A working roller of a leveling machine and a manufacturing method thereof

By adopting two-layer designs of the outer layer of high ferrochromium alloy and the inner core of the ferrozolis alloy, combined with the use of rare earth Mg and NbC, the problem of insufficient wear resistance of forged steel materials during high temperature tempering is solved, and the working roller is realized High wear resistance and efficient production have improved the production capacity of the leveling machine and the quality of the steel plate.

CN114367538BActive Publication Date: 2024-12-03SINOSTEEL XINGTAI MACHINERY & MILL ROLL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111589562.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-23
Publication Date
2024-12-03
Estimated Expiration
2041-12-23

AI Technical Summary

Technical Problem

The working roller material of the existing leveling machine is forged steel, which leads to orange peel phenomenon during the processing of high-demand steel plates, which limits the increase in production capacity. Moreover, the wear resistance of conventional forged steel materials during high-temperature tempering is insufficient, making it difficult to meet efficient production. need.

Method used

Using a two-layer design work roller, the outer layer is a high ferrochromium alloy and the inner core is a ferrozoic alloy. Through specific chemical composition and heat treatment processes, including high-temperature quenching and multiple tempering, combined with the use of rare earth Mg and NbC, the use of deteriorating agents such as rare earth Mg and NbC, ensures that High wear resistance and toughness of the roller sleeve.

Benefits of technology

It significantly improves the wear resistance and overall performance of the working roller, reduces the difficulty of manufacturing, can meet the characteristics of high iron chromium containing eutectic carbides, and improves the working efficiency and steel plate quality of the leveling machine.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114367538B_ABST
    Figure CN114367538B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of rolling mills, in particular to a working roll of a leveling machine and a manufacturing method thereof. The working roll comprises an outer layer and an inner core, wherein the outer layer is made of high chromium iron, the inner core is made of ductile iron, a roller sleeve is the outer layer and the core, the chemical composition of the outer layer is C: 2.1-3.0%, Si: 0.5-1.5%, Mn: 0.2-1.2%, P≤0.10%, S≤0.1%, Cr: 10-30%, Ni: 0.5-3.0%, Mo: 0.5-3.0%, V: 0.1-2.0, and the balance is Fe; the chemical composition of the core is C: 2.3-4.0%, Si: 1.0-4.0%, Mn: 0.1-1.0%, P≤0.10%, S≤0.1%, Cr≤1.0%, Ni≤2.0%, Mo: 0.1-3.0%, and the balance is iron; the working roll performance and quality are improved as a whole, and the requirements of conventional forged steel working rolls are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rolling mills, in particular to a working roll of a leveling machine and a manufacturing method thereof. Background Art

[0002] At present, the working rolls in the flattening machine are still mainly made of forged steel, with short on-machine time and low production line efficiency. Especially as the downstream customers of steel mills have higher and higher requirements for steel plate quality, the flattening amount gradually increases, and conventional forged steel materials will show orange peel during the rolling process, limiting the increase in production capacity.

[0003] At present, the material of the working rolls of the leveling machine has gradually begun to be upgraded. High chromium iron contains a large amount of eutectic carbides and has the characteristics of high tempering temperature, high wear resistance and high surface quality. The combined production of the working rolls of the leveling machine has the advantage of being recyclable. At the same time, the combined production also provides good and convenient conditions for upgrading the material of the roller sleeve. Summary of the invention

[0004] The present invention aims to design a working roll of a leveling machine, improve the performance and quality of the working roll as a whole, and meet the requirements of conventional forged steel working rolls.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0006] A working roller of a leveling machine comprises an outer layer and an inner core, wherein the outer layer is made of high chromium iron and the inner core is made of ductile iron; the roller sleeve is the outer layer and the core, the chemical composition of the outer layer is C: 2.1-3.0%, Si: 0.5-1.5%, Mn: 0.2-1.2%, P≤0.10%, S≤0.1%, Cr: 10-30%, Ni: 0.5-3.0%, Mo: 0.5-3.0%, V: 0.1-2.0, and the balance is Fe; the chemical composition of the core is C: 2.3-4.0%, Si: 1.0-4.0%, Mn: 0.1-1.0%, P≤0.10%, S≤0.1%, Cr≤1.0%, Ni≤2.0%, Mo: 0.1-3.0%, and the balance is iron.

