processing apparatus preferably used in one embodiment of the present disclosure, and is a block diagram showing a control system of the controller 121 in a block diagram.

[0020] Figure 4 This is a diagram showing a comparison between a process flow in one embodiment of the present disclosure (process flow A) and a process flow in a comparative example (process flow B).

[0021] Figure 5 It is a schematic configuration diagram of a vertical processing furnace of a substrate processing apparatus preferably used in one embodiment of the present disclosure, and is a diagram showing a processing furnace 202 portion in a state where a support member is carried out in a vertical cross-sectional view.

[0022] Figure 6 It is a schematic configuration diagram of a vertical processing furnace of a substrate processing apparatus that is preferably used in Modification 1 of the present disclosure, and shows a processing furnace 202 portion in a vertical cross-sectional view.

[0023] Figure 7 This is a schematic diagram of a vertical processing furnace of a substrate processing device suitable for use in one embodiment of the present disclosure. Figure 1 The AA line cross-sectional view shows a portion in the processing furnace 202 where a large number of films are formed.

[0024] Figure 8 It is a diagram showing the flow of oxidation treatment of deposited film in a furnace in one embodiment of the present disclosure.

[0025] Explanation of symbols

[0026] 200: wafer, 201: processing chamber, 217: wafer box. DETAILED DESCRIPTION

[0027] <One embodiment of the present disclosure>

[0028] Hereinafter, for one embodiment of the present disclosure, reference will be made mainly to Figure 1 to Figure 4 Provide explanation.

[0029] (1) Configuration of substrate processing apparatus

[0030] like Figure 1 As shown, the processing furnace 202 has a heater 207 as a temperature adjuster (heating unit). The heater 207 is cylindrical and is supported by a holding plate and installed vertically. The heater 207 also functions as an activation mechanism (excitation unit) that activates (excites) the gas by heat.

[0031] On the inner side of the heater 207, the reaction tube 203 is arranged concentrically with the heater 207. The reaction tube 203 is made of a heat-resistant material such as quartz (SiO2) or silicon carbide (SiC), and is formed into a cylindrical shape with an upper end closed and a lower end open. Below the reaction tube 203, a header 209 is arranged concentrically with the reaction tube 203. The header 209 is made of a metal material such as stainless steel (SUS), and is formed into a cylindrical shape with an upper end and a lower end open. The upper end of the header 209 is combined with the lower end of the reaction tube 203 to support the reaction tube 203. An O-ring 220a as a sealing member is provided between the upper end of the header 209 and the reaction tube 203. The reaction tube 203 is installed vertically in the same manner as the heater 207. The processing container (reaction container) is mainly composed of the reaction tube 203 and the header 209. The processing chamber 201 is formed in the hollow part of the cylinder of the processing container. The processing chamber 201 is configured to accommodate a wafer 200 as a substrate. The wafer 200 is processed in the processing chamber 201. The wafer 200 includes a product wafer as a product substrate and a test wafer as a test substrate. The test wafer includes a side test wafer arranged at the end of the product wafer arrangement area and a filling test wafer arranged in a portion not filled with the product wafer.

[0032] In the processing chamber 201, nozzles 249a to 249c are respectively provided as supply parts to penetrate the side wall of the manifold 209. The nozzles 249a to 249c are also referred to as the first to third nozzles, respectively. The nozzles 249a to 249c are made of heat-resistant materials such as quartz or SiC, for example. The nozzles 249a to 249c are connected to the gas supply pipes 232a to 232c, respectively. It should be noted that the nozzle 249a is also referred to as the first supply part. In addition, the nozzle 249b is also referred to as the second supply part. In addition, the nozzle 249c is also referred to as the second supply part. That is, a plurality of second supply parts are provided.

[0033] In the gas supply pipes 232a to 232c, mass flow controllers (MFCs) 241a to 241c as flow controllers (flow control units) and valves 243a to 243c as switch valves are respectively arranged in order from the upstream side of the gas flow. On the downstream side of the gas supply pipe 232a from the valve 243a, gas supply pipes 232d and 232g are connected respectively. On the downstream side of the gas supply pipe 232b from the valve 243b, gas supply pipes 232e and 232h are respectively connected. On the downstream side of the gas supply pipe 232c from the valve 243c, gas supply pipes 232f and 232i are connected. In the gas supply pipes 232d to 232i, MFCs 241d to 241i and valves 243d to 243i are respectively arranged in order from the upstream side of the gas flow. The gas supply pipes 232a to 232i are made of metal materials such as SUS, for example.

[0034] like Figure 2 As shown, the nozzles 249a to 249c are respectively arranged in the annular space between the inner wall of the reaction tube 203 and the wafers 200 in a plan view, and stand upright from the lower part to the upper part of the inner wall of the reaction tube 203 toward the arrangement direction of the wafers 200. That is, the nozzles 249a to 249c are respectively arranged along the wafer arrangement area in the area on the side of the wafer arrangement area where the wafers 200 are arranged and horizontally surrounding the wafer arrangement area.

[0035] Compared with nozzles 249b and 249c, nozzle 249a is arranged on the side farther from exhaust port 231a described later. That is, compared with nozzle 249a, nozzles 249b and 249c are arranged on the side closer to exhaust port 231a. In addition, in the plan view, the nozzles 249b and 249c are arranged line-symmetrically with the straight line passing through the center of wafer 200 (that is, the center of reaction tube 203) and the center of exhaust port 231a when wafer 200 is carried into processing chamber 201 as the axis of symmetry. In addition, nozzle 249a as the first supply unit and nozzle 249b as one of the second supply units are arranged to face each other on a straight line with the center of reaction tube 203 sandwiched therebetween. That is, nozzle 249b as one of the nozzles 249b and 249c as the plurality of second supply units is arranged to face (opposite to) nozzle 249a as the first supply unit.

[0036] Gas supply holes 250a to 250c for supplying gas are provided on the side surfaces of the nozzles 249a to 249c. The gas supply holes 250a to 250c are respectively opened toward the center of the reaction tube 203, and can supply gas to the wafer 200. The gas supply holes 250a and 250b are opened opposite to each other (opposite to each other) in a straight line with the center of the wafer 200 (i.e., the center of the reaction tube 203) sandwiched therebetween. A plurality of gas supply holes 250a to 250c are provided from the bottom to the top of the reaction tube 203.

[0037] The source gas is supplied from the gas supply pipe 232 a through the MFC 241 a , the valve 243 a , and the nozzle 249 a into the processing chamber 201 .

[0038] The reaction gas is supplied from the gas supply pipes 232 b and 232 c into the processing chamber 201 via the MFCs 241 b and 241 c , the valves 243 b and 243 c , and the nozzles 249 b and 249 c .

[0039] The cleaning gas is supplied from the gas supply pipe 232 d into the processing chamber 201 via the MFC 241 d , the valve 243 d , the gas supply pipe 232 a , and the nozzle 249 a .

[0040] For example, a gas containing oxygen (O) as an oxidizing gas (oxidant) is supplied from the gas supply pipe 232f into the processing chamber 201 via the MFC 241f, the valve 243f, the gas supply pipe 232c, and the nozzle 249c.

[0041] A gas containing hydrogen (H) as a reducing gas (reducing agent) is supplied from the gas supply pipe 232e via the MFC 241e, the valve 243e, the gas supply pipe 232b, and the nozzle 249b into the processing chamber 201. Although the H-containing gas cannot achieve oxidation by itself, it can react with the O-containing gas under certain conditions to generate oxidizing species such as atomic oxygen (atomic oxygen, O), thereby improving the oxidation treatment efficiency.

[0042] The inert gas is supplied from the gas supply pipes 232g to 232i through the MFCs 241g to 241i, valves 243g to 243i, gas supply pipes 232a to 232c, and nozzles 249a to 249c into the processing chamber 201. The inert gas functions as a purge gas, a carrier gas, a dilution gas, and the like.

[0043] The raw gas supply system is mainly composed of a gas supply pipe 232a, MFC241a, and valve 243a. The reaction gas supply system is mainly composed of gas supply pipes 232b, 232c, MFC241b, 241c, and valves 243b, 243c. The oxidation gas supply system (gas supply system including O) is mainly composed of a gas supply pipe 232f, MFC241f, and valve 243f. The reduction gas supply system (gas supply system including H) is mainly composed of a gas supply pipe 232e, MFC241e, and valve 243e. The cleaning gas supply system is mainly composed of a gas supply pipe 232d, MFC241d, and valve 243d. The inactive gas supply system is mainly composed of gas supply pipes 232g~232i, MFC241g~241i, and valves 243g~243i.

[0044] It should be noted that the raw material gas and the reaction gas may be referred to as film-forming gas, and the raw material gas supply system and the reaction gas supply system may be referred to as film-forming gas supply system. In addition, the O-containing gas and the H-containing gas may be referred to as oxidizing gas, and the O-containing gas supply system and the H-containing gas supply system may be referred to as oxidizing gas supply system.

[0045] Any one or all of the various gas supply systems described above may also be configured as an integrated gas supply system 248 formed by integrating valves 243a to 243i, MFCs 241a to 241i, etc. The integrated gas supply system 248 is configured to be connected to the gas supply pipes 232a to 232i, respectively, and the controller 121 described later controls the operation of supplying various gases into the gas supply pipes 232a to 232i, that is, the opening and closing operation of the valves 243a to 243i, the flow rate adjustment operation performed by the MFCs 241a to 241i, etc. The integrated gas supply system 248 is configured as a single-body or split-type integrated unit, and can be installed and removed relative to the gas supply pipes 232a to 232i, etc. as an integrated unit, and is configured to be able to perform maintenance, replacement, and additional installation of the integrated gas supply system 248 as an integrated unit.

[0046] An exhaust port 231a for exhausting the atmosphere in the processing chamber 201 is provided below the side wall of the reaction tube 203. The exhaust port 231a can also be provided along the lower part to the upper part of the side wall of the reaction tube 203, that is, along the wafer arrangement area. The exhaust port 231a is connected to the exhaust pipe 231. The exhaust pipe 231 is made of a metal material such as SUS. The exhaust pipe 231 is connected to a vacuum pump 246 as a vacuum exhaust device via a pressure sensor 245 as a pressure detector (pressure detection unit) for detecting the pressure in the processing chamber 201 and an APC (Auto Pressure Controller) valve 244 as a pressure regulator (pressure adjustment unit). The APC valve 244 is configured to: by opening and closing the valve when the vacuum pump 246 is in operation, the vacuum exhaust in the processing chamber 201 can be performed and stopped, and further, by adjusting the valve opening based on the pressure information detected by the pressure sensor 245 when the vacuum pump 246 is in operation, the pressure in the processing chamber 201 can be adjusted. The APC valve 244 is also referred to as an exhaust valve. The exhaust system is mainly composed of the exhaust pipe 231, the APC valve 244, and the pressure sensor 245. It is also conceivable to incorporate a vacuum pump 246 into the exhaust system.

[0047] Below the manifold 209, a sealing cap 219 as a furnace cover that can airtightly close the lower end opening of the manifold 209 is provided. The sealing cap 219 is configured to abut against the lower end of the manifold 209 from the lower side in the vertical direction. The sealing cap 219 is made of a metal material such as SUS and is formed in a disc shape. On the upper surface of the sealing cap 219, an O-ring 220b as a sealing member that abuts against the lower end of the manifold 209 is provided. Below the sealing cap 219, a rotating mechanism 267 for rotating the wafer box 217 described later is provided. The rotating shaft 255 of the rotating mechanism 267 is made of a metal material such as SUS, and penetrates the sealing cap 219 and is connected to the wafer box 217. The rotating mechanism 267 is configured to rotate the wafer 200 by rotating the wafer box 217. The sealing cap 219 is configured to be lifted and lowered in the vertical direction by the wafer box elevator 115 as a lifting mechanism provided outside the reaction tube 203. The cassette elevator 115 is configured as a transport device (transport mechanism) that transports the wafer 200 into and out of the processing chamber 201 by raising and lowering the sealing cap 219 .

