Preparation method of BC / PHB composite material for heavy metal ion removal
By dissolving bacterial cellulose and R. eutropha H16 under alkaline conditions, a BC/PHB composite material with a porous structure is formed, which solves the problems of complex and high cost of the existing technology and achieves efficient and environmentally friendly heavy metal ion adsorption and desorption. Effect.
Patent Information
- Application Number
- CN202111532753.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-12-15
AI Technical Summary
The preparation method of existing BC/PHB composite materials is complex and costly, and the materials prepared by DMF and high-temperature melting methods do not have a porous structure, which affects the adsorption effect of heavy metals.
Under alkaline conditions, bacterial cellulose and R. eutropha H16 are dissolved, and the PHB released after crushing and decomposition is combined with bacterial cellulose to form a fluffy and porous composite material. NaOH/Urea solution and H2SO4 are used for treatment, and PHB is omitted. Extraction steps simplify the preparation process.
A low-cost, porous structure BC/PHB composite material has been obtained, which has good heavy metal ion adsorption capacity, short adsorption time, good desorption performance and cycle stability. The material is biomass and can be microbially degraded after use without causing environmental pollution.
Smart Images

Figure CN114377660B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of BC / PHB composite materials, and in particular to a method for preparing a BC / PHB composite material for removing heavy metal ions. Background Art
[0002] As a biomass material, bacterial cellulose has high water holding capacity, high cellulose content, high hydrophilicity, and biodegradability. PHB is also a biomass material, synthesized in the cytoplasmic particles of R.eutropha H16 bacteria. PHB is usually extracted using organic solvents chloroform and sodium hypochlorite. The extraction process is complicated and time-consuming, and the organic matter used to extract PHB is harmful to the human body and has a great pollution effect on the environment.
[0003] The reported composite methods of BC and PHB so far include: N,N-dimethylformamide (DMF) solvent casting method, microbial co-cultivation method, high temperature melt blending method and trifluoroacetic acid co-dissolution method. In the above methods, bacterial cellulose is mainly composited with purchased or purified pure PHB, which greatly increases the application cost. In addition, the bacterial cellulose / PHB composite material prepared by DMF and high temperature melt method no longer has a porous structure, which is not conducive to the adsorption of heavy metals. Summary of the invention
[0004] The object of the present invention is to provide a simple, convenient and low-cost method for preparing a BC / PHB composite material for removing heavy metal ions, so as to solve the above technical problems.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] The preparation method of the BC / PHB composite material for heavy metal ion removal comprises dissolving bacterial cellulose and R.eutropha H16 in an alkaline solution in sequence, so that the bacterial cellulose is compounded with PHB released after the cell wall of R.eutropha H16 is broken and decomposed under alkaline conditions.
[0007] Preferably, the above preparation method comprises the following steps:
[0008] S1. Solvent preparation: 7 wt% NaOH and 12 wt% Urea were prepared with deionized water;
[0009] S2. Dissolution of bacterial cellulose: Add bacterial cellulose to the NaOH / Urea solution in step S1, and dissolve under low temperature magnetic stirring until the solution becomes transparent and colorless;
[0010] S3, add dried R.eutropha H16, stir at room temperature until the solution turns bright yellow;
[0011] S4. Regenerate the bacterial cellulose / poly 3-hydroxybutyrate composite material in step S3 with 0.5% H2SO4 solution; finally wash with deionized water until neutral and dry.
[0012] Since bacterial cellulose is soluble in NaOH / Urea solution and the cell wall and other lipid substances of R.eutrophaH16 can be broken and decomposed under alkaline conditions, the released PHB can be compounded with the dissolved bacterial cellulose macromolecules, and finally a fluffy and porous bacterial cellulose / PHB composite material is obtained. This material contains a large number of hydroxyl and carboxyl groups and has a porous structure, which is conducive to the adsorption and removal of heavy metal ions. In addition, this material has good desorption performance and can be reused many times. Both bacterial cellulose and PHB are biomass materials, which are biocompatible and biodegradable. After the heavy metal ions are desorbed, they can be decomposed into monomers by microorganisms without causing secondary pollution.
[0013] Preferably, the mass ratio of the bacterial cellulose to R. eutropha H16 is 0.1-10:1.
[0014] Preferably, in step S2, the dissolution temperature of bacterial cellulose is -10°C and the dissolution time is 2-3 hours.
[0015] Preferably, in step S4, the volume ratio of the H2SO4 solution to the composite material solution is 1:3.
[0016] Preferably, in step S3, the saponification reaction time of R.eutropha H16 in the NaOH / Urea solution is 10-12 hours.
