Preparation method and application of surface reconstructed PdFe / Cu nano-electrocatalyst for fuel cells

By alloying Pd and Cu, using ethylene glycol and CTAC/KBr as solvents and morphology control agents, PdFe/Cu catalyst was prepared, which solved the problems of high amount and low stability of precious metal Pd, and achieved efficient ethanol oxidation performance and Improved stability.

CN114373952BActive Publication Date: 2024-11-08WUXI MANGRO TRADING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111562368.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-20
Publication Date
2024-11-08
Estimated Expiration
2041-12-20

AI Technical Summary

Technical Problem

When using precious metal Pd, the existing direct ethanol fuel cell catalyst has problems of high cost and low utilization, and the catalyst stability is insufficient.

Method used

By adopting multi-step liquid phase synthesis technology, PdFe/Cu electrocatalyst with excellent ethanol oxidation properties is prepared by alloying Pd and transition metal Cu, using ethylene glycol and secondary distilled water as solvents, and CTAC and KBr as morphological control agents. Reduce the amount of Pd and improve the stability of the catalyst.

Benefits of technology

It realizes that without losing electrocatalytic performance, reduce the use of Pd, improve the utilization rate of Pd atoms, and significantly improves the stability of the catalyst and ethanol oxidation performance, and shows excellent electrocatalytic activity and great application prospects. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 211217143357
    Figure 211217143357
  • Figure 211217143400
    Figure 211217143400
  • Figure 211217143733
    Figure 211217143733
Patent Text Reader

Abstract

The present invention provides a surface reconstructed PdFe / Cu nano electrocatalyst for a fuel cell. The PdFe / Cu nano electrocatalyst for a fuel cell uses transition metal Cu as a seed, and the precursors of precious metals Pd and Fe are continuously replaced and deposited on the Cu surface to form a PdFe / Cu nano electrocatalyst. The preparation method is divided into two steps. The first step is to synthesize transition metal Cu seed crystals, and the second step is to form a spherical shell composed of Fe and precious metal Pd by replacement deposition. The ethylene glycol added in the reaction acts as a solvent and a reducing agent at the same time, which is low in cost and green and pollution-free. The CTAC and KBr used in the synthesis method are used as morphology control agents, and the prepared PdFe / Cu catalysts are uniform in size.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fuel cells and relates to a method for preparing a catalyst, in particular to a method for preparing a core-shell structured PdFe / Cu electrocatalyst for a direct ethanol fuel cell. Background Art

[0002] Fuel Cell is the fourth generation of power generation technology after thermal power, hydropower and nuclear power. It is a device that directly converts chemical energy in fuel into electrical energy. This energy conversion method is not limited by the Carnot cycle, and the emissions are clean and pollution-free. It is an efficient and environmentally friendly new energy technology. Direct ethanol fuel cells (DEFCs) are a type of low-temperature fuel cell. Because the fuel is liquid ethanol, it is superior to traditional hydrogen and oxygen fuel cells in storage, transportation, safety and cost. The direct ethanol fuel cell system has the characteristics of simple structure, rapid startup, easy fuel replenishment and high theoretical specific energy. In the oxidation of ethanol in alkaline systems, Pd-based nanomaterials have electrocatalytic properties comparable to Pt-based materials and are a very potential Pt substitute.

[0003] In the present invention, by preparing a surface-reconstructed PdFe / Cu nano-electrocatalyst, the amount of precious metal Pd can be further reduced without losing the electrocatalytic performance, effectively improving the utilization rate of Pd atoms; and compared with general catalysts, the catalyst in the present invention exhibits more lasting stability. The combination of precious metal Pd and non-precious metals is an effective means to reduce the amount of Pd in ​​the catalyst, and the particularity of this multi-element alloy is that there is a synergistic effect and stress-strain effect between heterogeneous elements, and the strain effect can be regulated by changing the ratio of precursors. In the present invention, transition metal Cu is used as a seed, and a multi-step liquid phase synthesis technology is used. Ethylene glycol and double distilled water serve as solvents, wherein ethylene glycol serves as a reducing agent, and CTAC and KBr serve as morphology control agents. The prepared catalyst particles have a smaller and more uniform particle size, and have a PdFe / Cu catalyst with excellent ethanol oxidation performance. Summary of the invention

[0004] The purpose of the present invention is to reduce the amount of precious metal Pd, and at the same time, prepare a PdFe / Cu electrocatalyst for fuel cells with excellent ethanol catalytic activity by controlling the alloy ratio and appropriately regulating the morphology.