[0048] A baffle 219 s is provided below the manifold 209 to serve as a furnace cover capable of airtightly closing the lower end opening of the manifold 209 when the sealing cap 219 is lowered to carry out the wafer cassette 217 from the processing chamber 201 . Figure 5The state shown is that the lower end opening of the manifold 209 is closed by the baffle 219s when the sealing cap 219 is lowered and the wafer box 217 is carried out from the processing chamber 201. The baffle 219s is made of a metal material such as SUS and is formed into a disc shape. An O-ring 220c is provided on the upper surface of the baffle 219s as a sealing member that abuts against the lower end of the manifold 209. The opening and closing action (lifting action, rotation action, etc.) of the baffle 219s is controlled by the baffle opening and closing mechanism 115s.

[0049] The wafer box 217, which is a support member for supporting the substrate, is configured to arrange multiple (e.g., 25 to 200) wafers 200 in a horizontal posture and in a mutually aligned state in the vertical direction and support them in multiple stages, that is, arranged at intervals. The wafer box 217 is made of, for example, a heat-resistant material such as quartz or SiC. At the bottom of the wafer box 217, a heat insulation plate 218 made of, for example, a heat-resistant material such as quartz or SiC is supported in multiple stages.

[0050] A temperature sensor 263 as a temperature detector is provided in the reaction tube 203. The temperature in the processing chamber 201 is adjusted to a desired temperature distribution by adjusting the power supply to the heater 207 based on the temperature information detected by the temperature sensor 263. The temperature sensor 263 is provided along the inner wall of the reaction tube 203.

[0051] like Figure 3 As shown, the controller 121 as a control unit (control unit) is configured as a computer having a CPU (Central Processing Unit) 121a, a RAM (Random Access Memory) 121b, a storage device 121c, and an I / O interface 121d. The RAM 121b, the storage device 121c, and the I / O interface 121d are configured to be able to exchange data with the CPU 121a via an internal bus. The controller 121 is connected to an input / output device 122 configured as, for example, a touch panel.

[0052] The storage device 121c is composed of, for example, a flash memory, a HDD (Hard Disk Drive), an SSD (Solid State Drive), etc. The control program for controlling the action of the substrate processing device, the process recipe that records the process and conditions of the later-described processing, etc., are stored in the storage device 121c and can be read out. The process recipe is a combination of the various processes in the later-described processing so that the substrate processing device is executed and a predetermined result is obtained through the controller 121, and functions as a program. Hereinafter, these process recipes, control programs, etc. are also simply collectively referred to as programs. In addition, the process recipe is also simply referred to as a recipe. When the term "program" is used in this specification, sometimes only a single recipe is included, sometimes only a single control program is included, and sometimes both are included. RAM121b is configured as a storage area (working area) for temporarily storing programs, data, etc. read by CPU121a.

[0053] The I / O interface 121d is connected to the above-mentioned MFC241a~241i, valves 243a~243i, pressure sensor 245, APC valve 244, vacuum pump 246, temperature sensor 263, heater 207, rotation mechanism 267, wafer box elevator 115, shutter switch mechanism 115s, etc.

[0054] The CPU 121a is configured to read out a control program from the storage device 121c and execute it, and to read out a recipe from the storage device 121c in response to input of an operation command from the input / output device 122. The CPU 121a is also configured to control, according to the contents of the read-out recipe, the flow rate adjustment operation of various gases by the MFCs 241a to 241h, the opening and closing operation of the valves 243a to 243h, the opening and closing operation of the APC valve 244 and the temperature adjustment operation by the APC valve 244 based on the pressure sensor 245, the rotation and rotation speed adjustment operation of the wafer cassette 217 by the rotation mechanism 267, the lifting and lowering operation of the wafer cassette 217 by the wafer cassette elevator 115, the opening and closing operation of the shutter 219s by the shutter opening and closing mechanism 115s, and the like.

[0055] The controller 121 can be constructed by installing the above-mentioned program stored in the external storage device 123 into the computer. The external storage device 123 includes, for example, a disk such as HDD, an optical disk such as CD, an optical disk such as MO, a USB memory, a semiconductor memory such as SSD, etc. The storage device 121c and the external storage device 123 are constructed as a recording medium that can be read by a computer. Hereinafter, these are also simply collectively referred to as recording media. When the term "recording medium" is used in this specification, sometimes only a separate storage device 121c is included, sometimes only a separate external storage device 123 is included, or sometimes both are included. It should be noted that providing a program to a computer can also be done without using an external storage device 123, but by using communication methods such as the Internet and dedicated lines.

[0056] (2) Processing

[0057] Main Use Figure 4 , Figure 8 The following process flow example is described, that is, using the above-mentioned substrate processing apparatus, as a process of manufacturing a semiconductor device, a process combination (set) including a process of forming a film on a wafer 200 as a substrate in a processing container and a process of oxidizing a part of the film formed in the processing container after the process to form an oxide film is performed a predetermined number of times, preferably a plurality of times. In the following description, the operation of each part constituting the substrate processing apparatus is controlled by the controller 121.

[0058] In the processing flow of this method, the following steps are performed:

[0059] (a) a step of loading the wafer 200 into the processing container,

[0060] (b) a process of performing the following process in the processing container, that is, a process of supplying a raw material gas from the nozzle 249a as the first supply part to the wafer 200 and a process of supplying a reaction gas from the nozzle 249b as the second supply part to the wafer 200 alternately or simultaneously for a predetermined number of times, thereby forming a film on the wafer 200,

[0061] (c) a step of unloading the processed wafer 200 from the processing container, and

[0062] (d) a step of oxidizing at least a portion of the film formed in the processing container in (b) to form an oxide film after the processed wafer 200 is removed from the processing container.

[0063] In (d), the O-containing gas and the H-containing gas are supplied into the processing container, and the H-containing gas is simultaneously supplied to the nozzle 249 a as the first supply unit.

[0064] In (d), it is preferred that the H-containing gas is supplied to the nozzle 249a from a position opposite to the nozzle 249a as the first supply unit. In addition, in (d), it is preferred that the amount of oxidation of the film formed in the nozzle 249a as the first supply unit and its periphery in the processing container is greater than the amount of oxidation of the film formed in the processing container outside the nozzle 249a as the first supply unit and its periphery (for example, the second supply unit and its periphery). That is, in (d), it is preferred that the oxide film formed by oxidizing the film formed in the processing container outside the nozzle 249a as the first supply unit and its periphery is thicker than the oxide film formed by oxidizing the film formed in the processing container outside the nozzle 249a as the first supply unit and its periphery (for example, the second supply unit and its periphery). In addition, in (d), it is preferred that the O-containing gas and the H-containing gas are supplied from any one of the nozzles 249b, 249c as the plurality of second supply units. For example, in (d), it is preferred that the H-containing gas is supplied to the nozzle 249a from the nozzle 249b as the second supply portion which is located at a position opposite to the nozzle 249a as the first supply portion. In this case, in (d), it is preferred that the O-containing gas is supplied from the nozzle 249c as the second supply portion which is located not at a position opposite to the nozzle 249a as the first supply portion. This is particularly effective in the case where, in (a), the film formed on the nozzle 249a as the first supply portion and its periphery in the processing container is thicker than the film formed on the portion other than the nozzle 249a as the first supply portion and its periphery in the processing container (e.g., the second supply portion and its periphery). In addition, this is particularly effective in the case where, in (a), the film formed on the nozzle 249a as the first supply portion and its periphery in the processing container and the film formed on the portion other than the nozzle 249a as the first supply portion and its periphery in the processing container (e.g., the second supply portion and its periphery) are of different compositions. Specifically, for example, this is particularly effective in the following case: in (a), the film formed around the nozzle 249a and its periphery as the first supply part in the processing container contains more elements (for example, silicon-enriched) in the raw material gas than the film formed outside the nozzle 249a and its periphery as the first supply part in the processing container (for example, the second supply part and its periphery).

[0065] In addition, in the process flow of this embodiment, the process combination of (a), (b), (c), and (d) is repeated multiple times. That is, in the process flow of this embodiment, (d) is performed once each time (a), (b), and (c) are performed. That is, in the process flow of this embodiment, (d) is performed once each time a film is formed on the wafer 200 by (a), (b), and (c).

[0066] It should be noted that, hereinafter, as a film, the formation of a nitride film is described as an example. Here, as a nitride film, in addition to a silicon nitride film (SiN film), it also includes a nitride film containing carbon (C), oxygen (O), boron (B), etc. That is, the nitride film includes a silicon nitride film (SiN film), a silicon carbonitride film (SiCN film), a silicon oxynitride film (SiON film), a silicon oxycarbonitride film (SiOCN film), a silicon boron carbon nitride film (SiBCN film), a silicon boron nitride film (SiBN film), a silicon boron oxycarbon nitride film (SiBOCN film), a silicon boron oxynitride film (SiBON film), etc. hereinafter, as a nitride film, the formation of a SiN film is described as an example.

[0067] In addition, the following description will be made by taking the example of carrying out a cycle of a predetermined number of times (m times, m is an integer greater than 1) including the step of supplying a raw material gas to the wafer 200 and the step of supplying a reaction gas to the wafer 200 in (b) as an example. It should be noted that the step of supplying the raw material gas and the step of supplying the reaction gas may be performed alternately, i.e., non-simultaneously, or these steps may be performed simultaneously. The following description will be made by taking the alternation of these steps as an example. In this specification, for convenience, such a gas supply process is also expressed as follows. The same expression method is also used in the description of the following other embodiments, variations, etc.

[0068] (raw material gas → reaction gas) × m

[0069] In addition, the following example is described below: in (d), O-containing gas and H-containing gas are supplied as oxidizing gas into a processing container in a heated state at a pressure less than atmospheric pressure (under reduced pressure) after the processed wafer 200 is unloaded, so that a portion of the film formed in the processing container in (b) is oxidized to become an oxide film, and other portions different from the portion of the film are not oxidized and the film remains as it is.

[0070] In this specification, when the word "wafer" is used, it includes the meaning of "the wafer itself" and the meaning of "a stack of a wafer and a predetermined layer, film, etc. formed on its surface." When the term "wafer surface" is used in this specification, it includes the meaning of "the surface of the wafer itself" and the meaning of "the surface of a predetermined layer, etc. formed on the wafer." In this specification, when it is recorded as "a predetermined layer is formed on the wafer," it includes the meaning of "a predetermined layer is directly formed on the surface of the wafer itself" and the meaning of "a predetermined layer is formed on a layer, etc. formed on the wafer." The word "substrate" in this specification also has the same meaning as the word "wafer."

[0071] (Wafer loading)

[0072] A plurality of wafers 200 are loaded into the wafer box 217 (wafer loading). Then, the shutter 219s is moved by the shutter opening mechanism 115s to open the lower end opening of the manifold 209 (shutter opening). As described above, the wafers 200 include product wafers and test wafers. That is, the product wafers and test wafers as the wafers 200 are loaded into the wafer box 217.

[0073] (Wafer cassette mounted)

[0074] Then, if Figure 1 As shown, the wafer cassette 217 supporting a plurality of wafers 200 is lifted by the wafer cassette elevator 115 and carried into the processing chamber 201 (wafer cassette loading). In this state, the sealing cap 219 closes the lower end of the manifold 209 via the O-ring 220b.