[0017] Preferably, the culture time of R.eutropha H16 is 72h.
[0018] Another object of the present invention is to provide an application of the composite material prepared by the above method in removing heavy metal ions, wherein the heavy metal ions are divalent nickel ions or divalent lead ions.
[0019] Another object of the present invention is to provide a method for using the composite material prepared by the above method, wherein the BC / PHB composite material is added to a solution to be adsorbed and shaken at room temperature.
[0020] Preferably, the pH value of the solution to be adsorbed is 6.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The present invention prepares bacterial cellulose / poly 3-hydroxybutyrate composite materials by a new method, which omits the step of extracting PHB, is simple and convenient, and has low preparation cost.
[0023] (2) The present invention has good adsorption capacity for heavy metal ions, short adsorption time, good desorption capacity, good cycle stability, and can be used repeatedly.
[0024] (3) Bacterial cellulose and PHB are both biomass materials that can be degraded by microorganisms after use and will not cause pollution to the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a photograph of the solution prepared in Example 1 of the present invention.
[0026] Figure 2 This is a scanning electron microscope image of Example 1 of the present invention.
[0027] Figure 3 This is the optimal adsorption capacity diagram of Example 1 of the present invention.
[0028] Figure 4 This is the optimal pH data diagram of Experimental Example 4 of the present invention. DETAILED DESCRIPTION
[0029] The following embodiments further illustrate the technical solution of the present invention, but are not intended to limit the protection scope of the present invention.
[0030] Example 1
[0031] The preparation method of BC / PHB composite material comprises the following steps:
[0032] S1. Solvent preparation: 7 wt % NaOH and 12 wt % Urea were prepared with deionized water (45 mL);
[0033] S2. Dissolution of bacterial cellulose: 0.2 g of bacterial cellulose was added to the NaOH / Urea solution in step S1, and dissolved under magnetic stirring at -10°C for 2.5 h until the solution was transparent and colorless;
[0034] S3, add 1.6g of dried R.eutropha H16, stir at room temperature for 10h, until the solution turns bright yellow;
[0035] S4, regenerating the bacterial cellulose / poly 3-hydroxybutyrate composite material in step S3 with 0.5% H2SO4 solution (V(H2SO4):V 混合溶液 =1:3); finally, wash with deionized water until neutral and dry.
[0036] The above composite materials were used for heavy metal ion adsorption test: 10 mg / L Ni 2+ Solution and Pb 2+ solution, and then add 0.1g / L BC / PHB composite material to 100mL Ni 2+ Solution and Pb 2+ The solution was shaken at 30° for 2 h. 2+ Solution and Pb 2+ The solution was filtered with a 0.22 μm filter head, and the filtrate was tested for Ni under an atomic absorption spectrometer ICP-3500 2+ and Pb 2+ residual concentration.
[0037] Performance test results: The product morphology was characterized by SEM. Figure 1 The pictures are respectively of bacterial cellulose (NaOH / Urea) solution, when R.eutrophaH16 is just added, and after bacterial cellulose and PHB are combined in the solution. Figure 2 This is a scanning electron microscope picture of the composite material, which shows that bacterial cellulose and PHB are well composited. Figure 3 This is the adsorption capacity diagram of the composite material.
[0038] Example 2
[0039] The preparation method of BC / PHB composite material comprises the following steps:
[0040] S1. Solvent preparation: 7 wt % NaOH and 12 wt % Urea were prepared with deionized water (45 mL);
[0041] S2. Dissolution of bacterial cellulose: 0.2 g of bacterial cellulose was added to the NaOH / Urea solution in step S1, and dissolved under magnetic stirring at -10°C for 2.5 h until the solution was transparent and colorless;
[0042] S3, add 1.6 g of dried R.eutropha H16, stir at room temperature for 11 h until the solution turns bright yellow;
[0043] S4, regenerating the bacterial cellulose / poly 3-hydroxybutyrate composite material in step S3 with 0.5% H2SO4 solution (V(H2SO4):V 混合溶液 =1:3); finally, wash with deionized water until neutral and dry.
[0044] The above composite materials were used for heavy metal ion adsorption test: 10 mg / L Ni 2+ Solution and Pb 2+solution, and then add 0.1g / L BC / PHB composite material to 100mL Ni 2+ Solution and Pb 2+ The solution was shaken at 30° for 2 h. 2+ Solution and Pb 2+ The solution was filtered with a 0.22 μm filter head, and the filtrate was tested for Ni under an atomic absorption spectrometer ICP-3500 2+ and Pb 2+ residual concentration.