[0007] A further improvement of the technical solution of the present invention is that the working roll and the roll sleeve are interference fitted, and the interference amount is 0.1 to 1‰.

[0008] A further improvement of the technical solution of the present invention is that the thickness of the roller sleeve working layer is 20 to 50 mm.

[0009] A method for manufacturing a working roll of a leveling machine comprises the following steps:

[0010] Step A, working roll smelting, the outer layer material is high chromium iron, the inner core material is ductile iron; roller sleeve smelting, the outer layer and the core iron are added with chemical components within the set range;

[0011] Step B, after the roller sleeve smelting composition reaches the standard, the outer layer and the core molten iron are heated to a temperature of 1400-1600°C and taken out of the furnace, and poured when the temperature drops to 1250-1400°C, the outer layer adopts a flip-over ladle, the core adopts a bottom-leaking ladle or a flip-over ladle, when pouring, the outer layer adopts a method of adding a modifier along the flow, and the core molten iron adopts a method of adding a spheroidizing agent and an inoculant to the bottom of the ladle, a 10-20mm thick steel plate is used to cover the top of the spheroidizing agent, and the steel plate is covered with scrap steel chips, and the amount of spheroidizing agent added is 1-5%; the amount of molten iron poured in the core is at least 1.6 times the amount of molten iron in the outer layer;

[0012] Step C, cold unpacking the roller sleeve 30-60 hours after casting, and rough machining after cold unpacking, roughing the outer diameter and inner hole diameter of the roller body by 5-15mm and the axial allowance by 5-200mm;

[0013] Step D, after the roughing is completed, the roller body is quenched and heated by high temperature heat treatment and the whole roller is tempered;

[0014] Step E, after the roller sleeve is quenched and tempered, fine processing and testing are performed until the finished product;

[0015] Step F, interference fit the roller sleeve and the working roller.

[0016] The further improvement of the technical solution of the present invention is that: the modifier in step B is a mixture of rare earth Mg and NbC, with a ratio of 1:1 and an addition amount of less than 0.2%; the spheroidizing agent is rare earth magnesium or cerium-rich rare earth, any one or more of which can be selected.

[0017] The further improvement of the technical solution of the present invention is that in the high temperature heat treatment method in step D, the furnace temperature is 900-1150°C, the heating time is 200-300min, the cooling method is air cooling to the roller temperature of 200-450°C and tempering, the tempering temperature is 460-600°C, the insulation time is 20-60h, and the tempering is performed by 1-4 tempering methods.

[0018] Compared with the prior art, the present invention provides a working roll of a leveling machine and a manufacturing method thereof, which have the following beneficial effects:

[0019] 1. The present invention proposes a working roller of a leveling machine and a manufacturing method thereof. The roller sleeve of the working roller is designed with two layers. The outer layer is made of high-chromium iron alloy material to ensure high wear resistance of the working layer. Good organizational morphology is obtained by adding rare earth Mg modifier and NbC. The core is made of ductile iron alloy with good toughness, which ensures that the assembly stress in the later assembly process is within a reasonable range and reduces the manufacturing difficulty. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 This is a photo of the high-chromium iron structure of the outer layer of the metallographic structure of the working roller of a leveling machine of the present invention. The white phase is carbide, the gray matrix is ​​the matrix, and the strength is relatively high. DETAILED DESCRIPTION