[0075] (Pressure adjustment and temperature adjustment)

[0076] After the wafer box is loaded, the vacuum pump 246 performs vacuum exhaust (decompression exhaust) so that the processing chamber 201 (i.e., the space where the wafer 200 exists) reaches the desired pressure (vacuum degree). At this time, the pressure in the processing chamber 201 is measured by the pressure sensor 245, and the APC valve 244 is feedback controlled (pressure adjusted) based on the measured pressure information. In addition, the heater 207 heats the wafer 200 in the processing chamber 201 so that it reaches the desired temperature. At this time, the power supply of the heater 207 is feedback controlled based on the temperature information detected by the temperature sensor 263 so that the desired temperature distribution (temperature adjustment) is achieved in the processing chamber 201. In addition, the rotating mechanism 26 starts to rotate the wafer 200. The exhaust in the processing chamber 201, the heating and rotation of the wafer 200 are all continued at least until the processing of the wafer 200 is completed.

[0077] (Film forming treatment)

[0078] Then, execute the following steps 1 and 2 in sequence.

[0079] [Step 1]

[0080] In step 1 , a source gas is supplied to the wafer 200 in the processing chamber 201 .

[0081] Specifically, valve 243a is opened to allow raw material gas to flow into gas supply pipe 232a. The raw material gas is adjusted in flow rate by MFC241a, supplied to processing chamber 201 via nozzle 249a, and exhausted from exhaust port 231a. At this time, raw material gas is supplied to wafer 200 (raw material gas supply). At this time, valves 243g to 243i may also be opened to supply inactive gas to processing chamber 201 via nozzles 249a to 249c, respectively.

[0082] The treatment conditions in this step are exemplified as follows:

[0083] Processing temperature (temperature of the wafer 200): 400-700°C, preferably 500-650°C,

[0084] Processing pressure (pressure in the processing chamber 201): 1 to 2666 Pa, preferably 67 to 1333 Pa,

[0085] Raw material gas supply flow rate: 0.01 to 2 slm, preferably 0.1 to 1 slm,

[0086] Raw material gas supply time: 1 to 120 seconds, preferably 1 to 60 seconds,

[0087] Inert gas supply flow rate (each gas supply pipe): 0~10slm

[0088] It should be noted that the representation of a numerical range such as "1 to 2666 Pa" in this specification means that the range includes a lower limit and an upper limit. Therefore, for example, "1 to 2666 Pa" means "above 1 Pa and below 2666 Pa". The same applies to other numerical ranges. In addition, the "processing temperature" in this specification refers to the temperature of the wafer 200 or the temperature in the processing chamber 201, and the "processing pressure" refers to the pressure in the processing chamber 201. In addition, a gas supply flow rate of 0 sccm means that the gas is not supplied. This is also the case in the following descriptions.

[0089] By supplying a raw material gas such as a chlorosilane-based gas to the wafer 200 under the above conditions, a Si-containing layer containing Cl is formed on the outermost surface of the wafer 200 serving as a substrate. The Si-containing layer containing Cl is formed by physical adsorption and chemical adsorption of chlorosilane-based gas molecules on the outermost surface of the wafer 200, physical adsorption and chemical adsorption of molecules of a substance after decomposition of a part of the chlorosilane-based gas on the outermost surface of the wafer 200, and accumulation of Si on the outermost surface of the wafer 200 due to thermal decomposition of the chlorosilane-based gas. The Si-containing layer containing Cl may be an adsorption layer (physical adsorption layer, chemical adsorption layer) of molecules of chlorosilane-based gas or molecules of a substance after decomposition of a part of the chlorosilane-based gas, or may be a stack of Si containing Cl. In this specification, the Si-containing layer containing Cl is also referred to as the Si-containing layer for short.

[0090] After the Si-containing layer is formed, the valve 243a is closed to stop supplying the raw material gas into the processing chamber 201. Then, the processing chamber 201 is evacuated to remove (purge) the residual gas in the processing chamber 201. At this time, the valves 243g to 243i are opened to supply an inert gas into the processing chamber 201. The inert gas functions as a purge gas.

[0091] As the raw material gas, for example, a silane-based gas containing silicon (Si) as a main element constituting the film formed on the wafer 200 can be used. As the silane-based gas, for example, a gas containing Si and a halogen, that is, a halosilane-based gas can be used. Halogen includes chlorine (Cl), fluorine (F), bromine (Br), iodine (I), etc. As the halosilane-based gas, for example, the above-mentioned chlorosilane-based gas containing Si and Cl can be used.

[0092] As the raw material gas, for example, chlorosilane-based gases such as monochlorosilane (SiH3Cl, abbreviated as MCS) gas, dichlorosilane (SiH2Cl2, abbreviated as DCS) gas, trichlorosilane (SiHCl3, abbreviated as TCS) gas, tetrachlorosilane (SiCl4, abbreviated as STC) gas, hexachlorodisilane (Si2Cl6, abbreviated as HCDS) gas, and octachlorotrisilane (Si3Cl8, abbreviated as OCTS) gas can be used. As the raw material gas, one or more of these can be used.

[0093] As the raw material gas, in addition to the chlorosilane gas, for example, fluorosilane gas such as tetrafluorosilane (SiF4) gas and difluorosilane (SiH2F2) gas, bromosilane gas such as tetrabromosilane (SiBr4) gas and dibromosilane (SiH2Br2) gas, iodosilane gas such as tetraiodosilane (SiI4) gas and diiodosilane (SiH2I2) gas can also be used. As the raw material gas, one or more of these can be used.

[0094] As the raw material gas, in addition to these, for example, a gas containing Si and an amino group, i.e., an aminosilane-based gas, can also be used. The amino group is a monovalent functional group obtained by removing hydrogen (H) from ammonia, primary ammonia, or secondary ammonia, and can be represented by -NH2, -NHR, or -NR2. It should be noted that R represents an alkyl group, and the two Rs of -NR2 can be the same or different.

[0095] As the raw material gas, for example, aminosilane-based gases such as tetrakis(dimethylamino)silane (Si[N(CH3)2]4, abbreviated as: 4DMAS) gas, tris(dimethylamino)silane (Si[N(CH3)2]3H, abbreviated as: 3DMAS) gas, bis(diethylamino)silane (Si[N(C2H5)2]2H2, abbreviated as: BDEAS) gas, bis(tert-butylamino)silane (SiH2[NH(C4H9)]2, abbreviated as: BTBAS) gas, and (diisopropylamino)silane (SiH3[N(C3H7)2], abbreviated as: DIPAS) gas can be used. As the raw material gas, one or more of these can be used.

[0096] As the inert gas, for example, inert gases such as nitrogen (N2) gas, argon (Ar) gas, helium (He) gas, neon (Ne) gas, and xenon (Xe) gas can be used. As the inert gas, one or more of these can be used. This also applies to each step described later.

[0097] [Step 2]

[0098] After step 1 is completed, a reaction gas is supplied to the wafer 200 in the processing chamber 201 , that is, the Si-containing layer formed on the wafer 200 .

[0099] Specifically, valves 243b and 243c are opened, and reaction gases flow into gas supply pipes 232b and 232c, respectively. The reaction gases are adjusted in flow rate by MFCs 241b and 241c, respectively, and are supplied to the processing chamber 201 through nozzles 249b and 249c, respectively, and exhausted by exhaust port 231a. At this time, reaction gases are supplied to the wafer 200 (reaction gas supply). At this time, valves 243g to 243i may also be opened, and inactive gases may be supplied to the processing chamber 201 through nozzles 249a to 249c, respectively. It should be noted that, at this time, reaction gases may be supplied from nozzle 249b instead of nozzle 249c, or reaction gases may be supplied from nozzle 249c instead of nozzle 249b. That is, it is sufficient to supply reaction gases from at least one of nozzles 249b and 249c.

[0100] The treatment conditions in this step are exemplified as follows:

[0101] Processing temperature (temperature of the wafer 200): 400-700°C, preferably 500-650°C,

[0102] Processing pressure (pressure in the processing chamber 201): 1 to 4000 Pa, preferably 1 to 3000 Pa,

[0103] Reaction gas supply flow rate: 0.1~10slm,

[0104] Reaction gas supply time: 1 to 120 seconds, preferably 1 to 60 seconds.

[0105] The other treatment conditions are the same as those in step 1.

[0106] By supplying a gas containing nitrogen (N) and hydrogen (H) as a reaction gas to the wafer 200 under the above conditions, at least a portion of the Si-containing layer formed on the wafer 200 can be nitrided (modified). As a result, a silicon nitride layer (SiN layer) as a layer containing Si and N is formed on the outermost surface of the wafer 200 as a base. When the SiN layer is formed, impurities such as Cl contained in the Si-containing layer constitute a gaseous substance containing at least Cl during the modification reaction of the Si-containing layer by the gas containing N and H, and are discharged from the processing chamber 201. As a result, the SiN layer becomes a layer with less impurities such as Cl than the Si-containing layer formed in step 1.

[0107] After the SiN layer is formed, valves 243b and 243c are closed to stop supplying the reaction gas into the processing chamber 201. Then, the gas remaining in the processing chamber 201 is exhausted (purged) from the processing chamber 201 by the same process as the purging in step 1.

[0108] As the reaction gas, for example, a nitriding gas (nitriding agent) can be used. As the nitriding gas, for example, the above-mentioned gas containing N and H can be used. Since the gas containing N and H is a N-containing gas, it is also a H-containing gas. The gas containing N and H preferably contains an NH bond.

[0109] As the reaction gas, for example, ammonia (NH 3 ) gas, diimide (N 2 H 2 ) gas, hydrazine (N 2 H 4 ) gas, N 3 H 8 gas or other hydrogen nitride-based gas can be used. As the reaction gas, one or more of these can be used.

[0110] As the reaction gas, in addition to the above, a gas containing nitrogen (N), carbon (C) and hydrogen (H) can be used. As the gas containing N, C and H, for example, an amine gas or an organic hydrazine gas can be used. The gas containing N, C and H is a gas containing N, a gas containing C, a gas containing H, or a gas containing N and C.

[0111] As the reaction gas, for example, ethylamine gases such as monoethylamine (C2H5NH2, abbreviated as MEA) gas, diethylamine ((C2H5)2NH, abbreviated as DEA) gas, triethylamine ((C2H5)3N, abbreviated as TEA) gas, methylamine gases such as monomethylamine (CH3NH2, abbreviated as MMA) gas, dimethylamine ((CH3)2NH, abbreviated as DMA) gas, trimethylamine ((CH3)3N, abbreviated as TMA) gas, monomethylhydrazine ((CH3)HN2H2, abbreviated as MMH) gas, dimethylhydrazine ((CH3)2N2H2, abbreviated as DMH) gas, trimethylhydrazine ((CH3)2N2(CH3)H, abbreviated as TMH) gas and other organic hydrazine gases can be used. As the reaction gas, one or more of these can be used.

[0112] [Perform the loop a predetermined number of times]

[0113] By performing the above-mentioned steps 1 and 2 non-simultaneously, i.e., non-synchronously, for a predetermined number of times (m times, m being an integer greater than 1), a predetermined thickness film, such as a SiN film of predetermined thickness, can be formed on the substrate using the surface of the wafer 200 as a substrate. The above-mentioned cycle is preferably repeated multiple times. That is, it is preferred that the thickness of the SiN layer formed in each cycle is thinner than the desired film thickness, and the above-mentioned cycle is repeated multiple times until the thickness of the SiN film formed by stacking SiN layers reaches the desired thickness. It should be noted that when a gas containing N, C and H is used as a reaction gas, for example, a silicon carbonitride layer (SiCN layer) can also be formed as a second layer, and by performing the above-mentioned cycle a predetermined number of times, for example, a silicon carbonitride film (SiCN film) can also be formed as a film on the surface of the wafer 200.