[0045] Performance test results: The product morphology was characterized by SEM, and the results were similar to those in Example 1.
[0046] Example 3
[0047] The preparation method of BC / PHB composite material comprises the following steps:
[0048] S1. Solvent preparation: 7 wt % NaOH and 12 wt % Urea were prepared with deionized water (45 mL);
[0049] S2. Dissolution of bacterial cellulose: 0.2 g of bacterial cellulose was added to the NaOH / Urea solution in step S1, and dissolved under magnetic stirring at -10°C for 2.5 h until the solution was transparent and colorless;
[0050] S3, add 1.6 g of dried R.eutropha H16, stir at room temperature for 12 h until the solution turns bright yellow;
[0051] S4, regenerating the bacterial cellulose / poly 3-hydroxybutyrate composite material in step S3 with 0.5% H2SO4 solution (V(H2SO4):V 混合溶液 =1:3); finally, wash with deionized water until neutral and dry.
[0052] The above composite materials were used for heavy metal ion adsorption test: 10 mg / L Ni 2+ Solution and Pb 2+ solution, and then add 0.1g / L BC / PHB composite material to 100mL Ni 2+ Solution and Pb 2+ The solution was shaken at 30° for 2 h. 2+ Solution and Pb 2+ The solution was filtered with a 0.22 μm filter head, and the filtrate was tested for Ni under an atomic absorption spectrometer ICP-3500 2+ and Pb 2+ residual concentration.
[0053] Performance test results: The product morphology was characterized by SEM, and the results were similar to those in Example 1.
[0054] Experimental Example 4
[0055] The composite material obtained in Example 3 was used for heavy metal ion adsorption test: 10 mg / L Ni and pH values of 2, 3, 4, 5, and 6 were prepared respectively. 2+ Solution and Pb 2+ solution, and then added 0.1 g / L BC / PHB composite material to 100 mL Ni 2+ Solution and Pb 2+ The solution was shaken at 30° for 2 h. 2+ Solution and Pb 2+ The solution was filtered with a 0.22 μm filter head, and the filtrate was tested for Ni under an atomic absorption spectrometer ICP-3500 2+ and Pb 2+ residual concentration.
[0056] Performance test results: refer to Figure 4 The corresponding Ni at pH 2, 3, 4, 5, 6, and 7 were measured. 2+ The residual concentrations were 10, 10, 7.98, 7.76, 7.68, 7.73 mg / L, and the corresponding adsorption capacities were 0, 0, 20.22, 22.38, 23.18, 22.72 mg / g. 2+ The residual concentrations were 9.57, 9.3, 3.74, 2.77, 1.99, and 3 mg / L, respectively. 2+ The adsorption capacities are 4.3, 7, 62.6, 72.3, 80.1 and 70 mg / g respectively.
[0057] Example 5
[0058] The preparation method of BC / PHB composite material comprises the following steps:
[0059] S1. Solvent preparation: 7 wt % NaOH and 12 wt % Urea were prepared with deionized water (45 mL);
[0060] S2. Dissolution of bacterial cellulose: 1.6 g of bacterial cellulose was added to the NaOH / Urea solution in step S1, and dissolved under magnetic stirring at -10°C for 2.5 h until the solution was transparent and colorless;
[0061] S3, add 0.2g of dried R.eutropha H16, stir at room temperature for 12h until the solution turns bright yellow;
[0062] S4, regenerating the bacterial cellulose / poly 3-hydroxybutyrate composite material in step S3 with 0.5% H2SO4 solution (V(H2SO4):V 混合溶液 =1:3); finally, wash with deionized water until neutral and dry.
[0063] The above composite materials were used for heavy metal ion adsorption test: 10 mg / L Ni 2+ Solution and Pb 2+ solution, and then add 0.1g / L BC / PHB composite material to 100mL Ni 2+ Solution and Pb 2+ The solution was shaken at 30° for 2 h. 2+ Solution and Pb 2+ The solution was filtered with a 0.22 μm filter head, and the filtrate was tested for Ni under an atomic absorption spectrometer ICP-3500 2+ and Pb 2+ residual concentration.
[0064] Performance test results: Ni 2+ and Pb 2+ The residual concentrations of Ni 2 + and Pb 2+ The adsorption capacities were 8 mg / g and 31 mg / g respectively.