[0005] The technical solution adopted by the present invention to achieve the above-mentioned purpose is as follows:

[0006] (1) Weigh hexadecyltrimethylammonium chloride (CTAC) and potassium bromide (KBr) and dissolve them in double distilled water, disperse them by ultrasonic, heat the oil bath to 50-70°C, stir, introduce N2, and drop an ethylene glycol solution of anhydrous copper chloride (CuCl2) (the introduction of N2 here creates an inert atmosphere to prevent Cu from being oxidized by O2 in the system during the reduction process to form Cu oxides); drop an ethylene glycol solution of sodium hydroxide (NaOH) into the mixed solution, adjust the solution pH to 9.5-10, seal the solution, heat to 100-120°C, remove N2 (the removal of N2 here is because the system is sealed and in an inert atmosphere, and no N2 is needed), keep the reaction warm for 1-2 hours, cool naturally to room temperature, centrifuge and wash with double distilled water and anhydrous ethanol at 8000-10000 rpm / min for 2-3 times, respectively, and vacuum dry the obtained Cu seed crystals and seal them for storage. The concentration of CTAC in the mixed solution is 10-15 mg / mL, the concentration of KBr is 3-5 mg / mL, the concentration of CuCl2 ethylene glycol solution is 1.3-1.5 mg / mL, and the concentration of NaOH ethylene glycol solution is 4 mg / mL.

[0007] (2) Weigh a certain amount of Cu seed crystals, CTAC and KBr, add double distilled water and ultrasonically dissolve; after stirring at 60℃ for 30min, add aqueous solutions of K2PdCl4 and FeCl3 to the mixture, and finally add ethylene glycol solution of NaOH. The concentration of CTAC in the mixture is 3.56 mg / mL, the concentration of KBr is 1.33 mg / mL, the concentration of Cu seed crystals is 0.02~0.03 mg / mL, the concentration of K2PdCl4 in the mixture is 1.3~1.4 mg / mL, the concentration of FeCl3 is 0.6~0.8 mg / mL, and the concentration of NaOH is 8 mg / mL.

[0008] (3) The uniformly mixed reaction solution is heated in an oil bath in a three-necked flask at 80-160°C for 1-4 hours.

[0009] (4) Cooling naturally to room temperature, centrifuging at 8000 rpm / min~10000 rpm / min, washing with double distilled water and anhydrous ethanol by centrifugation for 3~5 times respectively, and redissolving the final product in anhydrous ethanol for dispersion and storage to obtain PdFe / Cu electrocatalyst for fuel cell.

[0010] In step (1), double distilled water and ethylene glycol serve as solvents at the same time, wherein ethylene glycol serves as a reducing agent, and CTAC and KBr serve as morphology control agents. In the present invention, KBr can be replaced by KI, and CTAC and KBr can be replaced by hexadecyltrimethylammonium bromide (CTAB).

[0011] In step (2), the volume of the mixed liquid in the three-necked flask is 20-30 mL.

[0012] In step (3), during the centrifugal washing process, the catalyst is first washed with double distilled water for 2 to 3 times, and then washed with anhydrous ethanol for 2 to 3 times to ensure that unreacted reactants are removed from the catalyst surface.

[0013] The PdFe / Cu electrocatalyst for fuel cells has a spherical structure, and the catalyst particles have a uniform size with an average particle size of 2.5-7.0 nm.

[0014] The electrochemically active area (ECSA) of the PdFe / Cu electrocatalyst for the fuel cell is 50-75 m 2 / g Pd .

[0015] The PdFe / Cu electrocatalyst for fuel cells has a surface reconstructed structure, the surface of the spherical shell is enriched with Pd and the Fe bulk phase is mainly Cu, which greatly reduces the amount of precious metal Pd.

[0016] The outer surface of the PdFe / Cu electrocatalyst for fuel cells is composed of a ternary alloy, and its structure has a synergistic effect and a structural strain effect.

[0017] The surface reconstructed PdFe / Cu electrocatalyst for fuel cells and the preparation method thereof involved in the present invention have the following significant features:

[0018] (1) The preparation method is divided into two steps. The first step is to synthesize transition metal Cu seeds, and the second step is to form a spherical shell composed of Fe and precious metal Pd by replacement deposition.

[0019] (2) The ethylene glycol added in the reaction acts as both a solvent and a reducing agent, which is low-cost and green and pollution-free.