[0114] It should be noted that during the film forming process, a deposit containing a SiN film is formed in the process container, for example, on the inner wall of the process container (i.e., the inner wall of the reaction tube 203, the inner wall of the manifold 209, the surface of the nozzles 249a to 249c, the surface of the wafer box 217, etc.). Figure 7 The deposit containing SiN film formed in the shown area 500 (i.e., the nozzle 249a and its surrounding area serving as the first supply part in the processing container) becomes Si-enriched and thicker than the deposit containing SiN film formed in the part outside the above-mentioned area in the processing container (e.g., the second supply part and its surrounding area).

[0115] (Post-purge and atmospheric pressure recovery)

[0116] After the process of forming a SiN film of a desired thickness on the wafer 200 is completed, an inactive gas as a purge gas is supplied from the nozzles 249a to 249c to the process chamber 201, and the gas is exhausted from the exhaust port 231a. Thus, the process chamber 201 is purged, and the residual gas, reaction by-products, etc. in the process chamber 201 are removed from the process chamber 201 (post-purge). Then, the atmosphere in the process chamber 201 is replaced with an inactive gas (inactive gas replacement), and the pressure in the process chamber 201 is restored to normal pressure (atmospheric pressure restoration).

[0117] (Wafer Cassette Unloading)

[0118] Then, the sealing cap 219 is lowered by the wafer box elevator 115 to open the lower end of the manifold 209. Then, the processed wafers 200 are carried out from the lower end of the manifold 209 to the outside of the reaction tube 203 while being supported by the wafer box 217 (wafer box unloading). Figure 5 As shown, the baffle 219s is moved, and the lower end opening of the manifold 209 is closed by the baffle 219s via the O-ring 220c (closing the baffle).

[0119] (Wafer Cooling)

[0120] After the wafer cassette is unloaded, that is, after the shutter is closed, the processed wafers 200 are cooled to a predetermined temperature to be taken out while being supported by the wafer cassette 217 (wafer cooling).

[0121] (Wafer Release)

[0122] After the wafers are cooled, the processed wafers 200 cooled to a predetermined temperature at which they can be taken out are taken out from the wafer cassette 217 (wafer release).

[0123] (Oxidation treatment of film deposited in the furnace)

[0124] In parallel with the wafer cooling and wafer release, an oxidation treatment is performed on the film attached to the furnace during the film forming process (i.e., a deposit including a SiN film formed in the process container during the film forming process). The oxidation treatment performed on the SiN film formed in the process container is to perform unsaturated oxidation of the SiN film, that is, unsaturated oxidation.

[0125] That is, after the wafer box is unloaded and the shutter is closed, Figure 5 In the state of cooling the wafer and releasing the wafer, O-containing gas and H-containing gas are simultaneously supplied as oxidizing gas into the processing container in the reduced pressure state (less than atmospheric pressure) after the processed wafer 200 is unloaded. It should be noted that the processing container is in the reduced pressure state and is also in the heated state. Thus, a part of the SiN film formed in the processing container during the film forming process can be oxidized and converted into a SiO film, and other parts of the SiN film different from the part are not oxidized and remain the original state of the SiN film.

[0126] Specifically, after closing the baffle, the valves 243f and 243e are opened, and the O-containing gas and the H-containing gas flow into the gas supply pipes 232f and 232e, respectively. The O-containing gas and the H-containing gas flowing in the gas supply pipes 232f and 232e are adjusted in flow rate by the MFCs 241f and 241e, respectively, and are supplied to the processing chamber 201 through the nozzles 249c and 249b. The O-containing gas and the H-containing gas are mixed and reacted in the processing chamber 201, and then exhausted from the exhaust port 231a. At this time, an oxidizing species containing oxygen such as atomic oxygen generated by the reaction of the O-containing gas and the H-containing gas but not containing water (H2O) is supplied to the SiN film formed in the processing container (supply of O-containing gas + H-containing gas). At this time, the valves 243g to 243i may also be opened to supply an inactive gas into the processing chamber 201 through the nozzles 249a to 249c.

[0127] The treatment conditions in this step are exemplified as follows:

[0128] Processing temperature (temperature in the processing chamber 201): 400 to 800°C, preferably 600 to 700°C,

[0129] Processing pressure (pressure in the processing chamber 201): 1 to 2000 Pa, preferably 1 to 1000 Pa,

[0130] O-containing gas supply flow rate: 0.1~10slm,

[0131] H-containing gas supply flow rate: 0.1~15slm,

[0132] Inert gas supply flow rate (per gas supply pipe): 0~10slm,

[0133] Each gas supply time: 15 to 60 minutes.

[0134] The ratio of the H-containing gas (H-containing gas supply flow rate / (H-containing gas supply flow rate+O-containing gas supply flow rate)), that is, the concentration of the H-containing gas is preferably 50 to 60%.

[0135] By supplying an O-containing gas and a H-containing gas to the SiN film formed in the processing container under the above conditions, a portion of the SiN film formed in the processing container is oxidized to become a SiO film by utilizing the strong oxidizing power of oxidizing species such as atomic oxygen, while other portions of the SiN film different from the portion are not oxidized and remain the original state of the SiN film. For example, a portion of the surface side of the SiN film formed in the processing container can be oxidized to become a SiO film, while other portions of the SiN film different from the portion on the surface side (portions on the side opposite to the surface side) are not oxidized and remain the original state of the SiN film.

[0136] It should be noted that when a part of the SiN film formed in the processing container is transformed into a SiO film by oxidation, it expands due to the incorporation of O. Therefore, the SiO film obtained by oxidizing a part of the SiN film formed in the processing container becomes thicker than a part of the SiN film formed in the processing container before oxidation (a part of the SiN film that can be oxidized). The thickness of the SiO film obtained by oxidizing a part of the SiN film formed in the processing container sometimes increases to a thickness of about 1.4 to 1.5 times the thickness of the part of the SiN film formed in the processing container before oxidation.

[0137] Thus, the total thickness of the stacked structure of the SiO film obtained by oxidizing a portion of the SiN film formed in the processing container and the SiN film maintained without being oxidized in the SiN film formed in the processing container, that is, the stacked film (hereinafter also referred to as SiO / SiN stacked film) becomes thicker than the thickness of the SiN film formed in the processing container before oxidation.

[0138] In addition, the stress (film stress, internal stress, residual stress) possessed by the SiN film formed in the processing container is tensile stress, while the stress possessed by the SiO film obtained by oxidizing a portion of the SiN film formed in the processing container is compressive stress. If tensile stress is represented as "+" and compressive stress is represented as "-", the stress possessed by the SiN film formed in the processing container sometimes reaches, for example, +1.0 to +1.5 GPa, and the stress possessed by the SiO film obtained by oxidizing a portion of the SiN film formed in the processing container sometimes reaches, for example, -0.3 to -0.5 GPa.

[0139] Thus, the total stress of the stacked film of the SiO film obtained by oxidizing a part of the SiN film formed in the processing container and the SiN film that is not oxidized and maintained in the SiN film formed in the processing container, that is, the SiO / SiN stacked film, becomes smaller than the stress of the SiN film before oxidation formed in the processing container. This is because the tensile stress of the SiN film in the SiO / SiN stacked film and the compressive stress of the SiO film cancel each other out. By adjusting the thickness of the SiN film and the SiO film in the SiO / SiN stacked film, the stress balance of the tensile stress of the SiN film in the SiO / SiN stacked film and the compressive stress of the SiO film can be adjusted, and these stresses can also be offset. That is, by adjusting the stress balance, the total stress of the SiO / SiN stacked film can be made close to zero, and then the stress can be made zero. In this way, by reducing the stress of the film formed in the processing container, the generation of particles caused by the film formed in the processing container can be suppressed.

[0140] It should be noted that, from the perspective of suppressing the generation of particles caused by the film formed in the processing container, the total stress of the SiO / SiN stacked film is preferably close to zero, but in this case, the oxidation treatment of the SiN film formed in the processing container takes time. Figure 4 As shown in the process flow B, the oxidation treatment time (i.e., the oxidation treatment time of the deposited film in the furnace) may exceed the total time of the wafer cooling time and the wafer release time. Figure 4 In the process flow B shown, there is a time when only the oxidation process of the deposited film in the furnace is performed, that is, a standby time when the wafer is not cooled or released. In this case, the time when the film forming process cannot be performed (that is, the downtime of the substrate processing device) becomes longer, which sometimes affects the productivity of the film forming process.

[0141] In addition, although there is also a method of converting all SiN films into SiO films by oxidizing all SiN films formed in the processing container, that is, by saturating the oxidation of the SiN film formed in the processing container, in this case, the oxidation treatment of the SiN film formed in the processing container is more time-consuming, and the oxidation treatment time (that is, the oxidation treatment time of the attached film in the furnace) sometimes greatly exceeds the total time of the wafer cooling time and the wafer release time. In this case, the time when the film forming process cannot be performed, that is, the downtime of the substrate processing device will become longer, and sometimes the productivity of the film forming process will be greatly affected. It should be noted that when the SiN film formed in the processing container is saturatedly oxidized to convert the SiN film into a SiO film, the stress of the converted SiO film is a compressive stress.

[0142] On the other hand, if the total stress of the SiO / SiN stacked film is not set to zero or compressive stress, but to a tensile stress smaller than the stress (tensile stress) of the SiN film before oxidation formed in the processing container, the oxidation treatment time of the SiN film formed in the processing container can be shortened, such as Figure 4As shown in the process flow A, the oxidation treatment time of the SiN film formed in the processing container (i.e., the oxidation treatment time of the attached film in the furnace) can be made less than the total time of the wafer cooling time and the wafer release time. In this case, the time when the film forming process cannot be performed does not change compared with when the oxidation treatment of the attached film in the furnace is not performed, and the productivity of the film forming process will not be affected. It should be noted that the author of the present application has found that even when the total stress of the SiO / SiN stacked film is not zero, but a tensile stress smaller than the stress (tensile stress) of the SiN film before oxidation formed in the processing container, the effect of suppressing particle generation can be obtained. That is, by making the total stress of the SiO / SiN stacked film a tensile stress smaller than the stress of the SiN film before oxidation formed in the processing container, the effect of suppressing particle generation can be produced, and the productivity of the film forming process can be maintained. It should be noted that if the oxidation treatment time of the attached film in the furnace is further shortened and the total time of the wafer cooling time and the wafer release time is correspondingly shortened, the productivity of the film forming process can also be improved.

[0143] It should be noted that the author of the present application has found that by making the ratio of the SiO film in the SiO / SiN stacked film 75% or less, preferably 70% or less, that is, by making the ratio of the SiN film in the SiO / SiN stacked film 25% or more, preferably 30% or more, the total stress of the SiO / SiN stacked film can be made into a tensile stress smaller than the stress (tensile stress) of the SiN film before oxidation formed in the processing container, and the same effect as the above effect can be obtained. In addition, the author of the present application has found that when the ratio of the SiO film in the SiO / SiN stacked film formed in the oxidation treatment of the deposited film in the furnace exceeds 75%, the total stress of the SiO / SiN stacked film becomes a compressive stress.

[0144] In addition, the inventors of the present application have discovered that by making the thickness of the oxidized portion of the SiN film formed in the processing container less than 65%, preferably less than 60%, of the thickness of the SiN film before oxidation formed in the processing container, that is, by making the thickness of the portion of the SiN film formed in the processing container that is not oxidized and remains the SiN film original less than 35%, preferably more than 40%, of the thickness of the SiN film before oxidation formed in the processing container, the total stress of the SiO / SiN stacked film can be made a tensile stress smaller than the stress (tensile stress) of the SiN film before oxidation formed in the processing container, thereby obtaining the same effect as the above-mentioned effect.

[0145] In addition, the author of the present application has discovered that by making the thickness of the oxidized portion of the SiN film formed in the processing container thinner than the thickness of the portion of the SiN film formed in the processing container that is not oxidized and remains the SiN film as it is, the total stress of the SiO / SiN stacked film can be easily made a tensile stress smaller than the stress (tensile stress) of the SiN film before oxidation formed in the processing container, thereby reliably obtaining the same effect as the above-mentioned effect.

