Palladium-free chemical copper plating method on the surface of flexible nanofiber membrane

By performing plasma treatment and silver-catalyzed electroless copper plating process on the flexible nanofiber film, the problems of uneven copper plating and poor conductivity are solved, and the preparation of high-performance flexible conductive film with excellent electromagnetic shielding and bending resistance is achieved performance, suitable for electronic device applications.

CN114411414BActive Publication Date: 2024-10-25WUHAN TEXTILE UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202210078721.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-24
Publication Date
2024-10-25
Estimated Expiration
2042-01-24

AI Technical Summary

Technical Problem

The existing electroless copper plating process has problems such as uneven copper plating, poor conductivity, poor electromagnetic shielding, and easy peeling off of the coating. Especially when using polytetrafluoroethylene materials, uneven carboxyl groups lead to low bonding strength, resulting in poor product performance.

Method used

Using a palladium-free chemical copper plating method on the surface of a flexible nanofiber membrane, a polyvinyl alcohol-ethylene copolymer nanofiber membrane is prepared through plasma treatment and silver catalysis, increasing surface active sites, uniformly grafting carboxyl groups, and forming a dense copper coating. Electroless copper plating is performed using silver ions as a catalyst.

Benefits of technology

A flexible conductive film with high conductivity, excellent electromagnetic shielding efficiency, and good bending resistance has been realized. The process is simple, low-cost, easy for industrial production, and solves the problems of uneven plating and poor conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114411414B_ABST
    Figure CN114411414B_ABST
Patent Text Reader

Abstract

The present invention provides a method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane, comprising the following steps: uniformly spraying a polyvinyl alcohol-ethylene copolymer nanofiber suspension having a concentration of 0.5wt%-3.0wt% on the surface of a substrate, and drying to obtain a nanofiber membrane; treating the obtained nanofiber membrane with plasma, immersing it in an acrylic acid aqueous solution having a concentration of 5wt%-20wt%, washing and drying, and obtaining a modified nanofiber membrane; placing the obtained modified nanofiber membrane in a silver nitrate solution for 20-50min, washing and drying, and obtaining an activated nanofiber membrane; placing the obtained activated nanofiber membrane in a chemical plating solution, treating it at 60-80°C for 1-3h, washing and drying, and obtaining a flexible conductive film. The present invention is to modify the nanofiber membrane of a special structure so that acrylic acid is uniformly combined on the surface of the nanofiber membrane, and the obtained flexible conductive film has excellent performance after being treated with activated copper plating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electronic materials, and in particular to a palladium-free chemical copper plating method on the surface of a flexible nanofiber membrane. Background Art

[0002] With the rapid development of electronic technology, copper clad laminate, as the most basic material of PCB, has a significant growth trend in demand for high-performance flexible copper clad laminate. Copper clad laminate is a composite material composed of metal copper and polymer, which is mainly prepared by lamination, coating, vacuum sputtering, chemical copper plating and other methods.

[0003] Among them, polymers are generally polyester, polyimide, polyolefin, etc. Polyvinyl alcohol-ethylene copolymer (PVA-co-PE) film has excellent properties such as large specific surface area, high porosity, tortuous pore structure and high filtration accuracy. The flexible nanofiber copper film prepared by surface chemical copper plating has low dielectric constant and low dielectric loss factor. It is an ideal high-frequency microwave dielectric material and can be used in electronic products such as navigation equipment, aircraft instruments, digital cameras, LCD TVs, and laptops.

[0004] At present, the most commonly used preparation method for copper clad laminates is chemical copper plating. The steps of chemical copper plating are generally degreasing, modification, activation and chemical plating. During the activation process, although the conventional sodium-naphthalene tetrahydrofuran solution chemical modification can significantly improve the surface energy of the nanofiber film, the modification process will produce substances that damage the environment and the operation risk index is high; although the high-energy radiation grafting modification method has the advantages of easy control of the grafting rate and no need for initiators, the radiation amount is not easy to control and it is easy to cause uncontrollable damage to the physical and chemical properties of the material. In the chemical copper plating process, the traditional catalyst is a palladium catalyst. Since palladium is expensive, the cost is relatively high in practical applications. There are reports of using silver catalysts instead of palladium catalysts.