[0065] Example 6
[0066] The preparation method of BC / PHB composite material comprises the following steps:
[0067] S1. Solvent preparation: 7 wt % NaOH and 12 wt % Urea were prepared with deionized water (45 mL);
[0068] S2. Dissolution of bacterial cellulose: 1.2 g of bacterial cellulose was added to the NaOH / Urea solution in step S1, and dissolved under magnetic stirring at -10°C for 2.5 h until the solution was transparent and colorless;
[0069] S3, add 0.6g of dried R.eutropha H16, stir at room temperature for 12h until the solution turns bright yellow;
[0070] S4, regenerating the bacterial cellulose / poly 3-hydroxybutyrate composite material in step S3 with 0.5% H2SO4 solution (V(H2SO4):V 混合溶液 =1:3); finally, wash with deionized water until neutral and dry.
[0071] The above composite materials were used for heavy metal ion adsorption test: 10 mg / L Ni 2+ Solution and Pb 2+ solution, and then add 0.1g / L BC / PHB composite material to 100mL Ni 2+ Solution and Pb 2+ The solution was shaken at 30° for 2 h. 2+ Solution and Pb 2+ The solution was filtered with a 0.22 μm filter head, and the filtrate was tested for Ni under an atomic absorption spectrometer ICP-3500 2+ and Pb 2+ residual concentration.
[0072] Performance test results: Ni 2+ and Pb 2+ The residual concentrations of Ni 2 + and Pb 2+ The adsorption capacities are 13 mg / g and 42 mg / g respectively.
[0073] Example 7
[0074] The preparation method of BC / PHB composite material comprises the following steps:
[0075] S1. Solvent preparation: 7 wt % NaOH and 12 wt % Urea were prepared with deionized water (45 mL);
[0076] S2. Dissolution of bacterial cellulose: 0.9 g of bacterial cellulose was added to the NaOH / Urea solution in step S1, and dissolved under magnetic stirring at -10°C for 2.5 h until the solution was transparent and colorless;
[0077] S3, add 0.9 g of dried R.eutropha H16, stir at room temperature for 12 h until the solution turns bright yellow;
[0078] S4, regenerating the bacterial cellulose / poly 3-hydroxybutyrate composite material in step S3 with 0.5% H2SO4 solution (V(H2SO4):V 混合溶液 =1:3); finally, wash with deionized water until neutral and dry.
[0079] The above composite materials were used for heavy metal ion adsorption test: 10 mg / L Ni 2+ Solution and Pb 2+ solution, and then add 0.1g / L BC / PHB composite material to 100mL Ni 2+ Solution and Pb2+ The solution was shaken at 30° for 2 h. 2+ Solution and Pb 2+ The solution was filtered with a 0.22 μm filter head, and the filtrate was tested for Ni under an atomic absorption spectrometer ICP-3500 2+ and Pb 2+ residual concentration.
[0080] Performance test results: Ni 2+ and Pb 2+ The residual concentrations of Ni 2 + and Pb 2+ The adsorption capacities are 18 mg / g and 59 mg / g respectively.
[0081] Example 8
[0082] The preparation method of BC / PHB composite material comprises the following steps:
[0083] S1. Solvent preparation: 7 wt % NaOH and 12 wt % Urea were prepared with deionized water (45 mL);
[0084] S2. Dissolution of bacterial cellulose: 0.6 g of bacterial cellulose was added to the NaOH / Urea solution in step S1, and dissolved under magnetic stirring at -10°C for 2.5 h until the solution was transparent and colorless;
[0085] S3, add 1.2 g of dried R.eutropha H16, stir at room temperature for 12 h until the solution turns bright yellow;
[0086] S4, regenerating the bacterial cellulose / poly 3-hydroxybutyrate composite material in step S3 with 0.5% H2SO4 solution (V(H2SO4):V 混合溶液 =1:3); finally, wash with deionized water until neutral and dry.
[0087] The above composite materials were used for heavy metal ion adsorption test: 10 mg / L Ni 2+ Solution and Pb 2+ solution, and then add 0.1g / L BC / PHB composite material to 100mL Ni 2+ Solution and Pb 2+ The solution was shaken at 30° for 2 h. 2+ Solution and Pb 2+ The solution was filtered with a 0.22 μm filter head, and the filtrate was tested for Ni under an atomic absorption spectrometer ICP-3500 2+ and Pb2+ residual concentration.
[0088] Performance test results: Ni 2+ and Pb 2+ The residual concentrations of Ni 2 + and Pb 2+ The adsorption capacities are 22 mg / g and 78 mg / g respectively.