[0146] It should be noted that, as described above, in the SiN film formed in the processing container, Figure 7 The SiN film formed in the region 500 shown, i.e., the nozzle 249a as the first supply unit and the surrounding region in the processing container, is Si-enriched and thicker than the SiN film formed in the portion other than the above region in the processing container. Therefore, the risk of particle generation caused by the SiN film formed in the region 500 in the processing container is higher than the risk of particle generation caused by the SiN film formed in the portion other than the region 500 in the processing container.

[0147] In contrast, in this embodiment, when the oxidation treatment of the deposited film in the furnace is performed, the H-containing gas is supplied from the nozzle 249b as the second supply portion located at a position opposite to the nozzle 249a as the first supply portion toward the nozzle 249a. More specifically, the O-containing gas is supplied from the nozzle 249c as the second supply portion located not opposite to the nozzle 249a as the first supply portion, and the H-containing gas is supplied from the nozzle 249b as the second supply portion located at a position opposite to the nozzle 249a as the first supply portion toward the nozzle 249a, that is, toward the region 500.

[0148] Thus, when the oxidation treatment of the film deposited in the furnace is performed, the oxidation amount of the SiN film formed in the region 500 in the processing container can be made greater than the oxidation amount of the SiN film formed in the portion other than the region 500 in the processing container. That is, when the oxidation treatment of the film deposited in the furnace is performed, the SiO film formed by oxidizing the SiN film formed in the region 500 in the processing container can be made thicker than the SiO film formed by oxidizing the SiN film formed in the portion other than the region 500 in the processing container. Moreover, thereby, the stress of the Si-rich SiN film formed in the region 500 in the processing container where the risk of particle generation is relatively high can be appropriately controlled (relaxed) to be the same as the stress of the SiN film formed in the portion other than the region 500 in the processing container, and in particular, the generation of particles caused by the SiN film formed in the region 500 in the processing container can be suppressed. It should be noted that in this case, by making the supply flow rate of the H-containing gas greater than the supply flow rate of the O-containing gas, the above-mentioned effect can be further enhanced.

[0149] It should be noted that, when the oxidation treatment of the film attached in the furnace is performed, the processing container may be pulsed exhausted (intermittently exhausted) while the O-containing gas and the H-containing gas are continuously supplied to the processing container. That is, when the oxidation treatment of the film attached in the furnace is performed, the exhaust in the processing container may be stopped and the exhaust in the processing container may be alternately performed a predetermined number of times (preferably repeated multiple times) while the O-containing gas and the H-containing gas are continuously supplied to the processing container.

[0150] Specifically, when the oxidation treatment of the deposited film in the furnace is carried out, the following Figure 8 As shown, the APC valve 244 as the exhaust valve is opened and closed a predetermined number of times (n times, n is an integer greater than or equal to 1) while the O-containing gas and the H-containing gas are continuously supplied to the processing container. That is, when the oxidation treatment of the film deposited in the furnace is performed, the process of supplying the O-containing gas and the H-containing gas to the processing container with the APC valve 244 closed and the process of supplying the O-containing gas and the H-containing gas to the processing container with the APC valve 244 open may be alternately performed as one cycle, and the cycle may be performed a predetermined number of times (n times, n is an integer greater than or equal to 1). That is, when the oxidation treatment of the film deposited in the furnace is performed, the process of supplying the O-containing gas and the H-containing gas to the processing container with the exhaust in the processing container stopped and the process of supplying the O-containing gas and the H-containing gas to the processing container with the exhaust in the processing container may be alternately performed as one cycle, and the cycle may be performed a predetermined number of times (n times, n is an integer greater than or equal to 1). Figure 8 An example of repeating these cycles multiple times is shown. It should be noted that when the APC valve 244 is opened, the exhaust pipe 231 is opened, and when the APC valve 244 is closed, the exhaust pipe 231 is blocked. In these cases, that is, when the O-containing gas and the H-containing gas are continuously supplied to the processing container, it is preferred to maintain the processing container in a decompressed state when the APC valve 244 is opened and closed a predetermined number of times.

[0151] It should be noted that in this case, if Figure 8 As shown, the APC valve 244 as the exhaust valve is preferably kept closed for a longer time than the APC valve 244 is kept open. That is, the exhaust stop state in the processing container is preferably kept longer than the exhaust state in the processing container.

[0152] In addition, the O-containing gas and the H-containing gas may be supplied to the processing container not only continuously but also intermittently. When the O-containing gas and the H-containing gas are supplied to the processing container intermittently, it is preferred that at least a portion of the period during which the APC valve 244 is closed (i.e., the period during which exhaust in the processing container is stopped) overlaps with at least a portion of the period during which the O-containing gas and the H-containing gas are supplied to the processing container.

[0153] like Figure 2 , Figure 7 As shown, the nozzles 249c and 249b as the second supplying parts are both arranged near the exhaust port 231a, and the O-containing gas and the H-containing gas supplied from the nozzles 249c and 249b are sometimes exhausted from the exhaust port 231a before they travel to the part of the processing container, for example, on the opposite side of the exhaust port 231a. In the state where the O-containing gas and the H-containing gas are continuously or intermittently supplied to the processing container, by opening and closing the APC valve 244 a predetermined number of times (n times, n is an integer greater than 1), the timing and frequency of closing the APC valve 244 can be increased, and the O-containing gas and the H-containing gas can be sufficiently traveled (entered, diffused) to the part of the processing container, for example, on the opposite side of the exhaust port 231a. In addition, the O-containing gas and the H-containing gas can also be sufficiently traveled (entered, diffused) to the region 500 in the processing container. As a result, the SiN film formed in the part of the processing container, for example, on the opposite side of the exhaust port 231a, can be sufficiently oxidized. In addition, the SiN film formed in the region 500 in the processing container can also be sufficiently oxidized. That is, the SiN film formed in the processing container can be uniformly and sufficiently oxidized. It should be noted that the positional relationship between the nozzles 249c, 249b and the exhaust port 231a is not limited to the following. Figure 2 , Figure 7 As shown, even with Figure 2 The same effect can be achieved with different position relationships.

[0154] It should be noted that in this case, if Figure 8 As shown, by making the time for which the APC valve 244 serving as the exhaust valve is maintained in the closed state longer than the time for which the APC valve 244 is maintained in the open state longer, the period (time) during which the APC valve 244 is closed can be made longer. That is, by making the time during which the exhaust in the processing container is kept stopped longer than the time during which the exhaust in the processing container is maintained in the exhaust state longer, the period (time) during which the APC valve 244 is closed can be made longer. As a result, the O-containing gas and the H-containing gas can be made to more fully travel to the portion in the processing container, for example, the opposite side of the exhaust port 231a, and the SiN film formed in the portion in the processing container, for example, the opposite side of the exhaust port 231a, can be more fully oxidized. In addition, the SiN film formed in the region 500 in the processing container can also be more fully oxidized. As a result, the necessary and sufficient oxidation treatment can be more uniformly performed on the SiN film formed in the processing container. It should be noted that in this case, Figure 8 As shown, it is preferable to maintain the APC valve 244 as an exhaust valve in a fully closed state ( Figure 8 The time of maintaining the APC valve 244 in the fully open state ( Figure 8Thus, the above-mentioned effect can be obtained more fully.

[0155] It should be noted that Figure 8 The example shown in FIG. 1 is: from the closed state of the APC valve 244 as an exhaust valve ( Figure 8 The closed state in the APC valve 244 is changed to the open state ( Figure 8 During the process of the APC valve 244 being substantially closed, the APC valve 244 is slightly opened to slightly exhaust the inside of the processing container. That is, Figure 8 The example shown in FIG. 1 is that in the process of changing from the state of stopping exhaust in the processing container to the state of exhausting the processing container, a period of slightly exhausting the processing container is set while maintaining the state of substantially stopping exhaust in the processing container. The reason for setting the period of slightly exhausting the processing container while maintaining the substantially closed state of the APC valve 244, that is, maintaining the state of substantially stopping exhaust in the processing container, is to suppress the excessive increase in pressure in the processing container. Thus, the decrease in oxidation efficiency caused by excessive increase in pressure in the processing container can be suppressed. It should be noted that in this specification, the situation of slightly exhausting the processing container while maintaining the substantially closed state of the APC valve 244, that is, maintaining the state of substantially stopping exhaust in the processing container, is also referred to as "the state of closing the APC valve 244", that is, "the state of closing the exhaust valve". In addition, in this specification, the situation of slightly exhausting the processing container while maintaining the substantially closed state of the APC valve 244, that is, maintaining the state of substantially stopping exhaust in the processing container, is also referred to as "the state of stopping exhaust in the processing container".

[0156] It should be noted that if Figure 8 As shown in FIG. 1 , by making the time for which the APC valve 244 as the exhaust valve is kept in the closed state longer than the time for which the APC valve 244 is kept in the open state longer, the time for which the pressure in the processing container is increased can be made longer than the time for which the pressure in the processing container is decreased. That is, by making the time for which the pressure in the processing container is increased longer than the time for which the pressure in the processing container is decreased, the above-mentioned effect can also be obtained.

[0157] As Figure 8 The treatment conditions for the oxidation treatment of the deposited film in the furnace shown are exemplified as follows:

[0158] Processing temperature (temperature in the processing chamber 201): 400 to 800°C, preferably 600 to 700°C,

[0159] Processing pressure (pressure in the processing chamber 201): 1 to 2000 Pa, preferably 1 to 1000 Pa,

[0160] O-containing gas supply flow rate: 0.1~10slm,

[0161] H-containing gas supply flow rate: 0.1~15slm,

[0162] Inert gas supply flow rate (per gas supply pipe): 0~10slm,

[0163] Exhaust valve closing time: 2 to 60 seconds, preferably 10 to 50 seconds, more preferably 20 to 40 seconds,

[0164] Exhaust valve opening time: 0.5 to 50 seconds, preferably 2 to 30 seconds, more preferably 5 to 10 seconds,

[0165] Exhaust valve opening and closing times: 1 to 100 times, preferably 2 to 80 times, more preferably 10 to 50 times.

[0166] The ratio of the H-containing gas (H-containing gas supply flow rate / (H-containing gas supply flow rate+O-containing gas supply flow rate)), that is, the concentration of the H-containing gas is preferably 50 to 60%.

[0167] As the O-containing gas, for example, oxygen (O2) gas, ozone (O3) gas, water vapor (H2O gas), hydrogen peroxide (H2O2) gas, nitrous oxide (N2O) gas, nitric oxide (NO) gas, nitrogen dioxide (NO2) gas, carbon monoxide (CO) gas, carbon dioxide (CO2) gas, etc. can be used. As the O-containing gas, one or more of these can be used.

[0168] As the H-containing gas, for example, hydrogen (H2) gas, deuterium ( 2 H2) gas, etc. 2 H2 gas is called D2 gas. As H-containing gas, one or more of these can be used. It should be noted that in this step, it is also possible to supply O-containing gas alone as oxidizing gas without supplying H-containing gas.

[0169] In addition, in this step, at least one of the O-containing gas and the H-containing gas may be supplied by plasma excitation. For example, plasma-excited O2 gas and non-plasma-excited H2 gas may be supplied, non-plasma-excited O2 gas and plasma-excited H2 gas may be supplied, or plasma-excited O2 gas and plasma-excited H2 gas may be supplied. In addition, plasma-excited O2 gas may be supplied alone without supplying the H-containing gas. Thus, the oxidation treatment time can be further shortened.