[0005] The patent application number CN201610899123.2 discloses a palladium-free chemical copper plating method on the surface of polytetrafluoroethylene materials, which uses low-temperature plasma grafting modification to introduce a large number of carboxyl groups on the surface of polytetrafluoroethylene materials, and the copper-plated layer is firmly bonded to the surface of the material through chemical bonds. The surface energy of the polytetrafluoroethylene material used in this method is extremely low, and the film structure is relatively simple. The modification effect is not good through low-temperature plasma modification treatment. When the carboxyl groups are introduced into the activated polytetrafluoroethylene material, there are problems such as uneven carboxyl groups and low bonding strength between the two, which will lead to uneven copper plating, poor conductivity, and poor electromagnetic shielding of the final product.

[0006] In view of this, it is necessary to design an improved palladium-free chemical copper plating method on the surface of flexible nanofiber membrane to solve the above problems. Summary of the invention

[0007] The purpose of the present invention is to provide a palladium-free chemical copper plating method for a flexible nanofiber membrane surface, so as to solve the problems existing in the existing chemical copper plating process, such as uneven copper plating, poor conductivity, poor electromagnetic shielding, and easy detachment of the coating.

[0008] To achieve the above-mentioned object of the invention, the present invention provides a method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane, comprising the following steps:

[0009] S1. Preparation of nanofiber membrane: a polyvinyl alcohol-ethylene copolymer nanofiber suspension having a concentration of 0.5wt%-3.0wt% is uniformly sprayed on the surface of a pre-washed substrate, and dried to form a film to obtain a nanofiber membrane;

[0010] S2. Nanofiber membrane modification: The nanofiber membrane prepared in step S1 is treated with plasma, immersed in an acrylic acid aqueous solution with a concentration of 5wt%-20wt% at a bath ratio of 1:2-1:5, washed and dried to obtain a modified nanofiber membrane;

[0011] S3. Activation of the nanofiber membrane: placing the modified nanofiber membrane prepared in step S2 in a silver nitrate solution at a bath ratio of 1:1-1:8 for 20-50 min, washing and drying to obtain an activated nanofiber membrane;

[0012] S4. Copper plating of nanofiber membrane: the activated nanofiber membrane prepared in step S3 is placed in a chemical plating solution at a bath ratio of 1:1-1:5, treated at 60-80°C for 1-3h, washed and dried to obtain a flexible conductive membrane.

[0013] As a further improvement of the present invention, the diameter of the polyvinyl alcohol-ethylene copolymer nanofibers in step S1 is 50nm-800nm.

[0014] As a further improvement of the present invention, the duration of the plasma treatment in step S2 is 2 min-20 min.

[0015] As a further improvement of the present invention, the treatment time in the acrylic acid aqueous solution is 2-12 hours.

[0016] As a further improvement of the present invention, the pre-washing treatment of the substrate in step S1 is to place the substrate in a solution of detergent, sodium carbonate and deionized water in a mass ratio of 1:3:1000, treat it in a water bath at 80°C for 1 hour, take it out and wash it with deionized water until it is neutral, and dry it at 60°C for 1 hour.

[0017] As a further improvement of the present invention, the concentration of the silver nitrate solution in step S3 is 1-2 g / L.

[0018] As a further improvement of the present invention, the chemical plating solution in step S4 is a mixture of copper sulfate pentahydrate, disodium ethylenediaminetetraacetate dihydrate, potassium sodium tartrate, sodium hydroxide, potassium ferrocyanide dihydrate, 2,2'-bipyridine and 37 wt% formaldehyde.

[0019] As a further improvement of the present invention, the concentration of each substance in the chemical plating solution is 16 g / L copper sulfate pentahydrate, 19.5 g / L disodium ethylenediaminetetraacetic acid dihydrate, 14 g / L potassium sodium tartrate, 14.5 g / L sodium hydroxide, 0.01 g / L potassium ferrocyanide dihydrate, 0.02 g / L 2,2'-bipyridine, and 5 mL / L 37 wt% formaldehyde.

[0020] As a further improvement of the present invention, the conductivity of the flexible conductive film is as high as 4897.1s / cm, the electromagnetic shielding effectiveness is as high as 58dB, and the absorption efficiency is more than 90%.

[0021] As a further improvement of the present invention, the substrate in step S1 includes one or more of polyethylene non-woven fabric and polypropylene non-woven fabric.