[0022] like Figure 1 As shown, a working roller of a leveling machine comprises an outer layer and an inner core, wherein the outer layer is made of high chromium iron, and the inner core is made of ductile iron; the roller sleeve is the outer layer and the core, and the chemical composition of the outer layer is C: 2.1-3.0%, Si: 0.5-1.5%, Mn: 0.2-1.2%, P≤0.10%, S≤0.1%, Cr: 10-30%, Ni: 0.5-3.0%, Mo: 0.5-3.0%, V: 0.1-2.0, and the balance is Fe; the chemical composition of the core is C: 2.3-4.0%, Si: 1.0-4.0%, Mn: 0.1-1.0%, P≤0.10%, S≤0.1%, Cr≤1.0%, Ni≤2.0%, Mo: 0.1-3.0%, and the balance is iron;

[0023] The working roll and the roll sleeve are interference fitted, and the interference is 0.1 to 1‰; the thickness of the roll sleeve working layer is 20 to 50 mm.

[0024] A method for manufacturing a working roll of a leveling machine comprises the following steps:

[0025] Step A, working roll smelting, the outer layer material is high chromium iron, the inner core material is ductile iron; roller sleeve smelting, the outer layer and the core iron are added with chemical components within the set range;

[0026] Step B, after the roller sleeve smelting composition reaches the standard, the outer layer and the core molten iron are heated to a temperature of 1400-1600°C by electricity and taken out of the furnace, and poured when the temperature drops to 1250-1400°C, the outer layer adopts a flip-over ladle, the core adopts a bottom-leaking ladle or a flip-over ladle, when pouring, the outer layer adopts a method of adding a modifier along the flow, and the core molten iron adopts a method of adding a spheroidizing agent and an inoculant at the bottom of the ladle, a 10-20mm thick steel plate is used to cover the top of the spheroidizing agent, and the steel plate is covered with scrap steel chips, and the amount of spheroidizing agent added is 1-5%; the amount of molten iron poured in the core is at least 1.6 times the amount of molten iron in the outer layer; the modifier is a mixture of rare earth Mg and NbC, the ratio is 1:1, and the amount added is less than 0.2%; the spheroidizing agent is rare earth magnesium, cerium-rich rare earth, any one or more of them are selected;

[0027] Step C, cold unpacking the roller sleeve 30-60 hours after casting, and rough machining after cold unpacking, roughing the outer diameter and inner hole diameter of the roller body by 5-15mm and the axial allowance by 5-200mm;

[0028] Step D, after the rough addition is completed, the roller body is quenched and heated by high-temperature heat treatment and tempered as a whole; the furnace temperature of the high-temperature heat treatment method is 900-1150°C, the heating time is 200-300min, the cooling method is air cooling to the roller temperature of 200-450°C and tempering, the tempering temperature is 460-600°C, the insulation time is 20-60h, and the tempering is performed by 1-4 tempering methods.

[0029] Step E, after the roller sleeve is quenched and tempered, fine processing and testing are performed until the finished product;

[0030] Step F, interference fit the roller sleeve and the working roller.

[0031] The roller sleeve in the working roller is designed with two layers. The outer layer of high-chromium iron alloy material ensures the high wear resistance of the working layer. A good organizational morphology is obtained by adding rare earth Mg modifier and NbC. The core is made of ductile iron alloy with good toughness, which ensures that the assembly stress in the later assembly process is within a reasonable range. The working roller of the leveling machine has a long roller body, and its manufacturing difficulty is much higher than that of conventional roller ring assembly. This method greatly reduces the manufacturing difficulty.