[0170] After the oxidation treatment of the film attached in the furnace is completed, the valves 243f and 243e are closed to stop supplying the O-containing gas and the H-containing gas into the processing chamber 201. Then, the inactive gas as the purge gas is supplied into the processing chamber 201 from the nozzles 249a to 249c, respectively, and the gas is exhausted from the exhaust port 231a. Thus, the processing chamber 201 is purged, and the residual gas, reaction by-products, etc. in the processing chamber 201 are removed from the processing chamber 201 (purge). Then, the atmosphere in the processing chamber 201 is replaced with the inactive gas (inactive gas replacement), and the pressure in the processing chamber 201 is restored to normal pressure (atmospheric pressure restoration).

[0171] By such a series of treatments, the first process combination (first batch treatment) in which the above-mentioned process combination (a), (b), (c), and (d) is repeated multiple times is performed in sequence, that is, Figure 4 The first round in the process is completed. Moreover, this process combination (batch processing) is performed multiple times, during which the generation of particles caused by the film formed in the processing container can be appropriately suppressed.

[0172] It should be noted that, as described above, the oxidation treatment of the film attached in the furnace is performed in a state where the baffle is closed. That is, the oxidation treatment of the film attached in the furnace is performed without moving (accommodating) the processed wafer box 217 and wafer 200 (product wafer, test wafer) into the processing container. Therefore, the above-mentioned oxidation treatment is not performed on the SiN film formed on the surface of the processed wafer box 217 and wafer 200 (product wafer, test wafer), and the SiN film formed on the surface of the wafer box 217 and wafer 200 (product wafer, test wafer) is not oxidized and maintains the original state, that is, the original state of the SiN film is maintained.

[0173] Thus, after the second process combination (second batch processing), that is, Figure 4 After the second round, the film forming process can be performed while the wafer 200 (ie, the product wafer to be processed next and the test wafer with the SiN film formed on the surface) is supported by the wafer box 217 with the SiN film formed on the surface.

[0174] That is, after the second process combination (second batch processing), the wafer 200 contacts the wafer box 217 via the SiN film formed on the surface of the wafer box 217. Specifically, the wafer box 217 contacts the product wafer to be processed next via the SiN film formed on the surface of the wafer box 217. In addition, the wafer box 217 contacts the test wafer via the SiN film formed on each surface. The SiN film formed on the surface of the wafer box 217 and the surface (back side) of the product wafer are materials with close thermal expansion coefficients to each other, so even if they are heated and thermally expanded during the film forming process, since the degree of their respective thermal expansion is close, it is possible to suppress the generation of particles from their contact parts. In addition, the SiN film formed on the surface of the wafer box 217 and the SiN film formed on the surface of the test wafer are the same material and have the same thermal expansion coefficient, so even if they are heated and thermally expanded during the film forming process, since they are thermally expanded in the same way, it is possible to suppress the generation of particles from their contact parts.

[0175] (3) Effects based on this method

[0176] According to this aspect, one or more of the following effects can be obtained.

[0177] In the oxidation treatment of the film attached in the furnace, an O-containing gas and a H-containing gas are supplied into the processing container, and at the same time, an H-containing gas is also supplied to the first supply part, so that the Si-enriched SiN film formed in the first supply part and its surrounding area (area 500) where the risk of particle generation is relatively high can be fully oxidized. That is, the oxidation amount of the SiN film formed in the area where the risk of particle generation is relatively high can be greater than the oxidation amount of the SiN film formed in the part outside the said area. In other words, the SiO film formed by oxidizing the SiN film formed in the area where the risk of particle generation is relatively high can be made thicker than the SiO film formed by oxidizing the SiN film formed in the part outside the said area. As a result, the stress of the SiN film formed in the area where the risk of particle generation is relatively high can be appropriately controlled (relaxed) to be the same as the stress of the SiN film formed in the part outside the said area, and in particular, the generation of particles caused by the SiN film formed in this area can be fully suppressed.

[0178] It should be noted that, in this case, by supplying H-containing gas to the first supply unit from a position opposite to the first supply unit, the SiN film formed in the region where the risk of particle generation is relatively high can be effectively oxidized. In addition, in this case, by supplying H-containing gas and O-containing gas from any one of the plurality of second supply units, the H-containing gas is supplied from the second supply unit opposite to the first supply unit to the first supply unit, so that the SiN film formed in the region where the risk of particle generation is relatively high can be efficiently oxidized. Furthermore, since there is no need to separately provide a supply unit for supplying H-containing gas and O-containing gas, the second supply unit for supplying the reaction gas can be shared (used concurrently), thereby reducing the cost of the device.

[0179] In the oxidation treatment of the film attached in the furnace, while O-containing gas and H-containing gas are continuously or intermittently supplied to the processing container, by pulse exhausting the processing container, that is, by opening and closing the exhaust valve a predetermined number of times, preferably a plurality of times, the O-containing gas and H-containing gas can be sufficiently moved to the portion of the processing container, for example, the opposite side of the exhaust port. Thus, the SiN film formed in the processing container, for example, the portion opposite to the exhaust port, can also be sufficiently oxidized. That is, the SiN film formed in the processing container can be uniformly oxidized. As a result, the necessary and sufficient oxidation treatment can be uniformly performed on the SiN film formed in the processing container. In this case, while O-containing gas and H-containing gas are continuously or intermittently supplied to the processing container, it is desired to alternately stop the exhaust in the processing container and exhaust the processing container a predetermined number of times, preferably a plurality of times.

[0180] It should be noted that in this case, the process of supplying O-containing gas and H-containing gas into the processing container in a state where exhaust in the processing container is stopped and the process of supplying O-containing gas and H-containing gas into the processing container in a state where exhaust in the processing container is performed may be alternately performed a predetermined number of times, preferably multiple times. In addition, the process of supplying O-containing gas and H-containing gas into the processing container in a state where the exhaust valve is closed and the process of supplying O-containing gas and H-containing gas into the processing container in a state where the exhaust valve is opened may be alternately performed a predetermined number of times, preferably multiple times. In these cases, the same effects as the above effects can be obtained.

[0181] In addition, in this case, by making the exhaust stop state in the processing container longer than the exhaust state in the processing container, that is, the exhaust valve closed state is maintained longer than the exhaust valve open state, the above effect can be further improved. That is, the O-containing gas and the H-containing gas can be more fully moved to the portion in the processing container, such as the opposite side of the exhaust port, and the SiN film formed in the portion in the processing container, such as the opposite side of the exhaust port, can be more fully oxidized. As a result, the SiN film formed in the processing container can be more uniformly subjected to necessary and sufficient oxidation.

[0182] In the oxidation treatment of the film attached in the furnace, since a part of the SiN film formed in the processing container is oxidized to become a SiO film, and other parts of the SiN film different from the part are not oxidized and the SiN film is maintained as it is, the stress balance of the film formed in the processing container can be adjusted so that the stress of the film formed in the processing container is smaller than the stress of the SiN film before oxidation formed in the processing container. As a result, the generation of particles caused by the film formed in the processing container can be appropriately suppressed, the cleaning cycle can be extended, and the productivity of the film forming treatment can be improved.

[0183] In the oxidation treatment of the attached film in the furnace, since a part of the SiN film formed in the processing container is oxidized to become a SiO film, other parts of the SiN film different from the part are not oxidized and the SiN film is maintained as it is, the oxidation time can be shortened and the productivity can be maintained or improved.

[0184] In the oxidation treatment of the film attached in the furnace, a part of the SiN film formed in the processing container is oxidized to become a SiO film, and other parts of the SiN film different from the part are not oxidized to maintain the original state of the SiN film. Therefore, compared with the case where the SiO film is deposited on the surface of the SiN film formed in the processing container, the cumulative film thickness in the processing container can be suppressed to be thin, and the thickness of the SiN film itself formed in the processing container can also be reduced. As a result, the risk of generating particles caused by the increase in the cumulative film thickness in the processing container and the thickness of the SiN film can be reduced. It should be noted that in the case where the SiO film is deposited on the surface of the SiN film formed in the processing container, the thickness of the SiN film itself formed in the processing container cannot be thinned, and its thickness is maintained as it is.

[0185] In the oxidation treatment of the film attached in the furnace, since a part of the SiN film formed in the processing container is oxidized to become a SiO film, and other parts of the SiN film different from the part are not oxidized to maintain the original state of the SiN film, compared with the case where the SiO film is deposited on the surface of the SiN film formed in the processing container, it is possible to reduce the contamination at the interface between the SiO film and the SiN film, stabilize the interface, and suppress the film peeling at the interface. It should be noted that in the case where the SiO film is deposited on the surface of the SiN film formed in the processing container, it is believed that it is easy to cause contamination at the interface between the SiO film and the SiN film and film peeling occurs, and further, it is believed that there is a risk of particle generation due to the gas phase reaction when the SiO film is deposited.

[0186] By adjusting the thickness of the SiN film and the SiO film in the stacked film (i.e., the SiO / SiN stacked film) of the SiO film obtained by oxidizing a portion of the SiN film formed in the processing container and the SiN film that is not oxidized and maintained in the SiN film formed in the processing container, the stress balance of the tensile stress of the SiN film and the compressive stress of the SiO film in the SiO / SiN stacked film can be adjusted. Thus, these stresses can be offset each other, and the total stress of the SiO / SiN stacked film can be close to zero, and then the stress can be zero. Thus, the generation of particles caused by the film formed in the processing container can be appropriately suppressed.

[0187] By making the total stress of the SiO / SiN stacked film a tensile stress, that is, a tensile stress that is smaller than the stress (tensile stress) of the SiN film before oxidation formed in the processing container, the oxidation treatment time can be shortened, and the productivity of the film forming process can be maintained or improved while producing the effect of suppressing particle generation.

[0188] By setting the ratio of SiO film in the SiO / SiN stacked film to be less than 75%, preferably less than 70%, the total stress of the SiO / SiN stacked film can be made into a tensile stress smaller than the stress (tensile stress) of the SiN film before oxidation formed in the processing container, thereby maintaining or improving the productivity of the film forming process while producing the effect of suppressing the generation of particles.

[0189] By not accommodating (carrying in) the processed wafer box 217 into the processing container for the oxidation treatment of the film attached in the furnace, the SiN film formed on the surface of the wafer box 217 can be kept in its original state without being oxidized. Thus, after the second process combination (second batch processing), the film forming treatment can be performed in a state where the wafer 200 to be processed next is supported by the wafer box 217 with the SiN film formed on the surface. That is, after the second process combination (second batch processing), the wafer 200 contacts the wafer box 217 via the SiN film formed on the surface of the wafer box 217. Thus, compared with the case where the SiN film formed on the surface of the wafer box 217 is oxidized, the generation of particles from the contact portion between the wafer 200 and the wafer box 217 can be suppressed.

[0190] It should be noted that when the processed wafer box 217 is contained (moved) in the processing container and the attached film oxidation treatment is performed in the furnace, at least the surface of the SiN film formed on the surface of the wafer box 217 will be oxidized, and the outermost surface of the wafer box will become a SiO film. In this case, after the second process combination (second batch processing), the wafer 200 contacts the wafer box 217 through the SiO film formed on the outermost surface of the wafer box 217. In this case, the SiO film formed on the outermost surface of the wafer box 217 and the surface (back side) of the wafer 200 to be processed next are materials with greatly different thermal expansion coefficients. Therefore, when each is heated and thermally expanded during the film forming process, due to the difference in thermal expansion of each material, the friction of their contact parts will increase, and sometimes particles will be generated from their contact parts.

[0191] By not accommodating (carrying in) the processed wafer box 217 and wafer 200 (product wafer, test wafer) into the processing container and performing the oxidation treatment of the attached film in the furnace, it is possible to prevent the SiN film formed on the surface of the wafer box 217 and wafer 200 (product wafer, test wafer) from being oxidized, and maintain the original state of the SiN film. Thus, after the second process combination (second batch processing), the film forming process can be performed in a state where the product wafer to be processed next and the test wafer to be processed next with the SiN film formed on the surface supported by the wafer box 217 with the SiN film formed on the surface. That is, after the second process combination (second batch processing), the wafer box 217 and the product wafer to be processed next are in contact with each other through the SiN film formed on the surface of the wafer box 217, and the wafer box 217 and the test wafer are in contact with each other through the SiN film formed on their respective surfaces. Thus, the generation of particles from the contact portion between the wafer 200 and the wafer box 217 can be suppressed.