[0022] The beneficial effects of the present invention are:

[0023] (1) The present invention provides a method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane, wherein polyvinyl alcohol-ethylene copolymer nanofibers are made into a polyvinyl alcohol-ethylene copolymer nanofiber suspension, and the suspension is evenly sprayed on the surface of a substrate, so that individual fibers are cross-linked to varying degrees to form a nanofiber membrane with a special pore size, pores, and pore structure. On the one hand, the nanofiber membrane has a microporous structure, a large specific surface area, a high porosity, and a tortuous pore structure; on the other hand, the surface of the PVA-co-PE nanofiber membrane contains abundant highly active hydroxyl groups, which can effectively increase its surface polarity and surface energy. The special surface structure of the PVA-co-PE nanofiber membrane provides a larger specific surface area and higher activity for plasma treatment, making the plasma modification treatment more sufficient. The plasma-modified PVA-co-PE nanofiber membrane can provide a rougher surface and more binding sites, so that the surface of the nanofiber membrane is evenly grafted with highly active carboxyl groups through chemical bonds. The presence of carboxyl groups enables silver ions to be evenly grafted onto the surface of the nanofiber membrane through coordination, providing active centers for the copper plating reaction, making the final flexible conductive film dense and uniform, with high conductivity and low surface resistance, reaching the conductor level, with excellent conductivity and electromagnetic shielding properties.

[0024] (2) The present invention provides a palladium-free chemical copper plating method on the surface of a flexible nanofiber membrane. The nanofiber membrane is used as the substrate to prepare a flexible conductive membrane with excellent bending resistance, which can be reused and is not easily damaged, thus solving the problem of poor bending resistance of conventional electronic copper-clad laminates. The plasma-induced grafting method is adopted, which is pollution-free, easy to operate and low in cost, thus solving the problem that the conductive membrane materials for electronic use are difficult to promote due to the cost. The microporous structure of the nanofiber membrane and the copper plating layer on the surface give the material excellent electromagnetic shielding performance, thus solving the problem of mutual interference between electronic components. Based on the copper-plated conductive material on the surface of the flexible nanofiber membrane, the hydrophobicity is improved, which is of great significance for expanding the application range of electronic components.

[0025] (3) The present invention provides a palladium-free chemical copper plating method on the surface of a flexible nanofiber membrane. Instead of using traditional palladium catalysis, silver catalysis is used. The method is simple to operate, the process is easy to control, it is economical and environmentally friendly, and it is easy to be mass-produced industrially. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The present invention is a flow chart of the method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane.

[0027] Figure 2 This is a scanning electron microscope image of the flexible conductive film and nanofiber membrane substrate prepared in Example 1.

[0028] Figure 3 This is the conductivity diagram of the flexible conductive film prepared in Example 1.

[0029] Figure 4 This is a diagram showing the electromagnetic shielding performance of the flexible conductive film prepared in Example 1.

[0030] Figure 5 This is a diagram of the water contact angle of the flexible conductive film prepared in Example 1. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0032] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0033] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0034] See also Figure 1 As shown, the present invention provides a method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane, comprising the following steps:

[0035] S1. Nanofiber membrane preparation:

[0036] The substrate was placed in a solution of detergent, sodium carbonate and deionized water in a mass ratio of 1:3:1000, treated in a water bath at 80°C for 1 hour, the substrate was taken out and washed with deionized water until neutral, and dried at 60°C for 1 hour to obtain a pre-washed substrate. This process can remove oil stains and other impurities on the surface of the substrate, providing conditions for the subsequent firm coating of the polyvinyl alcohol-ethylene copolymer (PVA-co-PE) nanofiber suspension.

[0037] Wherein, the substrate includes one or more of polyethylene non-woven fabric and polypropylene non-woven fabric.

[0038] Polyvinyl alcohol-ethylene copolymer nanofibers with a diameter of 50nm-800nm ​​are configured into a polyvinyl alcohol-ethylene copolymer nanofiber suspension with a concentration of 0.5wt%-3.0wt%, and the suspension is evenly sprayed on the surface of a pre-washed substrate. After drying, a layer of PVA-co-PE film is formed on the surface of the substrate to obtain a nanofiber membrane.

[0039] S2. Nanofiber membrane modification:

[0040] The nanofiber membrane prepared in step S1 is treated with plasma for 2-20 minutes, immersed in an acrylic acid aqueous solution with a concentration of 5wt%-20wt% at a bath ratio of 1:2-1:5 for 2-12 hours, and washed and dried to obtain a modified nanofiber membrane.

