Thickener with fine particle structure that improves the feel during use
The fine particle morphological thickener prepared by PIT polymerization solves the problems of opacity and unstable viscosity of traditional thickeners, achieving morphological maintenance and high stability in the moisture phase, and improving the sense of use.
Patent Information
- Application Number
- CN202080066518.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-10
- Filing Date
- 2020-09-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-09-24
AI Technical Summary
Traditional water dispersion thickeners have problems of opacity, unstable viscosity and poor use during use, especially when developing multiple dosage forms.
The thickener in the form of fine particles is prepared by PIT polymerization. It is converted into a water-in-oil reverse phase emulsion by heating in an oil-in-water emulsion, and polymerization is carried out at opposite temperatures to form a uniform small particle size. crosslinked polymer.
The prepared thickener remains transparent in the moisture phase, with high stability and improved usage, including application and moisture.
Smart Images

Figure CN114423403B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a thickener having a fine particle structure with improved feeling during use. Background Art
[0002] Traditional water-dispersible thickeners have soft and thick spreadability, a reduced finish, and a greater stickiness the more they are used.
[0003] Therefore, an AMPS (Acrylamidopropylmethyl Sulfonic acid)-based thickener having a silky feel has been reported. It is reported that the above-mentioned AMPS-based thickener is usually synthesized by precipitation polymerization (Patent Document 1). If synthesized by the above-mentioned precipitation polymerization method, the thickener particles exist in an amorphous state, and are therefore dispersed in the aqueous phase in an irregular form and swell (swelling), thereby increasing the viscosity of the dosage form and imparting stability. However, the thickener obtained by the above-mentioned precipitation polymerization method is opaque when dispersed in the aqueous phase, and is therefore difficult to apply to transparent dosage forms. Therefore, there is a concern that limitations may arise when developing a variety of dosage forms.
[0004] [Prior art literature]
[0005] [Patent Document]
[0006] 1. European Patent 1746114 Summary of the invention
[0007] Technical issues
[0008] An object of the present invention is to provide a thickener having a fine particle structure with improved feeling during use.
[0009] Technical Solution
[0010] The present invention provides a method for preparing a thickener, comprising:
[0011] The step of preparing an oil-in-water emulsion composition, the oil-in-water emulsion composition comprising an aqueous phase comprising a compound represented by the following Chemical Formula 1 and a crosslinking monomer and a solvent having a solubility parameter of 15 (MPa) 1 / 2 The oil phase of the above non-polar organic solvent;
[0012] The step of heating to above 60° C. to prepare a water-in-oil type reverse emulsion composition; and
[0013] A step of preparing a crosslinked polymer by adding a reaction initiator to carry out a polymerization reaction.
[0014] [Chemical formula 1]
[0015]
[0016] In addition, the present invention relates to a composition comprising the thickener prepared by the above preparation method.
[0017] Effects of the Invention
[0018] In the present invention, the polymerization reaction is carried out in a uniform reverse emulsion phase with a small particle size by using the PIT (phase inversion temperature) polymerization method, so that a thickener in the form of homogeneous fine particles can be prepared. The thickener in the form of spherical particles prepared by the present invention has the following advantages: even if it swells in a water phase, the particle shape is not only maintained, but also the particles are uniformly dispersed, transparent in appearance, and highly stable.
[0019] Unlike most thickeners synthesized by precipitation polymerization, which have a chain-entangled structure in an amorphous form and are dispersed in an aqueous phase, the thickener prepared (polymerized) by the present invention is dispersed in water in the form of fine particles, thereby maintaining the form even in the dosage form. In addition, when applied to the skin, the physical bonding structure between the particles is easily collapsed, thereby improving the feel of use such as spreadability, moisture, and nutrition. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Shown are photographs comparing the transparency of thickeners prepared in Examples of the present invention.
[0021] Figure 2 and Figure 4 Shown are the results of measuring the morphology of spherical fine particles prepared in Examples of the present invention.
[0022] Figure 3 A photograph comparing particles of thickeners prepared in Example 2 of the present invention and Comparative Example 1 is shown.
[0023] Figure 5 The results of measuring the rheological properties of the thickeners prepared in Examples of the present invention are shown.
[0024] Figure 6 Optical images of frost prepared in an example of the present invention are shown. DETAILED DESCRIPTION
[0025] The present invention relates to a method for preparing a thickener, comprising:
[0026] (1) a step of preparing an oil-in-water emulsion composition, the oil-in-water emulsion composition comprising an aqueous phase comprising a compound represented by the following Chemical Formula 1 and a crosslinking monomer and a solvent having a solubility parameter of 15 (MPa): 1 / 2 The oil phase of the above non-polar organic solvent;
[0027] (2) heating to above 60° C. to prepare a water-in-oil type reverse emulsion composition; and
[0028] (3) A step of preparing a crosslinked polymer by adding a reaction initiator to carry out a polymerization reaction.
[0029] [Chemical formula 1]
[0030]
[0031] Next, the configuration of the present invention will be described in detail.
[0032] In the present invention, the thickener is prepared by using the PIT (phase inversion temperature) polymerization method.