[0192] It should be noted that when the processed wafer box 217 is contained (moved) in the processing container and the attached film oxidation treatment is performed in the furnace, at least the surface of the SiN film formed on the surface of the wafer box 217 is oxidized, and the outermost surface of the wafer box becomes a SiO film. In this case, after the second process combination (second batch processing), the wafer 200 (the product wafer to be processed next, the test wafer with the SiN film formed on the surface) contacts the wafer box 217 through the SiO film formed on the outermost surface of the wafer box 217. In this case, the SiO film formed on the outermost surface of the wafer box 217 and the surface (back side) of the wafer 200 (the product wafer to be processed next, the test wafer with the SiN film formed on the surface) are materials with greatly different thermal expansion coefficients. Therefore, when each is heated and thermally expanded during the film forming process, due to the difference in thermal expansion of each material, the friction of their contact parts increases, and sometimes particles are produced from their contact parts.

[0193] In addition, by performing in-furnace oxidation treatment of the attached film without containing (moving into) the processed wafer box 217 into the processing container, the wafer box loading time and wafer box unloading time used for in-furnace oxidation treatment of the attached film can be eliminated, the time when the film forming process cannot be performed can be shortened to a corresponding extent, and the productivity of the film forming process can be improved.

[0194] By performing the oxidation process of the deposited film in the furnace in parallel with the wafer cooling, it is not necessary to set time for the oxidation process of the deposited film in the furnace in addition to the wafer cooling, and the productivity of the film forming process can be maintained or improved. It should be noted that, depending on the conditions of the oxidation process of the deposited film in the furnace, the oxidation process of the deposited film in the furnace can also be performed in parallel with the wafer cooling so that it can be completed before the wafer release starts.

[0195] By performing the oxidation process of the film deposited in the furnace in parallel with the wafer cooling and the wafer releasing, it is not necessary to set time for performing the oxidation process of the film deposited in the furnace in addition to the wafer cooling and the wafer releasing, and the productivity of the film forming process can be maintained or improved. It should be noted that, depending on the conditions of the oxidation process of the film deposited in the furnace, the oxidation process of the film deposited in the furnace can also be performed in parallel with the wafer cooling and the wafer releasing, so that it can be completed in the middle of the wafer releasing process.

[0196] Since each batch (each round), that is, each batch process, requires one furnace-attached film oxidation treatment, a portion of the SiN film can be oxidized in a state where the SiN film formed in the processing container is thinner, compared with the case where the furnace-attached film oxidation treatment is performed each time the batch processes are performed multiple times. As a result, the SiN film formed in the processing container can be oxidized each time in the area where the oxidation rate can be increased, and the oxidation treatment time can be shortened. On the other hand, in the case where the furnace-attached film oxidation treatment is performed each time the batch processes are performed multiple times, a portion of the SiN film is oxidized in a state where the SiN film formed in the processing container is thicker. In this case, there is a need to perform oxidation treatment in the area where the oxidation rate is reduced, and the oxidation treatment time may be prolonged. It should be noted that, compared with the case where the furnace-attached film oxidation treatment is performed each time the batch processes are performed multiple times, the ratio of the SiO film in the accumulated film formed in the processing container can be increased when the furnace-attached film oxidation treatment is performed for each batch, and the stress of the accumulated film can be further reduced. That is, by performing the oxidation treatment of the deposited film in the furnace for each batch, it is possible to produce an effect of suppressing the generation of particles and further enhance the effect while maintaining or improving the productivity of the film forming process.

[0197] (4) Modification

[0198] The processing flow of this embodiment can be changed into the following modified examples. These modified examples can be combined arbitrarily. Unless otherwise specified, the processing process and processing conditions in each step of each modified example can be the same as the processing process and processing conditions in each step of the above-mentioned processing process.

[0199] (Variant 1)

[0200] In step 2 of the film forming process, the gas containing N and H as the reaction gas can be plasma-excited, that is, activated into a plasma state and supplied to the wafer 200 in the processing chamber 201, that is, the Si-containing layer formed on the wafer 200. That is, in the film forming process, each gas can be supplied as shown in the following gas supply flow to form a SiN film on the wafer 200.

[0201] (raw material gas → plasma excited reaction gas) × n

[0202] In this case, in step 2 of the film forming process, for example, Figure 6 As shown, the gas containing N and H as the reaction gas supplied into the gas supply pipes 232b and 232c can be respectively plasma excited by remote plasma units 300b and 300c as plasma excitation units (plasma generation units) respectively provided on the downstream side of the gas supply pipes 232b and 232c relative to the valves 243b and 243c, and then supplied to the processing chamber 201. It should be noted that Figure 6 In Figure 1 The same parts described in the same manner are given the same symbols, and the description thereof is omitted.

[0203] This modification can also achieve the same effect as the above embodiment. In addition, according to this modification, compared with the case where the film forming process is performed in a non-plasma atmosphere as in the above embodiment, the film forming process can be further cooled down. By using plasma in this way, the same effect as the above embodiment can be achieved even when the film forming process is performed at a lower temperature.

[0204] (Variant 2)

[0205] When the oxidation treatment of the deposited film in the furnace is performed, at least one of the O-containing gas and the H-containing gas is plasma-excited, that is, activated into a plasma state and supplied into the processing chamber 201 .

[0206] In this case, in the oxidation treatment of the deposited film in the furnace, for example, Figure 6 As shown, at least one of the H-containing gas and the O-containing gas supplied from the gas supply pipes 232e and 232f to the gas supply pipes 232c and 232c can be excited into plasma by remote plasma units 300b and 300c respectively provided on the downstream side of the gas supply pipes 232b and 232c relative to the valves 243b and 243c, and then supplied to the processing chamber 201. It should be noted that Figure 6 In Figure 1 The same parts described in the same manner are given the same symbols, and the description thereof is omitted.

[0207] It should be noted that, in the oxidation treatment of the deposited film in the furnace, the H-containing gas may not be plasma-excited, but the O-containing gas may be plasma-excited. Alternatively, the O-containing gas may not be plasma-excited, but the H-containing gas may be plasma-excited. Alternatively, both the O-containing gas and the H-containing gas may be plasma-excited.

[0208] The same effects as those of the above-mentioned embodiment can also be obtained in this variant. In addition, according to this variant, the temperature of the oxidation treatment of the film attached in the furnace can be further reduced compared to the case where the film forming treatment is performed in a non-plasma atmosphere as in the above-mentioned embodiment. By using plasma in this way, the same effects as those of the above-mentioned embodiment can be obtained even when the oxidation treatment of the film attached in the furnace is performed at a lower temperature. In addition, since the temperature of the oxidation treatment of the film attached in the furnace can be reduced, the processing temperatures of the film forming treatment and the oxidation treatment of the film attached in the furnace can be made the same, and the time for changing the temperature in the processing container can be eliminated. As a result, the productivity of the film forming treatment can be further improved. In addition, especially when the H-containing gas plasma is excited and supplied, the Cl contained in the SiN film attached in the processing container can be detached and removed, and the stress of the film attached in the processing container can be further reduced.

[0209] (Variant 3)

[0210] The oxidation treatment of the film attached in the furnace can be performed not only in parallel with wafer cooling and wafer release, but also in parallel with the wafer loading of the wafer 200 to be processed next. That is, the oxidation treatment of the film attached in the furnace can be performed in parallel with wafer cooling, wafer release, and wafer loading of the wafer 200 to be processed next.

[0211] This variation can also achieve the same effects as those of the above-described embodiment. In addition, according to this variation, the oxidation amount of the deposits including the SiN film formed in the processing container can be further increased, the stress of the film formed in the processing container can be further reduced, and the generation of particles caused by the film formed in the processing container can be further suppressed.

[0212] (Variant 4)

[0213] In the film forming process, as a nitride film, in addition to the SiN film, a SiN film containing at least any one of C, O, and B may be formed. That is, in the film forming process, as a nitride film, a SiN film, a SiCN film, a SiON film, a SiOCN film, a SiBN film, a SiBCN film, a SiBOCN film, a SiBON film, etc. may be formed. When forming these films, at least any one of a C-containing gas, an O-containing gas, and a B-containing gas may be further supplied from the film forming gas supply system in the film forming process.

[0214] In addition, in the film forming process, as a nitride film, in addition to a silicon-based nitride film (a nitride film containing silicon, a silicon nitride film), a germanium-based nitride film (a nitride film containing germanium, a germanium nitride film) can also be formed. As a germanium nitride film (GeN film), for example, in addition to a GeN film, a GeN film containing at least any one of C, O, and B can also be formed. When forming these films, in the film forming process, it is sufficient to use a Ge-containing gas instead of a Si-containing gas, and further, the film forming gas supply system contains at least any one of a C gas, an O-containing gas, and a B-containing gas.

[0215] In addition, in the film forming process, as a nitride film, in addition to a silicon-based nitride film (a nitride film containing silicon, a silicon nitride film), a metal-based nitride film (a nitride film containing metal, a metal nitride film) can also be formed. As a metal nitride film, for example, an aluminum nitride film (AlN film), a titanium nitride film (TiN film), a zirconium nitride film (ZrN film), a hafnium nitride film (HfN film), a tantalum nitride film (TaN film), a tungsten nitride film (WN film), a molybdenum nitride film (MoN film), etc. can be formed. When forming these films, in the film forming process, instead of the Si-containing gas, at least one of the Al-containing gas, the Ti-containing gas, the Zr-containing gas, the Hf-containing gas, the Ta-containing gas, the W-containing gas, and the Mo-containing gas can be supplied by the film forming gas supply system.

[0216] In this way, in the film formation process, a film containing at least one of a semiconductor element and a metal element and nitrogen can be formed as a nitride film.

[0217] In these cases, you can use Figure 1 The substrate processing device shown in the figure performs film forming processing in a non-plasma atmosphere, and can also be used Figure 6 The substrate processing apparatus shown performs film formation processing using plasma.

[0218] In this modification example as well, the same effects as those of the above-described embodiment can be obtained.

[0219] <Other embodiments of the present disclosure>

[0220] The embodiments of the present disclosure have been specifically described above, but the present disclosure is not limited to the above embodiments, and various modifications can be made without departing from the gist of the present disclosure.

[0221] For example, after the above steps (a), (b), (c), and (d) are combined and repeated a plurality of times, the inside of the processing container may be cleaned.

[0222] That is, by repeating the above-mentioned steps (a), (b), (c), and (d) multiple times, a SiO / SiN stacked film is accumulated in the processing container. In this case, before the SiO / SiN stacked film accumulated in the processing container exceeds a critical film thickness, cracks, or film peeling occurs, the processing container can be cleaned.

[0223] When the processing container is cleaned, the cleaning gas is supplied into the processing container by the cleaning gas supply system without accommodating the wafer 200, and the exhaust is performed by the exhaust pipe 231. At this time, the cleaning gas may be supplied into the processing container while the wafer box 217 having the SiN film formed on the surface is accommodated in the processing container. In addition, the cleaning gas may be supplied into the processing container while the test wafer having the SiN film formed on the surface is accommodated in the processing container.

[0224] The following are examples of treatment conditions in the cleaning treatment:

[0225] Processing temperature (temperature in the processing chamber 201): 200-500°C,

[0226] Processing pressure (pressure in processing chamber 201): 1330~26600Pa,

[0227] Clean gas supply flow rate: 0.5~5slm,

[0228] Inert gas supply flow rate: 1~20slm

[0229] As the cleaning gas, for example, fluorine (F2) gas, chlorine trifluoride (ClF3) gas, chlorine monofluoride (ClF) gas, nitrogen trifluoride (NF3) gas, hydrogen fluoride (HF) gas or other fluorine (F)-containing gas can be used. As the cleaning gas, one or more of these can be used.