[0041] The PVA-co-PE nanofiber membrane has a microporous structure, with a large specific surface area, high porosity, and a tortuous pore structure. In addition, the surface of the PVA-co-PE nanofiber membrane contains abundant highly active hydroxyl groups, and the polar group hydroxyl groups can effectively increase its surface polarity and surface energy. Therefore, the special surface structure of the PVA-co-PE nanofiber membrane provides a larger specific surface area for plasma treatment, making the plasma modification treatment more sufficient. During the plasma treatment process, the PVA-co-PE nanofiber membrane is etched, which not only increases the surface roughness and further increases its specific surface area, but also makes the hydroxyl content on the surface of the PVA-co-PE nanofiber membrane higher, increasing the active sites on the surface.

[0042] When the plasma-treated PVA-co-PE nanofiber membrane is further placed in an acrylic acid solution for treatment, more acrylic acid adheres to the surface of the nanofiber membrane due to the increase in the surface roughness of the nanofiber membrane and the increase in the surface hydroxyl content, and the abundant hydroxyl groups in the PVA-co-PE molecules are bonded to the carboxyl groups in the acrylic acid molecules through hydrogen bonds, and finally a large amount of acrylic acid is firmly bonded to the surface of the nanofiber membrane to obtain a modified nanofiber membrane. A large number of polar group carboxyl groups can further increase the surface polarity and surface energy of the nanofiber membrane, greatly improving the chemical activity of the modified nanofiber membrane.

[0043] In addition, since hydrophilic polyvinyl alcohol exists in the PVA-co-PE molecule, and acrylic acid liquid is a hydrophilic substance; and the PVA-co-PE membrane itself has a porous structure, a large amount of acrylic acid is further grafted onto the surface of the nanofiber membrane.

[0044] S3. Nanofiber membrane activation:

[0045] The modified nanofiber membrane prepared in step S2 is placed in a silver nitrate solution with a concentration of 1-2 g / L at a bath ratio of 1:1-1:8 for 20-50 min, and then washed and dried to obtain an activated nanofiber membrane.

[0046] In this process, silver ions coordinate (electrostatically) with carboxyl groups in acrylic acid, so that silver ions are firmly loaded on the surface of modified nanofiber membrane. Silver ions not only provide activation centers for modified nanofiber membrane, but also serve as catalysts for subsequent copper plating, which can accelerate the chemical plating reaction.

[0047] S4. Nanofiber membrane copper plating:

[0048] The activated nanofiber membrane prepared in step S3 is placed in a chemical plating solution at a bath ratio of 1:1-1:5, and treated at 60-80°C for 1-3h to subject the activated nanofiber membrane that adsorbs silver ions to a chemical copper plating reaction, thereby depositing a copper layer on the surface of the PVA-co-PE nanofiber membrane. After washing and drying, a flexible conductive membrane is obtained.

[0049] The composition and concentration of the chemical plating solution are as follows: 16 g / L copper sulfate pentahydrate, 19.5 g / L disodium ethylenediaminetetraacetic acid dihydrate, 14 g / L potassium sodium tartrate, 14.5 g / L sodium hydroxide, 0.01 g / L potassium ferrocyanide dihydrate, 0.02 g / L 2,2'-bipyridine, 5 mL / L 37 wt% formaldehyde, and the rest is water.

[0050] Specifically, copper sulfate is the main raw material for providing the required plating metal; potassium sodium tartrate and disodium ethylenediaminetetraacetic acid dihydrate can form complexes with copper ions, providing long-term stable conditions for copper ions; formaldehyde can reduce divalent copper ions to metallic copper; sodium hydroxide provides a suitable pH value for the reduction reaction; potassium ferrocyanide dihydrate can properly control the reduction rate to prevent the plating solution from violently decomposing and causing the plating solution to fail; 2,2'-bipyridine is used as a brightener to make the surface of the final copper plating layer bright.

[0051] In the presence of silver ion catalyst, copper ions are reduced to metallic copper by formaldehyde. When metallic copper begins to deposit on the surface, the copper layer acts as a catalyst for further reactions, allowing chemical copper plating to continue.