[0020] (3) CTAC and KBr are used as morphology control agents in this synthesis method, and the PdFe / Cu catalysts prepared are uniform in size.

[0021] (4) The prepared catalyst has excellent electrocatalytic oxidation performance and stability for ethanol, and has great application and development prospects in direct ethanol fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 : Transmission electron microscopy image of the PdFe / Cu-1 electrocatalyst for fuel cell prepared in Example 1.

[0023] Figure 2 : Cyclic voltammetry curve of the PdFe / Cu-1 electrocatalyst for the fuel cell prepared in Example 1 for electrocatalytic oxidation of ethanol.

[0024] Figure 3 : Transmission electron microscopy image of the PdFe / Cu-2 electrocatalyst for fuel cell prepared in Example 2.

[0025] Figure 4 : Cyclic voltammetry curve of the PdFe / Cu-2 electrocatalyst for the fuel cell prepared in Example 2 for electrocatalytic oxidation of ethanol.

[0026] Figure 5 : Transmission electron microscopy image of the PdFe / Cu-3 electrocatalyst for fuel cell prepared in Example 3.

[0027] Figure 6 : Cyclic voltammetry curve of the PdFe / Cu-3 electrocatalyst for the fuel cell prepared in Example 3 for electrocatalytic oxidation of ethanol.

[0028] Figure 7 : Comparison of the cyclic voltammetric activities of the PdFe / Cu electrocatalyst for fuel cells prepared in Examples 1, 2, and 3 and commercial Pd black electrocatalytic oxidation of ethanol. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation cases. It should be stated here that these implementation cases are only used to illustrate the present invention rather than to limit the scope of the present invention. After reading the present invention, modifications to various equivalent forms by those skilled in the art all fall within the scope defined by the claims attached to this application.

[0030] Example 1

[0031] (1) Weigh 384 mg of CTAC into a 50 mL round-bottom spherical bottle, add 15 mL of double distilled water and sonicate to dissolve it; add CuCl2 ethylene glycol solution (40.335 mg CuCl2 dissolved in 5 mL ethylene glycol) to the mixture, sonicate and transfer to an oil bath, introduce N2, and stir at 60 °C for 30 min; add NaOH ethylene glycol solution (96 mg NaOH dissolved in 20 mL ethylene glycol) dropwise, heat to 110 °C, remove N2, keep warm for 1-2 hours, cool naturally to room temperature, wash with double distilled water and anhydrous ethanol at 10000 rpm / min for 2-3 times, respectively, and store the resulting Cu seed crystals in a vacuum oven and sealed.

[0032] (2) Weigh 0.53 mg of Cu seed crystals, 64 mg of CTAC and 24 mg of KBr into a 50 mL three-necked flask, add 18 mL of double distilled water and dissolve under ultrasonication; stir at 60 °C for 30 min, then add NaOH ethylene glycol solution (96 mg NaOH dissolved in 12 mL ethylene glycol) and aqueous solution of K2PdCl4 and FeCl3 (8.16 mg K2PdCl4 and 4.5 mgFeCl3·6H2O dissolved in 6 mL double distilled water) dropwise into the mixture and stir thoroughly.

[0033] (3) The mixed reaction solution was placed in a 50 mL three-necked flask and heated to 110 °C in an oil bath for 2 h.

[0034] (4) Cooling naturally to room temperature and keeping it still, the black precipitate obtained after the reaction was centrifuged at 10000 rpm / min, washed three times with double distilled water, and then washed three times with anhydrous ethanol. Finally, the obtained product was dispersed and protected by adding anhydrous ethanol to obtain the PdFe / Cu-1 electrocatalyst for fuel cells.

[0035] Figure 1 This is a transmission electron microscope (TEM) image of the PdFe / Cu-1 electrocatalyst for fuel cells prepared in Example 1. As can be seen from the figure, the prepared catalyst particles are uniform in size and have slight agglomeration.

[0036] The PdFe / Cu electrocatalyst prepared in this example was modified on a glassy carbon electrode to prepare a working electrode, and a cyclic voltammetry test was performed on it. The test conditions were: the scanning range was -0.8~0.2 V (vs. SCE), the scanning speed was 50 mV / s, and the solution was a nitrogen-saturated 1 mol / L KOH+1 mol / L C2H5OH solution. The test results are as follows: Figure 2 shown.

[0037] Depend on Figure 2 It can be seen that the prepared PdFe / Cu-1 electrocatalyst exhibits excellent electrocatalytic oxidation performance, with a maximum ethanol oxidation peak current density of about 794.97 mA / mg at a potential of -0.1 V. Pd , showing the best electrocatalytic activity for ethanol oxidation.