[0032] The present invention is further described in detail below in conjunction with embodiments:

[0033] Example 1

[0034] The roller sleeve of the working roll is made of scrap steel, nickel iron, vanadium iron, chromium iron, molybdenum iron and electrode powder, and is smelted in a medium frequency furnace to reach the designed composition range: the outer layer molten iron is C2.33%, Si0.85%, Mn0.9%, P0.05%, S0.06%, Cr20.56%, Ni0.98%, Mo0.85%, V1.01%, W0.5% and the balance is Fe; the core molten iron is C3.05%, Si1.36%, Mn0.95%, P0.06%, S0.07%, Cr0.03%, Ni0.12%, Mo0.3% and the balance is Fe. The outer layer is melted at a temperature of 1510℃, and after the composition meets the standard, the temperature is raised to 1530℃ and then centrifugally poured out of the furnace. The core molten steel melting temperature is 1490℃, the pouring temperature is 1510℃, the outer layer pouring water volume is 2.1t, and the core pouring water volume is 4.5t. After pouring, the roll was unpacked for 39 hours, and the axial allowance was 25mm and the radial allowance was 12mm. The roll was heated at 980℃ for 230min, air-cooled for 2.5h until the roll body reached 431℃ and then tempered in a furnace for 35h. The roll was tempered twice. After the roll sleeve was processed to the finished product, it was fitted with the working roll with an interference fit. The inner diameter of the roll sleeve was 625.03mm, and the inner diameter of the roll shaft was 625.56mm.

[0035] Example 2

[0036] The roller sleeve of the working roll is made of scrap steel, nickel iron, vanadium iron, chromium iron, molybdenum iron and electrode powder, and is smelted in a medium frequency furnace to reach the designed composition range: the outer layer molten iron is C2.33%, Si0.85%, Mn0.9%, P0.05%, S0.06%, Cr20.56%, Ni0.98%, Mo0.85%, V1.01%, W0.5% and the balance is Fe; the core molten iron is C3.05%, Si1.36%, Mn0.95%, P0.06%, S0.07%, Cr0.03%, Ni0.12%, Mo0.3% and the balance is Fe. The outer layer is melted at a temperature of 1510℃, and after the composition meets the standard, the temperature is raised to 1530℃ and then centrifugally poured out of the furnace. The core molten steel melting temperature is 1490℃, the pouring temperature is 1510℃, the outer layer pouring water volume is 2.1t, and the core pouring water volume is 4.5t. After pouring, the roll was unpacked for 39 hours, and the axial allowance was 25mm and the radial allowance was 12mm. The roll was heated at 980℃ for 230min, air-cooled for 2.5h until the roll body reached 431℃ and then tempered in a furnace for 35h. The roll was tempered twice. After the roll sleeve was processed to the finished product, it was fitted with the working roll with an interference fit. The inner diameter of the roll sleeve was 625.00mm and the inner diameter of the roll shaft was 625.55mm.

[0037] Example 3

[0038] The sleeve of the working roll is made of scrap steel, nickel iron, vanadium iron, chromium iron, molybdenum iron and electrode powder, and is smelted in a medium frequency furnace to reach the designed composition range: the outer layer molten iron is C2.81%, Si0.89%, Mn0.92%, P0.06%, S0.07%, Cr22.36%, Ni1.32%, Mo0.99%, V1.03%, W0.45% and the balance is Fe; the core molten iron is C3.12%, Si1.31%, Mn0.91%, P0.05%, S0.06%, Cr0.01%, Ni0.11%, Mo0.2% and the balance is Fe. The outer layer is melted at a temperature of 1520℃, and after the composition meets the standard, the temperature is raised to 1535℃ and then centrifugally poured out of the furnace. The core molten steel melting temperature is 1485℃, the pouring temperature is 1505℃, the outer layer pouring water volume is 1.9t, and the core pouring water volume is 4.3t. After pouring, the roller was unpacked for 35 hours, and the axial allowance was 23mm and the radial allowance was 11mm. The roller was heated at 1000℃ for 220 minutes, air-cooled for 2.3 hours until the roller body reached 436℃, and then tempered in a furnace for 32 hours. The roller was tempered twice. After the roller sleeve was processed to the finished product, it was fitted with the working roller. The inner diameter of the roller sleeve was 625.05mm, and the inner diameter of the roller shaft was 625.53mm.