[0089] Comparative Example 9
[0090] Regenerated bacterial cellulose for Ni 2+ , Pb 2+ Study on adsorption performance:
[0091] S1. Solvent preparation: 7 wt % NaOH and 12 wt % Urea were prepared with deionized water (45 mL);
[0092] S2. Dissolution of bacterial cellulose: 0.9 g of bacterial cellulose was added to the NaOH / Urea solution in step S1, and dissolved under magnetic stirring at -10°C for 2.5 h until the solution was transparent and colorless;
[0093] S3, regenerating the bacterial cellulose in step S2 with 0.5% H2SO4 solution (V(H2SO4):V 混合溶液 =1:3); finally, wash with deionized water until neutral and dry.
[0094] Take the above materials to conduct heavy metal ion adsorption test: prepare 10 mg / L Ni 2+ Solution and Pb 2+ solution, and then add 0.1g / L of the above materials to 100mL Ni 2+ Solution and Pb 2+ The solution was shaken at 30° for 2 h. 2+ Solution and Pb 2+ The solution was filtered with a 0.22 μm filter head, and the filtrate was tested for Ni under an atomic absorption spectrometer ICP-3500 2+ and Pb 2+ residual concentration.
[0095] Performance test results: Ni 2+ and Pb 2+ The residual concentrations of Ni 2 + and Pb 2+ The adsorption capacities are 5 mg / g and 27 mg / g respectively.
[0096] Comparative Example 10
[0097] PHB to Ni 2+ , Pb 2+ Study on adsorption performance:
[0098] S1. Solvent preparation: 7 wt % NaOH and 12 wt % Urea were prepared with deionized water (45 mL);
[0099] S2, add 1.2g of dried R.eutropha H16, stir at room temperature for 12h until the solution turns bright yellow;
[0100] S3, regenerate the PHB in step S2 with 0.5% H2SO4 solution (V(H2SO4):V 混合溶液 =1:3); finally, wash with deionized water until neutral and dry.
[0101] Take the above materials to conduct heavy metal ion adsorption test: prepare 10 mg / L Ni 2+ Solution and Pb 2+ solution, and then add 0.1g / L of the above materials to 100mL Ni 2+ Solution and Pb 2+ The solution was shaken at 30° for 2 h. 2+ Solution and Pb 2+ The solution was filtered with a 0.22 μm filter head, and the filtrate was tested for Ni under an atomic absorption spectrometer ICP-3500 2+ and Pb 2+ residual concentration.
[0102] Performance test results: Ni 2+ and Pb 2+ The residual concentrations of Ni 2 + and Pb 2+ The adsorption capacities are 17 mg / g and 42 mg / g respectively.
[0103] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a BC / PHB composite material for heavy metal ion removal, characterized in that: Bacterial cellulose and R.eutropha H16 was dissolved in alkaline solution in turn, so that bacterial cellulose and R.eutropha The PHB produced by H16 is compound; The preparation method of the BC / PHB composite material with heavy metal ions removed comprises the following steps: S1. Solvent preparation: 7 wt% NaOH and 12 wt% Urea were prepared with deionized water; S2. Dissolution of bacterial cellulose: Add bacterial cellulose to the NaOH / Urea solution in step S1, and dissolve under low temperature magnetic stirring until the solution becomes transparent and colorless; S3, add dried R.eutropha H16, stirred at room temperature until the solution turned bright yellow; S4, regenerating the bacterial cellulose / poly 3-hydroxybutyrate composite material in step S3 with a 0.5% H2SO4 solution; finally washing with deionized water until neutral and drying; In the step S2, the dissolution temperature of bacterial cellulose is -10°C and the dissolution time is 2-3 hours.
2. The method for preparing the BC / PHB composite material for heavy metal ion removal according to claim 1, characterized in that: The bacterial cellulose R.eutropha The mass ratio of H16 is 0.1-10:
1.
3. The method for preparing the BC / PHB composite material for heavy metal ion removal according to claim 1, characterized in that: In step S4, the volume ratio of the H2SO4 solution to the composite material solution is 1:
3.
4. The method for preparing the BC / PHB composite material for heavy metal ion removal according to claim 1, characterized in that: In the step S3, R.eutropha The saponification time of H16 in NaOH / Urea solution is 10-12h.
5. The method for preparing the BC / PHB composite material for heavy metal ion removal according to claim 1, characterized in that: Said R.eutropha The culture time of H16 is 72h.
6. Use of the composite material prepared by any one of claims 1 to 5 in the removal of heavy metal ions, characterized in that: The heavy metal ions are divalent nickel ions or divalent lead ions.
7. A method for using the composite material prepared by any one of claims 1 to 5, characterized in that: The BC / PHB composite material was added to the solution to be adsorbed and shaken at room temperature.
8. The method of use according to claim 7, characterized in that: The pH value of the solution to be adsorbed is 6.