[0052] The present invention is described in detail below through a number of embodiments:

[0053] Example 1

[0054] A method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane comprises the following steps:

[0055] S1. Nanofiber membrane preparation:

[0056] The flexible polyethylene non-woven fabric substrate was placed in a solution of detergent, sodium carbonate and deionized water in a mass ratio of 1:3:1000, treated in a water bath at 80°C for 1 hour, the polyethylene non-woven fabric was taken out and washed with deionized water until neutral, and dried at 60°C for 1 hour to obtain a pre-washed flexible polyethylene non-woven fabric.

[0057] PVA-co-PE nanofibers with a diameter of 200 nm are configured into a PVA-co-PE nanofiber suspension with a concentration of 1 wt%, and the suspension is evenly sprayed on the surface of a pre-washed flexible polyethylene non-woven fabric. After drying, a layer of PVA-co-PE porous nanofiber membrane is formed on the surface of the polyethylene non-woven fabric to obtain a nanofiber membrane. The thickness of the obtained nanofiber membrane is 50 μm.

[0058] like Figure 2 The scanning electron microscope image of the original membrane morphology shown in the middle left figure has a scale of 5μm. The PVA-co-PE nanofibers are cross-linked with each other and have uniform pores, which provide conditions for subsequent plasma treatment and acrylic acid grafting.

[0059] Due to the presence of similar polyethylene segments in PVA-co-PE molecules and polyolefin molecules, the molecules of the two are arranged relatively neatly and the bonding force between the two is very strong, so that the PVA-co-PE nanofiber membrane is firmly coated on the surface of the polyolefin non-woven fabric.

[0060] S2. Nanofiber membrane modification:

[0061] The nanofiber membrane prepared in step S1 was treated with plasma for 5 minutes, immersed in a 10 wt % acrylic acid aqueous solution at a bath ratio of 1:2 for 10 hours, and washed and dried to obtain a modified nanofiber membrane.

[0062] S3. Nanofiber membrane activation:

[0063] The modified nanofiber membrane (4 cm × 3 cm) prepared in step S2 was placed in a 1.5 g / L silver nitrate solution at a bath ratio of 1:5 for 30 min, and the unadsorbed Ag was washed away with deionized water. + After drying, an activated nanofiber membrane is obtained.

[0064] The preparation method of silver nitrate solution is as follows: weigh 0.15 g of silver nitrate, add deionized water to dissolve it, and dilute to 100 mL for later use.

[0065] S4. Nanofiber membrane copper plating:

[0066] The activated nanofiber membrane (4 cm×3 cm) prepared in step S3 was placed in a chemical plating solution at a bath ratio of 1:2 and treated at 70°C for 2 h to perform a chemical copper plating reaction on the activated nanofiber membrane that adsorbed silver ions, thereby depositing a copper layer on the surface of the PVA-co-PE membrane. After washing and drying, a flexible conductive membrane was obtained.

[0067] The preparation method of the chemical plating solution is as follows: 16.00 g of sulfuric acid pentahydrate, 19.50 g of disodium ethylenediaminetetraacetate dihydrate, and 14.00 g of potassium sodium tartrate are weighed and placed in a beaker, deionized water is added to dissolve them, and then 14.50 g of sodium hydroxide is added. After it is fully dissolved, 0.01 g of potassium ferrocyanide dihydrate, 0.02 g of 2,2'-bipyridine, and 5 mL of 37 wt% formaldehyde solution are added to make up to 1000 mL for use.

[0068] like Figure 2 The scanning electron microscope image of the copper-plated film morphology shown in the middle right figure has a scale of 10μm. A dense copper film is formed on the nanofiber membrane, which improves its electromagnetic shielding performance, indicating that the flexible conductive film obtained by this process has good performance.

[0069] like Figure 3 As shown in the conductivity diagram, after copper plating, the conductivity of the nanofiber membrane increased from 386.3s / cm to 4897.1s / cm. The conductivity was greatly improved, indicating that it has a good conductive effect.

[0070] like Figure 4The electromagnetic shielding performance diagram shown in the figure (measured by a vector network analyzer) shows that EMI shielding refers to the attenuation of electromagnetic wave energy caused by absorption or reflection of the material. The greater the attenuation value, the better the shielding performance. SE represents the shielding effectiveness of the shielding material. SE (A) represents the attenuation of electromagnetic wave energy caused by absorption of the material. SE (R) represents the attenuation of electromagnetic wave energy caused by reflection of the material. SE (T) represents the total attenuation of electromagnetic wave energy caused by absorption and reflection of the material, i.e., the electromagnetic shielding effectiveness of the material. As can be seen from the figure, the electromagnetic shielding effectiveness of the flexible conductive film is as high as 58dB, of which the absorption efficiency is more than 90%, indicating that the obtained flexible conductive film has good absorption of electromagnetic waves. In addition, it also shows that the appropriate amount of holes on the surface of the nanofiber film and the conductive flexible film can increase the reflection process of electromagnetic waves, thereby improving the electromagnetic shielding performance from both absorption and reflection.