[0039] Example 4

[0040] The roller sleeve of the working roll is made of scrap steel, nickel iron, vanadium iron, chromium iron, molybdenum iron and electrode powder, and is smelted in a medium frequency furnace to reach the designed composition range: the outer layer molten iron is C2.75%, Si0.81%, Mn0.81%, P0.03%, S0.04%, Cr19.87%, Ni1.12%, Mo0.95%, V1.01%, W0.41% and the balance is Fe; the core molten iron is C3.10%, Si1.25%, Mn0.83%, P0.02%, S0.03%, Cr0.02%, Ni0.08%, Mo0.1% and the balance is Fe. The outer layer is melted at a temperature of 1511℃, and after the composition meets the standard, the temperature is raised to 1521℃ and then centrifugally poured out of the furnace. The core molten steel melting temperature is 1480℃, the pouring temperature is 1501℃, the outer layer pouring water volume is 1.85t, and the core pouring water volume is 4.1t. 33 hours after pouring, the box was opened cold, 16mm of axial allowance and 9mm of radial allowance were added, heated at 1011℃ for 205min, air-cooled for 2.5h until the roller body reached 431℃, and then tempered in a furnace for 31h, and tempered twice. After the roller sleeve was processed to the finished product, it was fitted with the working roller in an interference fit, with the inner diameter of the roller sleeve being 625.02mm and the inner diameter of the roller shaft being 625.49mm.

[0041] Example 5

[0042] The roll sleeve of the working roll is made of scrap steel, nickel iron, vanadium iron, chromium iron, molybdenum iron and electrode powder as raw materials and is smelted in a medium frequency furnace to reach the designed composition range: the outer layer molten iron contains C2.71%, Si0.78%, Mn0.79%, P0.01%, S0.03%, Cr19.25%, Ni1.05%, Mo0.91%, V1.15%, W0.10% and the balance is Fe; the core molten iron contains C3.35%, Si1.22%, Mn0.81%, P0.03%, S0.05%, Cr0.08%, Ni0.06%, Mo0.09% and the balance is Fe. The outer layer is melted at 1501℃, and after the composition meets the standard, it is heated to 1516℃ and then centrifugally poured. The core molten steel melting temperature is 1483℃, the pouring temperature is 1512℃, the outer layer pouring water volume is 1.89t, and the core pouring water volume is 4.25t. After pouring, it is cold unpacked 35h after pouring, and the axial allowance is 19mm and the radial diameter allowance is 10mm. It is heated at 1019℃ for 207min, air-cooled for 2.8h to the roller body at 439℃, and tempered in the furnace for 36h, and tempered twice. After the roller sleeve is processed to the finished product, it is interference-fitted with the working roller. The inner diameter of the roller sleeve is 625.12mm, and the inner diameter of the roller shaft is 625.65mm.

[0043] Example 6

[0044] The sleeve of the working roll is made of scrap steel, nickel iron, vanadium iron, chromium iron, molybdenum iron and electrode powder, and is smelted in a medium frequency furnace to reach the designed composition range: the outer layer molten iron is C2.79%, Si0.75%, Mn0.78%, P0.02%, S0.06%, Cr19.26%, Ni1.08%, Mo0.89%, V1.01%, W0.15% and the balance is Fe; the core molten iron is C3.36%, Si1.29%, Mn0.83%, P0.04%, S0.06%, Cr0.09%, Ni0.07%, Mo0.12% and the balance is Fe. The outer layer is melted at a temperature of 1509℃, and after the composition meets the standard, the temperature is raised to 1513℃ and then centrifugally poured out of the furnace. The core molten steel melting temperature is 1483℃, the pouring temperature is 1509℃, the outer layer pouring water volume is 1.79t, and the core pouring water volume is 4.03. After pouring, the roller was unpacked for 39 hours, and the axial allowance was 21mm and the radial allowance was 11mm. The roller was heated at 1018℃ for 201min, air-cooled for 2.6h until the roller body reached 433℃ and then tempered in a furnace for 37h. The roller was tempered twice. After the roller sleeve was processed to the finished product, it was fitted with the working roller. The inner diameter of the roller sleeve was 625.09mm and the inner diameter of the roller shaft was 625.69mm.