[0038] Example 2

[0039] (1) Weigh 384 mg of CTAC into a 50 mL round-bottom spherical bottle, add 15 mL of double distilled water and sonicate to dissolve it; add CuCl2 ethylene glycol solution (40.335 mg CuCl2 dissolved in 5 mL ethylene glycol) to the mixture, sonicate and transfer to an oil bath, introduce N2, and stir at 60 °C for 30 min; add NaOH ethylene glycol solution (96 mg NaOH dissolved in 20 mL ethylene glycol) dropwise, heat to 110 °C, remove N2, keep warm for 1-2 hours, cool naturally to room temperature, wash with double distilled water and anhydrous ethanol at 10000 rpm / min for 2-3 times, respectively, and store the resulting Cu seed crystals in a vacuum oven and sealed.

[0040] (2) Weigh 0.53 mg of Cu seed crystals, 192 mg of CTAC and 24 mg of KBr into a 50 mL three-necked flask, add 18 mL of double distilled water and dissolve under ultrasonication; after stirring at 60 °C for 30 min, add NaOH ethylene glycol solution (96 mg NaOH dissolved in 12 mL ethylene glycol) and aqueous solution of K2PdCl4 and FeCl3 (8.16 mg K2PdCl4 and 4.5 mgFeCl3·6H2O dissolved in 6 mL double distilled water) dropwise into the mixture and stir thoroughly.

[0041] (3) The mixed reaction solution was placed in a 50 mL three-necked flask and heated to 110 °C in an oil bath for 2 h.

[0042] (4) Cooling naturally to room temperature and keeping it still, the black precipitate obtained after the reaction was centrifuged at 10000 rpm / min, washed three times with double distilled water, and then washed three times with anhydrous ethanol. Finally, the obtained product was dispersed and protected by adding anhydrous ethanol to obtain PdFe / Cu-2 electrocatalyst for fuel cells.

[0043] Figure 3 Transmission electron microscopy (TEM) images of the PdFe / Cu-2 electrocatalyst for fuel cells prepared in Example 2. As can be seen from the figure, due to the increase in the amount of CTAC, the catalyst particles prepared partially present irregular morphology and also agglomerate.

[0044] The PdFe / Cu-2 electrocatalyst prepared in this example was modified on a glassy carbon electrode to prepare a working electrode, and a cyclic voltammetry test was performed on it. The test conditions were: the scanning range was -0.8~0.2 V (vs. SCE), the scanning speed was 50mV / s, and the solution was a nitrogen-saturated 1 mol / L KOH+1 mol / L C2H5OH solution. The test results are as follows: Figure 4 shown.

[0045] Depend on Figure 4 It can be seen that the prepared PdFe / Cu-2 electrocatalyst exhibits excellent electrocatalytic oxidation performance, with a maximum ethanol oxidation peak current density of about 574.71 mA / mg at a potential of -0.2 V. Pd , showing good electrocatalytic activity for ethanol oxidation.

[0046] Example 3

[0047] (1) Weigh 384 mg of CTAC into a 50 mL round-bottom spherical bottle, add 15 mL of double distilled water and sonicate to dissolve it; add CuCl2 ethylene glycol solution (40.335 mg CuCl2 dissolved in 5 mL ethylene glycol) to the mixture, sonicate and transfer to an oil bath, introduce N2, and stir at 60 °C for 30 min; add NaOH ethylene glycol solution (96 mg NaOH dissolved in 20 mL ethylene glycol) dropwise, heat to 110 °C, remove N2, keep warm for 1-2 hours, cool naturally to room temperature, wash with double distilled water and anhydrous ethanol at 10000 rpm / min for 2-3 times, respectively, and store the resulting Cu seed crystals in a vacuum oven and sealed.

[0048] (2) Weigh 0.53 mg of Cu seed crystals, 64 mg of CTAC and 72 mg of KBr into a 50 mL three-necked flask, add 18 mL of double distilled water and dissolve under ultrasonication; after stirring at 60°C for 30 min, add NaOH ethylene glycol solution (96 mg NaOH dissolved in 12 mL ethylene glycol) and aqueous solution of K2PdCl4 and FeCl3 (8.16 mg K2PdCl4 and 4.5 mgFeCl3·6H2O dissolved in 6 mL double distilled water) dropwise into the mixture and stir thoroughly.