[0071] like Figure 5 The water contact angle diagram of the flexible conductive film shown in the figure shows that the original film is hydrophilic and water can wet the original film, while the prepared flexible conductive film is difficult to be wetted by water and its hydrophobicity is greatly improved, which is of great significance for expanding the application range of electronic components.

[0072] Embodiment 2-6

[0073] A method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane is disclosed. Compared with Example 1, the difference lies in that in step S1, the concentration of the PVA-co-PE nanofiber suspension and the diameter of the PVA-co-PE nanofiber are different. The rest is roughly the same as Example 1 and will not be repeated here.

[0074] The performance of the flexible conductive films prepared in Examples 1-6 was tested, and the results are shown in Table 1:

[0075] Table 1 Performance test of the flexible conductive films prepared in Examples 1-6

[0076] Example Concentration (wt%) Diameter(nm) Conductivity(s / cm) Electromagnetic shielding effectiveness (dB) Example 1 1 200 4897.1 58.0 Example 2 0.5 200 3508.7 35.6 Example 3 3 200 5107.5 60.4 Example 4 1 50 4386.8 55.2 Example 5 1 400 5604.2 62.7 Example 6 1 800 5237.1 61.2

[0077] It can be seen from Table 1 that with the increase of the diameter of the nanofibers, the conductivity and electromagnetic shielding properties of the flexible conductive film both increase first and then decrease; with the increase of the concentration of the nanofiber suspension, the conductivity and electromagnetic shielding properties of the flexible conductive film both increase.

[0078] When the diameter of the nanofiber is small (Example 4), the fiber membrane generated after the intersection of different fibers is relatively dense, and there are more pores on the surface of the nanofiber membrane, resulting in a large degree of surface roughness. After copper is deposited, a discontinuous copper layer is easily formed on the surface due to the presence of a large number of pores, resulting in a decrease in electrical conductivity and poor electromagnetic shielding performance.

[0079] As the diameter of the nanofiber increases (Examples 1 and 5), the pore density and pore size of the fiber membrane decrease after different fibers intersect, and the deposited copper easily covers the pores to form a flat copper layer, making the copper membrane denser and free of rough faults, thereby improving the conductivity of the flexible conductive membrane. At the same time, the flexible conductive membrane is denser, so that it absorbs more electromagnetic waves. In addition, the appropriate amount of pores in the nanofiber membrane and the copper-plated layer of the conductive membrane increase the reflection of electromagnetic waves by the flexible conductive membrane, so the electromagnetic shielding performance of the flexible conductive membrane is better.

[0080] As the diameter of the nanofibers increases further (Example 6), the pore depth of the nanofiber membrane increases, the deposited copper is insufficient to cover the holes, and the thicker fibers will form ridges, causing copper faults, making the copper distribution of the final flexible conductive membrane uneven, resulting in poor conductivity, and thus weakening its electromagnetic shielding performance.

[0081] As the concentration of nanofibers increases, the surface structure of the nanofiber membrane is affected, which in turn affects the conductivity and electromagnetic shielding performance of the conductive membrane. When the concentration is low, multiple coatings are required to achieve the same thickness, and the intersection between the fibers increases, resulting in more holes in the nanofiber membrane and difficulty in forming a continuous copper layer, which leads to poor performance of the flexible conductive membrane; when the concentration is high, the surface of the nanofiber membrane is smoother and it is easier to form a continuous copper layer, which leads to better performance of the flexible conductive membrane.

[0082] Embodiment 7-11

[0083] A method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane is disclosed. Compared with Example 1, the difference lies in that in step S2, the plasma treatment time and the concentration of the acrylic acid solution are different. The rest is substantially the same as Example 1 and will not be repeated here.