[0230] After the cleaning process, the adhesion state of the film in the processing container can be reset before the effect brought by the above embodiment disappears, and then the effect brought by the above embodiment can be continuously obtained again. It should be noted that according to the above embodiment, the cumulative thickness of the film accumulated in the processing container until it exceeds the critical film thickness, cracks, and film peeling can be greatly increased, the cycle of the cleaning process described here can be greatly extended, and the productivity of the overall film forming process can be greatly improved.

[0231] The recipes for each of these treatments are preferably prepared separately according to the treatment content, and are pre-stored in the storage device 121c via the communication circuit and the external storage device 123. Moreover, it is preferred that when each treatment is started, the CPU 121a appropriately selects a suitable recipe from the multiple recipes stored in the storage device 121c according to the treatment content. Thus, a thin film of various film types, composition ratios, film qualities, and film thicknesses can be formed with good reproducibility by one substrate processing device. In addition, through these treatments, for the films of various film types, composition ratios, film qualities, and film thicknesses formed in the processing container, the oxidation treatment of the attached film in the furnace can be appropriately performed. In addition, the operating burden of the operator can be reduced, operating errors can be avoided, and each treatment can be started quickly.

[0232] The above-mentioned recipe is not limited to the case of newly making, and can also be prepared by, for example, changing an existing recipe already installed in the substrate processing device. When changing the recipe, the changed recipe can be installed in the substrate processing device via a communication circuit and a recording medium recording the recipe. In addition, the input / output device 122 of the existing substrate processing device can be operated to directly change the existing recipe already installed in the substrate processing device.

[0233] In the above embodiment, an example of forming a film using a batch-type substrate processing device that processes multiple substrates at a time is described. However, the present disclosure is not limited to the above embodiment, and can also be well applied to the case where a film is formed using a single-piece substrate processing device that processes one or more substrates at a time. In addition, in the above embodiment, an example of forming a film using a substrate processing device having a hot wall type processing furnace is described. However, the present disclosure is not limited to the above embodiment, and can also be well applied to the case where a film is formed using a substrate processing device having a cold wall type processing furnace.

[0234] When using these substrate processing apparatuses, each process can be performed according to the same process and process conditions as those in the above-mentioned embodiment and the above-mentioned modified example, and the same effects as those in the above-mentioned embodiment and the above-mentioned modified example can be obtained.

[0235] The above-mentioned embodiments and the above-mentioned modified examples can be used in combination as appropriate. The processing procedure and processing conditions in this case may be, for example, the same as those in the above-mentioned embodiments and the above-mentioned modified examples.

Claims

1. A substrate processing method, comprising the following steps: (a) a step of loading a substrate into a processing container, (b) performing the following process in the processing container, that is, a process of forming a nitride film on the substrate by alternately or simultaneously performing a process of supplying a raw material gas to the substrate by the first supply unit and a process of supplying a reaction gas to the substrate by the second supply unit a predetermined number of times, (c) a step of removing the processed substrate from the processing container, and (d) a step of oxidizing a portion of the nitride film formed in the processing container in (b) to convert the nitride film into an oxide film after the processed substrate is removed from the processing container; In (d), oxygen-containing gas and hydrogen-containing gas are supplied into the processing container, and the hydrogen-containing gas is supplied to the first supply part from a position opposite to the first supply part so that the supply flow rate of the hydrogen-containing gas is greater than the supply flow rate of the oxygen-containing gas.

2. The substrate processing method according to claim 1, in, In (d), an oxidation amount of the nitride film formed in the first supply portion and its periphery in the processing container is made larger than an oxidation amount of the nitride film formed in the processing container other than the first supply portion and its periphery.

3. The substrate processing method according to claim 1, in, In (d), an oxide film formed by oxidizing the nitride film formed on the first supply portion and its periphery in the processing container is made thicker than an oxide film formed by oxidizing the nitride film formed on a portion other than the first supply portion and its periphery in the processing container.

4. The substrate processing method according to claim 1, in, In (b), the nitride film formed on the first supply part and its periphery in the processing container is made thicker than the nitride film formed on a portion other than the first supply part and its periphery in the processing container.

5. The substrate processing method according to claim 1, in, A plurality of the second supply parts are provided, In (d), the oxygen-containing gas and the hydrogen-containing gas are supplied from any one of the plurality of second supply units, respectively.

6. The substrate processing method according to claim 5, in, One of the plurality of second supply parts is opposite to the first supply part, In (d), the hydrogen-containing gas is supplied to the first supply portion from the second supply portion that is opposed to the first supply portion.

7. The substrate processing method according to claim 1, in, In (d), while the oxygen-containing gas and the hydrogen-containing gas are continuously or intermittently supplied into the processing container, exhaustion in the processing container is stopped and exhausted in the processing container is alternately performed a predetermined number of times.

8. The substrate processing method according to claim 1, in, In (d), the following steps are performed alternately: a step of supplying the oxygen-containing gas and the hydrogen-containing gas into the processing container while exhaust in the processing container is stopped, and The step of supplying the oxygen-containing gas and the hydrogen-containing gas into the processing container while the processing container is exhausted.

9. The substrate processing method according to claim 1, in, In (d), while the oxygen-containing gas and the hydrogen-containing gas are continuously or intermittently supplied into the processing container, an exhaust valve provided in an exhaust pipe for exhausting the processing container is opened and closed a predetermined number of times.

10. The substrate processing method according to claim 1, in, In (d), the following steps are alternately performed a predetermined number of times: The step of supplying the oxygen-containing gas and the hydrogen-containing gas into the processing container with an exhaust valve provided in an exhaust pipe for exhausting the processing container closed, and and supplying the oxygen-containing gas and the hydrogen-containing gas into the processing container in a state where the exhaust valve is opened.

11. The substrate processing method according to claim 1, in, In (d), the processing container is pulse-exhausted while the oxygen-containing gas and the hydrogen-containing gas are continuously or intermittently supplied into the processing container.

12. The substrate processing method according to claim 1, in, In (d), the oxygen-containing gas and the hydrogen-containing gas are supplied to the processing container in a heated state at a pressure lower than atmospheric pressure.

13. The substrate processing method according to claim 1, in, The reaction gas is a nitriding gas, The nitride film is a nitride film containing at least one of a semiconductor element and a metal element and nitrogen.

14. A substrate processing method comprising the following steps: (a) a step of loading a substrate into a processing container, (b) performing the following process in the processing container, that is, a process of forming a nitride film on the substrate by alternately or simultaneously performing a process of supplying a raw material gas to the substrate by the first supply unit and a process of supplying a reaction gas to the substrate by the second supply unit a predetermined number of times, (c) a step of removing the processed substrate from the processing container, and (d) a step of oxidizing a portion of the nitride film formed in the processing container in (b) to convert the nitride film into an oxide film after the processed substrate is removed from the processing container; In (d), an oxygen-containing gas and a hydrogen-containing gas are supplied into the processing container, and the hydrogen-containing gas is supplied to the first supply part from a position opposite to the first supply part. In (d), while the oxygen-containing gas and the hydrogen-containing gas are continuously or intermittently supplied into the processing container, exhausting the processing container is stopped and exhausted alternately for a predetermined number of times. In (d), the time for which the exhaust in the processing container is kept in the stopped state is made longer than the time for which the exhaust in the processing container is kept in the exhausted state.

15. A substrate processing method comprising the following steps: (a) a step of loading a substrate into a processing container, (b) performing the following process in the processing container, that is, a process of forming a nitride film on the substrate by alternately or simultaneously performing a process of supplying a raw material gas to the substrate by the first supply unit and a process of supplying a reaction gas to the substrate by the second supply unit a predetermined number of times, (c) a step of removing the processed substrate from the processing container, and (d) a step of oxidizing a portion of the nitride film formed in the processing container in (b) to convert the nitride film into an oxide film after the processed substrate is removed from the processing container; In (d), an oxygen-containing gas and a hydrogen-containing gas are supplied into the processing container, and the hydrogen-containing gas is supplied to the first supply part from a position opposite to the first supply part. In (d), while the oxygen-containing gas and the hydrogen-containing gas are continuously or intermittently supplied into the processing container, an exhaust valve provided in an exhaust pipe for exhausting the processing container is opened and closed a predetermined number of times, In (d), the time for which the exhaust valve is maintained in the closed state is made longer than the time for which the exhaust valve is maintained in the open state.

16. A method for manufacturing a semiconductor device, comprising the following steps: (a) a step of loading a substrate into a processing container, (b) performing the following process in the processing container, that is, a process of forming a nitride film on the substrate by alternately or simultaneously performing a process of supplying a raw material gas to the substrate by the first supply unit and a process of supplying a reaction gas to the substrate by the second supply unit a predetermined number of times, (c) a step of removing the processed substrate from the processing container, and (d) a step of oxidizing a portion of the nitride film formed in the processing container in (b) to convert the nitride film into an oxide film after the processed substrate is removed from the processing container; in, In (d), oxygen-containing gas and hydrogen-containing gas are supplied into the processing container, and the hydrogen-containing gas is supplied to the first supply part from a position opposite to the first supply part so that the supply flow rate of the hydrogen-containing gas is greater than the supply flow rate of the oxygen-containing gas.

17. A substrate processing device comprising: a processing container for processing a substrate, a raw material gas supply system, wherein a first supply unit supplies a raw material gas to the substrate in the processing container; a reaction gas supply system, wherein the reaction gas is supplied to the substrate in the processing container by a second supply unit, an oxygen-containing gas supply system for supplying oxygen-containing gas into the processing container, a hydrogen-containing gas supply system for supplying hydrogen-containing gas into the processing container, a transport device for transporting the substrate into and out of the processing container, and A control unit is configured to control the raw material gas supply system, the reaction gas supply system, the oxygen-containing gas supply system, the hydrogen-containing gas supply system and the transport device to perform the following processes: (a) a process of loading a substrate into the processing container, (b) a process of forming a nitride film on the substrate by alternately or simultaneously supplying the raw material gas to the substrate by the first supply unit and supplying the reaction gas to the substrate by the second supply unit a predetermined number of times in the processing container, (c) a process of unloading the processed substrate from the processing container, and (d) a process of oxidizing a portion of the nitride film formed in the processing container in (b) to convert it into an oxide film in a state where the processed substrate is unloaded from the processing container, and in (d), the oxygen-containing gas and the hydrogen-containing gas are supplied to the processing container, the hydrogen-containing gas is supplied to the first supply unit from a position opposite to the first supply unit, and the supply flow rate of the hydrogen-containing gas is greater than the supply flow rate of the oxygen-containing gas.

18. A computer-readable recording medium having a program recorded thereon for causing a substrate processing apparatus to execute the following process via a computer: (a) a process of loading a substrate into a processing container of the substrate processing apparatus, (b) a process of performing the following process in the processing container, that is, a process of supplying a raw material gas to the substrate by the first supply unit and a process of supplying a reaction gas to the substrate by the second supply unit alternately or simultaneously for a predetermined number of times, thereby forming a nitride film on the substrate, (c) a process of removing the processed substrate from the processing container, (d) a process of oxidizing a portion of the nitride film formed in the processing container in (b) to convert the nitride film into an oxide film after the processed substrate is removed from the processing container, In (d), oxygen-containing gas and hydrogen-containing gas are supplied into the processing container, and the hydrogen-containing gas is supplied to the first supply part from a position opposite to the first supply part so that the supply flow rate of the hydrogen-containing gas is greater than the supply flow rate of the oxygen-containing gas.