[0033] Specifically, in the present invention, the solubility parameter is 15 (MPa). 1 / 2 The above non-polar organic solvent, water, surfactant, specifically a suitable combination of a surfactant with an HLB value of 3 to 8 and a surfactant with an HLB value of 8 to 16, or a surfactant with an HLB value of 5 to 7 and a surfactant with an HLB value of 9 to 11, is used to carry out the polymerization reaction in a uniform reverse emulsion phase with a small particle size by using the PIT (phase inversion temperature) polymerization method, which is an oil-in-water (o / w) emulsion phase at room temperature but is converted into an oil-in-water (w / o) emulsion phase at a certain temperature or above. Thus, in the present invention, a thickener in the form of homogeneous fine particles can be prepared. The thickener in the form of spherical fine particles polymerized in the above manner has the following advantages: even if it swells in the water phase, it not only maintains the shape of the particles, but also the particles are uniformly dispersed, transparent in appearance, and highly stable.
[0034] In the present invention, the "thickener" refers to the cross-linked polymer prepared according to the preparation method of the present invention, and may also refer to a solution in which the cross-linked polymer is dispersed.
[0035] In the present invention, step (1) is to prepare an aqueous phase comprising a compound represented by the following chemical formula 1 and a crosslinking monomer and a solvent having a solubility parameter of 15 (MPa): 1 / 2 The above steps are to prepare an oil-in-water emulsion composition of the oil phase of the non-polar organic solvent.
[0036] The aqueous phase includes a compound represented by the following Chemical Formula 1 and a cross-linking monomer.
[0037] In a specific example, the compound represented by Chemical Formula 1 may be 2-acrylamidopropylmethyl sulfonic acid (AMPS).
[0038] The content of the compound represented by Chemical Formula 1 is not particularly limited, and may be 95 to 99.5 parts by weight relative to the total weight (100 parts by weight) of the compound represented by Chemical Formula 1 and the cross-linking monomer.
[0039] In a specific example, the crosslinking monomer can be a compound having more than 2 acrylate groups, more than 2 acrylamide groups or more than 2 vinyl groups. As such a crosslinking monomer, for example, one or more selected from the group consisting of trimethylolpropane ethoxylate triacrylate (TMPETA), methylenebisacrylamide, divinyl sulfone, divinylbenzene, divinyl ether, divinyl acetylene, polyethylene glycol diacrylate, polyethylene glycol triacrylate and 4-arm-polyethylene glycol tetraacrylate can be used. In the present invention, specifically, trimethylolpropane ethoxylate triacrylate (TMPETA), which is a compound represented by the following chemical formula 2, can be used. The above-mentioned TMPETA, as a compound having three crosslinking points, can increase the molecular weight of the crosslinked product, thereby increasing the viscosity.
[0040] [Chemical formula 2]
[0041]
[0042] The content of the cross-linking monomer is not particularly limited, and may be 0.5 to 5.0 parts by weight relative to the total weight (100 parts by weight) of the compound represented by Chemical Formula 1 and the cross-linking monomer.
[0043] In one embodiment, the solvent of the aqueous phase may be water (distilled water).
[0044] In one specific example, the pH of the aqueous phase may be 5 to 9. The pH may be adjusted using aqueous ammonia.
[0045] In the present invention, the oil phase may contain an organic solvent and a surfactant.
[0046] In one specific example, the organic solvent may have a solubility parameter of 15 (MPa). 1 / 2 The above non-polar organic solvent may be, specifically, a hydrocarbon oil having 7 to 17 carbon atoms, or a linear saturated hydrocarbon oil having 7 to 17 carbon atoms. The above solubility coefficient is well known to those skilled in the art and is generally used as a guide for determining the compatibility and solubility of a substance.
[0047] In the present invention, heptane can be used as the non-polar organic solvent.
[0048] The above-mentioned heptane has a boiling point of 98°C and is not limited in the polymerization process according to the present invention compared with other organic solvents. For hexane (Hexane), which is one of the organic solvents, the boiling point is 68°C, and the synthesis temperature cannot be increased to more than 60°C, so there are many problems in the process. During the process, due to the explosive reaction during the initiator input process, heat is generated, so there is a danger that the temperature inside the reactor rises by about 5-10°C. The method of slowly adding initiators to maintain the constancy of the reaction temperature has the following disadvantages when applied to large-scale production processes: it leads to an increase in process time, thereby increasing production costs. In addition, if heated to above the boiling point, the reactants will collide (bumping), thereby increasing the risk of reactor explosion, so the reaction heat management is a very important factor in large-scale production. Therefore, in the present invention, by using heptane as an organic solvent, the thickener desired by the present invention can be easily prepared without process restrictions.