[0049] (3) The mixed reaction solution was placed in a 50 mL three-necked flask and heated to 110 °C in an oil bath for 2 h.

[0050] (4) Cool naturally to room temperature and keep it still. Centrifuge the black precipitate obtained after the reaction at 10000 rpm / min, wash it three times with double distilled water, and then wash it three times with anhydrous ethanol. Finally, add anhydrous ethanol to disperse the obtained product to obtain PdFe / Cu-3 electrocatalyst for fuel cells.

[0051] Figure 5 The transmission electron microscopy (TEM) images of the PdFe / Cu-3 electrocatalyst for fuel cells prepared in Example 3 are shown in Figure 1. As can be seen, the particle size of the catalyst prepared by increasing the amount of KBr is significantly different, and the uniformity is not as good as the first two examples.

[0052] The PdFe / Cu-3 electrocatalyst prepared in this example was modified on a glassy carbon electrode to prepare a working electrode, and a cyclic voltammetry test was performed on it. The test conditions were: the scanning range was -0.8~0.2 V (vs. SCE), the scanning speed was 50mV / s, and the solution was a nitrogen-saturated 1 mol / L KOH+1 mol / L C2H5OH solution. The test results are as follows: Figure 6 shown.

[0053] Depend on Figure 6 It can be seen that the prepared PdFe / Cu-3 electrocatalyst exhibits excellent electrocatalytic oxidation performance, with a maximum ethanol oxidation peak current density of about 524.29 mA / mg at a potential of -0.2 V. Pd , showing good electrocatalytic activity for ethanol oxidation.

[0054] Figure 7 The activity comparison diagram of the PdFe / Cu alloy electrocatalyst for fuel cells prepared in Examples 1, 2, and 3 and the commercial Pd black catalyst for electrocatalytic oxidation of ethanol is shown in the figure. It can be seen intuitively from the figure that the electrocatalytic oxidation activity of ethanol in Example 1 is significantly better than that in Example 2 and Example 3 and the commercial Pd black nanocatalyst, and the catalysts prepared in Examples 1, 2, and 3 are all better than the commercial Pd black. Among them, the ethanol electrooxidation specific activity of Example 1 is the highest, which is about 1.38 times that of Example 2, 1.52 times that of Example 3, and 2.52 times that of the commercial Pd black.

Claims

1. Preparation method of surface reconstructed PdFe / Cu nano-electrocatalyst for fuel cells, It is characterized in that The specific steps are as follows: (1) Weigh 384 mg of CTAC into a 50 mL round-bottom spherical bottle, add 15 mL of double distilled water and ultrasonically dissolve it; add CuCl 2 Ethylene glycol solution, CuCl 2 The ethylene glycol solution is 40.335 mg CuCl 2 Dissolve in 5 mL of ethylene glycol, transfer to an oil bath after ultrasonic dissolution, and pass N 2 , stirred at 60℃ for 30 min; after dropping NaOH ethylene glycol solution, the NaOH ethylene glycol solution was 96 mg NaOH dissolved in 20 mL ethylene glycol, heated to 110℃, and N 2 , keep the reaction warm for 1-2 hours, cool naturally to room temperature, wash with double distilled water and anhydrous ethanol at 10000 rpm / min by centrifugation for 2-3 times respectively, and vacuum dry and seal the obtained Cu seed crystals for storage; (2) Weigh 0.53 mg of Cu seed, 64 mg of CTAC and 24 mg of KBr in a 50 mL three-necked flask, add 18 mL of double distilled water and ultrasonically dissolve; stir at 60 °C for 30 min, then add ethylene glycol solution of NaOH, KBr and the like dropwise to the mixture. 2 PdCl 4 and FeCl 3 The aqueous solution of NaOH is 96 mg NaOH dissolved in 12 mL ethylene glycol. 2 PdCl 4 and FeCl 3 The aqueous solution is 8.16 mg K 2 PdCl 4 and 4.5 mg FeCl 3 6H 2 O was dissolved in 6 mL of double distilled water and stirred thoroughly; (3) The mixed reaction solution was placed in a 50 mL three-necked flask and heated to 110 °C in an oil bath for 2 h; (4) Cooling naturally to room temperature and keeping it still, the black precipitate obtained after the reaction was centrifuged at 10000 rpm / min, washed three times with double distilled water, and then washed three times with anhydrous ethanol. Finally, the obtained product was dispersed and protected in anhydrous ethanol to obtain PdFe / Cu-1 electrocatalyst for fuel cells.