[0084] The performance of the flexible conductive films prepared in Examples 7-11 was tested, and the results are shown in Table 2:

[0085] Table 2 Performance test of flexible conductive films prepared in Examples 7-11

[0086] Example Time (min) Concentration (wt%) Conductivity(s / cm) Electromagnetic shielding effectiveness (dB) Example 1 5 10 4897.1 58.0 Example 7 2 10 4302.4 52.6 Example 8 10 10 4985.2 59.4 Example 9 20 10 4632.7 55.8 Example 10 5 5 4536.8 54.4 Embodiment 11 5 20 5243.7 60.4

[0087] As shown in Table 2, as the plasma treatment time increases, the conductivity and electromagnetic shielding performance of the flexible conductive film first increase and then decrease. This is mainly because as the plasma treatment time increases, the etching degree and roughness of the nanofiber membrane surface increase, which not only provides more attachment sites for acrylic acid, but also increases the number of hydroxyl groups exposed on the surface, further providing more binding sites for acrylic acid, so that acrylic acid is evenly bonded to the surface of the nanofiber membrane, providing conditions for the subsequent grafting of silver ions, and then making the copper deposition of the conductive film more uniform and dense, so that its conductivity performance is better; plasma treatment changes the surface structure of the nanofiber membrane, and the special surface structure of the nanofiber membrane and the uniform and dense copper plating layer of the conductive membrane make its electromagnetic shielding performance better. If the plasma treatment time is too long, since the nanofiber membrane itself has a special pore structure, long-term etching will destroy the original structure of the nanofiber membrane, so that the performance of the final flexible conductive membrane is poor.

[0088] As the concentration of acrylic acid solution increases, the conductivity and electromagnetic shielding performance of the flexible conductive film first increase and then remain basically unchanged. This is because as the concentration of acrylic acid solution increases, the amount of acrylic acid grafted on the surface of the nanofiber membrane increases, providing more binding sites for silver ions, thereby allowing copper to be evenly and densely deposited on the surface of the nanofiber membrane, thereby making its performance better. However, as the concentration of acrylic acid solution increases further, on the one hand, due to steric hindrance, more acrylic acid cannot be grafted on the surface of the nanofiber membrane. On the other hand, silver ions only act as catalysts to promote the copper plating reaction. This process does not require too much silver ions. Therefore, the copper finally deposited on the surface of the nanofiber membrane remains basically unchanged, making its performance stable.

[0089] Examples 12-14

[0090] A method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane is disclosed. Compared with Example 1, the difference lies in that in step S4, the copper plating time is different, and the rest is substantially the same as Example 1 and will not be repeated here.

[0091] The performance of the flexible conductive films prepared in Examples 12-14 was tested, and the results are shown in Table 3:

[0092] Table 3 Performance test of flexible conductive films prepared in Examples 12-14

[0093] Example Time (h) Conductivity(s / cm) Electromagnetic shielding effectiveness (dB) Example 1 2 4897.1 58.0 Example 12 1 3824.1 43.7 Embodiment 13 3 5046.2 60.5 Embodiment 14 4 5085.7 60.6

[0094] It can be seen from Table 3 that with the increase of copper plating time, the conductivity and electromagnetic shielding performance of the flexible conductive film both increase. The increase in conductivity indicates that with the increase of copper plating time, the copper deposited on the surface of the nanofiber is increasing; the increase in electromagnetic shielding performance indicates that the structure of the nanofiber membrane and the structure of the copper-plated layer of the conductive film achieve better synergy.

[0095] However, after the copper plating time increases to a certain extent, as the copper plating time increases, the conductivity and electromagnetic shielding properties of the flexible conductive film basically tend to be stable.

[0096] Comparative Example 1

[0097] A method for palladium-free chemical copper plating on the surface of a PVA-co-PE film. Compared with Example 1, the difference lies in that the structure of the PVA-co-PE film used is different. A film with the same thickness as that in Example 1 is prepared by a high-temperature molding method, and then the film is pressed onto a polyethylene non-woven fabric. The rest is roughly the same as Example 1 and will not be repeated here.

[0098] The conductivity of the obtained flexible conductive film is 500s / cm, and the electromagnetic shielding performance is 5.6dB. The conductivity and electromagnetic shielding performance are obviously poor, indicating that the PVA-co-PE film prepared in Comparative Example 1 does not have a special structure of pore size and porosity, and the surface structure of the film is single, which makes the performance of the final flexible conductive film poor.