[0045] Example 7

[0046] Example 7 is a control example, which is a conventional forged steel working roll.

[0047] The products of Examples 1 to 7 were taken for testing of tensile mechanical properties of the samples. The performance test was carried out in accordance with the national standard GB / T228. The test results are shown in Table 1.

[0048] Table 1 Example product performance test results

[0049]

[0050] Through the development of a working roll manufacturing method for a leveling machine, the wear resistance of the developed combined leveling machine working roll is more than twice that of the conventional forged steel working roll.

[0051] According to the performance test results, a method for manufacturing the working rolls of a leveling machine was developed. In actual use, the method can better adapt to the working characteristics of the leveling machine frame, and in particular can significantly improve the roll service life.

[0052] The embodiments described above are merely descriptions of preferred implementation modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the scope of protection determined by the claims of the device of the present invention.

Claims

1. A method for manufacturing a working roll of a leveling machine, It is characterized in that The steps include: Step A, working roll smelting; roll sleeve smelting, the roll sleeve is an outer layer and a core, and the outer layer and the core molten iron are added with chemical components in a set range; the chemical composition of the outer layer is C: 2.1-3.0%, Si: 0.5-1.5%, Mn: 0.2-1.2%, P≤0.10%, S≤0.1%, Cr: 10-30%, Ni: 0.5-3.0%, Mo: 0.5-3.0%, V: 0.1-2.0, and the balance is Fe; the chemical composition of the core is C: 2.3-4.0%, Si: 1.0-4.0%, Mn: 0.1-1.0%, P≤0.10%, S≤0.1%, Cr≤1.0%, Ni≤2.0%, Mo: 0.1-3.0%, and the balance is iron; the thickness of the roll sleeve working layer is 20-50 mm; Step B, after the roller sleeve smelting composition reaches the standard, the outer layer and the core molten iron are heated to a temperature of 1400-1600°C and taken out of the furnace, and poured when the temperature drops to 1250-1400°C, the outer layer adopts a flip-over ladle, the core adopts a bottom-leaking ladle or a flip-over ladle, when pouring, the outer layer adopts a method of adding a modifier along the flow, and the core molten iron adopts a method of adding a spheroidizing agent and an inoculant to the bottom of the ladle, a 10-20mm thick steel plate is used to cover the top of the spheroidizing agent, and the steel plate is covered with scrap steel chips, and the amount of spheroidizing agent added is 1-5%; the amount of molten iron poured in the core is at least 1.6 times the amount of molten iron in the outer layer; Step C, cold unpacking the roller sleeve 30-60 hours after casting, and rough machining after cold unpacking, roughing the outer diameter and inner hole diameter of the roller body by 5-15mm and the axial allowance by 5-200mm; Step D, after the roughing is completed, the roller body is quenched and heated by high temperature heat treatment and the whole roller is tempered; Step E, after the roller sleeve is quenched and tempered, fine processing and testing are performed until the finished product; Step F, interference fit the roller sleeve with the working roller and the roller shaft; the interference amount is 0.1 to 1‰.

2. A method for manufacturing a working roll of a skin pass mill according to claim 1, Features: In step B, the modifier is a mixture of rare earth Mg and NbC, with a ratio of 1:1 and an addition amount of less than 0.2%; the spheroidizing agent is rare earth magnesium or cerium-rich rare earth, any one or more of which can be selected.

3. A method for manufacturing a working roll of a skin pass mill according to claim 1, Features: In step D, the furnace temperature of the high temperature heat treatment method is 900-1150°C, the heating time is 200-300min, the cooling method is air cooling to the roller temperature of 200-450°C, the tempering temperature is 460-600°C, the insulation time is 20-60h, and the tempering is performed by 1-4 tempering methods.