[0099] In summary, the present invention provides a method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane, by uniformly spraying a polyvinyl alcohol-ethylene copolymer nanofiber suspension on the surface of a substrate, so that different degrees of cross-linking occur between single fibers, forming a nanofiber membrane with a special structure; and the surface of the PVA-co-PE nanofiber membrane contains abundant highly active hydroxyl groups, which can effectively increase its surface polarity and surface energy. The special surface structure of the PVA-co-PE nanofiber membrane provides a larger specific surface area and higher activity for plasma treatment, making the plasma modification treatment more sufficient. The plasma-modified PVA-co-PE nanofiber membrane can provide a rougher surface and more binding sites, so that the surface of the nanofiber membrane is uniformly grafted with highly active carboxyl groups through chemical bonds. The presence of carboxyl groups allows silver ions to be uniformly grafted to the surface of the nanofiber membrane through coordination, providing active centers for the copper plating reaction, so that the final flexible conductive membrane is dense and uniform, with excellent performance. The method is simple to operate, the process is easy to control, it is economical and environmentally friendly, and it is easy to mass-produce industrial products. The resulting flexible conductive film has excellent anti-bending properties; high electrical conductivity and low surface resistance, reaching the conductor level; good electromagnetic shielding performance; and strong hydrophobicity.

[0100] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane, characterized in that: The steps include: S1. Preparation of nanofiber membrane: spraying a polyvinyl alcohol-ethylene copolymer nanofiber suspension with a concentration of 0.5wt%-3.0wt% uniformly on the surface of a pre-washed substrate, and drying to form a film to obtain a nanofiber membrane; the substrate comprises one or more of polyethylene non-woven fabric and polypropylene non-woven fabric; the diameter of the polyvinyl alcohol-ethylene copolymer nanofiber is 50nm-800nm; S2. Modification of nanofiber membrane: The nanofiber membrane prepared in step S1 is treated with plasma, immersed in an acrylic acid aqueous solution with a concentration of 5wt%-20wt% at a bath ratio of 1:2-1:5, washed and dried to obtain a modified nanofiber membrane; the plasma treatment time is 2-20min; the treatment time in the acrylic acid aqueous solution is 2-12h; the surface of the nanofiber membrane contains highly active hydroxyl groups, and the nanofiber membrane is uniformly grafted with highly active carboxyl groups through chemical bonds; S3. Activation of the nanofiber membrane: placing the modified nanofiber membrane prepared in step S2 in a silver nitrate solution at a bath ratio of 1:1-1:8 for 20-50 min, washing and drying to obtain an activated nanofiber membrane; S4. Copper plating of nanofiber membrane: place the activated nanofiber membrane prepared in step S3 in a chemical plating solution at a bath ratio of 1:1-1:5, treat at 60-80°C for 1-3h, wash and dry to obtain a flexible conductive membrane; the conductivity of the flexible conductive membrane is as high as 4897.1s / cm, the electromagnetic shielding effectiveness is as high as 58dB, and the absorption efficiency is more than 90%.

2. The method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane according to claim 1, characterized in that: The pre-washing treatment of the substrate in step S1 is to place the substrate in a solution of detergent, sodium carbonate and deionized water in a mass ratio of 1:3:1000, treat it in a water bath at 80°C for 1 hour, take it out and wash it with deionized water until it is neutral, and dry it at 60°C for 1 hour.

3. The method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane according to claim 1, characterized in that: The concentration of the silver nitrate solution in step S3 is 1-2 g / L.

4. The method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane according to claim 1, characterized in that: The chemical plating solution in step S4 is a mixture of copper sulfate pentahydrate, disodium ethylenediaminetetraacetate dihydrate, potassium sodium tartrate, sodium hydroxide, potassium ferrocyanide dihydrate, 2,2'-bipyridine and 37 wt % formaldehyde.

5. The method for palladium-free chemical copper plating on the surface of a flexible nanofiber membrane according to claim 4, characterized in that: In the chemical plating solution, the concentrations of various substances are 16 g / L copper sulfate pentahydrate, 19.5 g / L disodium ethylenediaminetetraacetic acid dihydrate, 14 g / L potassium sodium tartrate, 14.5 g / L sodium hydroxide, 0.01 g / L potassium ferrocyanide dihydrate, 0.02 g / L 2,2'-bipyridine, and 5 mL / L 37 wt% formaldehyde.

Citation Information

Cited By

  • Composite film for monitoring piezoelectricity

    CN116176074A

  • Method for reducing chemical copper plating and diffusion plating of laser activated flexible substrate

    CN120193264A