[0049] In a specific example, as a surfactant, more than one surfactant can be used. The HLB value of the above-mentioned surfactant can be 6 to 14, 7 to 10 or 8 to 9. At this time, the total HLB value refers to the HLB value of the above-mentioned one surfactant when one surfactant is used, and can also refer to the sum of the HLB values of two or more surfactants when two or more surfactants are used. When the above-mentioned total HLB value is less than 6, due to the strong hydrophobicity of the surfactant, it exists as an oil-in-water type reverse emulsion from room temperature, so that polymerization is carried out without a phase inversion process, so the effect of reducing the emulsion size may not be sufficient. In addition, when the total HLB value is more than 14, due to the strong hydrophilicity of the surfactant, the water-in-oil emulsion with the external phase as the water phase is maintained, so that spherical particles are not formed, so there is a concern that the amorphous state of the prepared thickener may increase.
[0050] In one specific example, two surfactants can be used as surfactants. In this case, a surfactant having an HLB value of 3 to 8 and a surfactant having an HLB value of 8 to 16 can be used in combination, or a surfactant having an HLB value of 5 to 7 and a surfactant having an HLB value of 9 to 11 can be used in combination.
[0051] In the present invention, as a surfactant, polyoxyethylene (3) oleyl ether (HLB = 6.6) and polyoxyethylene (6) oleyl ether (HLB = 9.6) can be used in combination. Specifically, polyoxyethylene (3) oleyl ether (HLB = 6.6) and polyoxyethylene (6) oleyl ether (HLB = 9.6) can be used in combination at a weight ratio of 1:1, and the HLB value can be 8.1.
[0052] The content of the above-mentioned surfactant is not particularly limited and can vary according to the type of organic solvent. Specifically, relative to the total weight of the organic solvent (100 parts by weight), the content of the above-mentioned surfactant can be 5 to 30 parts by weight. Within the above-mentioned content range, phase inversion of the emulsion can be performed, and PIT polymerization can be easily performed.
[0053] In one specific example, the weight ratio of the water phase to the oil phase may be 30:70 to 70:30.
[0054] In the present invention, step (2) is a step of heating to above 60° C. to prepare a water-in-oil type reverse emulsion composition.
[0055] The emulsion prepared in step (1) has an oil-in-water type at room temperature, but can be inverted into an oil-in-water type emulsion by heating. The emulsion generated by the above phase inversion can have the effect of reducing the size of the emulsion and has the effect of reducing the particle size of the polymer prepared in the subsequent step.
[0056] In a specific example, the reaction temperature may be 62° C. or higher, 65° C. or higher, 70° C. or higher, or 75° C., and the upper limit may be 100° C. The thickener may be stably prepared within the above temperature range.
[0057] In the present invention, step (3) is a step of preparing a cross-linked polymer by adding a reaction initiator to carry out a polymerization reaction.
[0058] In a specific example, the type of reaction initiator is not particularly limited, as long as it has the ability to initiate free radical polymerization, and can be selected from the group consisting of peroxides and azo compounds, etc. As the above-mentioned peroxide initiator, benzoyl peroxide, acetyl peroxide, dilauryl peroxide, di-tert-butyl peroxide, cumyl hydroperoxide, hydrogen peroxide, potassium persulfate, etc. can be used, and as the azo compound initiator, azo nitrile, azo ester, azo amide, azo imidazoline, azo amidine, macro azo initiator, etc. can be used. In the present invention, 4,4′-azobis(4-cyanovaleric acid) can be used as the initiator.
[0059] In the present invention, after preparing the reverse emulsion, an initiator is added and reacted, thereby obtaining a cross-linked polymer having the desired viscosity of the present invention, i.e., a thickener, and increasing the yield of the thickener. In the present invention, a solution formed by the cross-linked polymer prepared by the above preparation method can be used as a thickener, and further, a thickener in powder form can be finally prepared by precipitating the above solution with a precipitant. In this case, acetone or the like can be used as the precipitant.
[0060] In a specific example, the above steps can be performed at above 65° C. for 2 to 6 hours.
[0061] In addition, the present invention provides a thickener prepared by the above-mentioned thickener preparation method.
[0062] The thickener according to the present invention has a spherical fine particle morphology and swells in water, ethanol or a water-ethanol mixed solution, thereby providing a high-viscosity solution that is visually uniform in appearance.
[0063] The thickener prepared by the present invention may have an average particle size of 10 to 300 μm.
[0064] In addition, the thickener prepared in the present invention may have a viscosity of 500 to 70,000 cPs, or 5,000 to 50,000 cPs in a 1% (w / v) aqueous dispersion at 25°C.
[0065] In addition, the present invention provides a cosmetic composition comprising the thickener.
[0066] The content of the thickener is not particularly limited and can be appropriately determined according to the desired cosmetic material. From the perspective of usability, the content of the above thickener can be 0.01 to 10% by weight, or 0.1 to 5% by weight.
[0067] Cosmetics can be prepared by appropriately mixing oily bases, surfactants, powders, moisturizers, ultraviolet absorbers, alcohols, chelating agents, pH adjusters, preservatives, antioxidants, thickeners, drugs, dyes, pigments, fragrances, water, etc. according to the dosage form within the range that does not impair the effects of the invention.
[0068] The type of the cosmetic of the present invention is not particularly limited. For example, it can be applied to basic cosmetics, color cosmetics, facial mask cosmetics, hair cosmetics, etc.
[0069] In addition, the thickener according to the present invention can be used in pharmaceuticals, food stabilizers or lubricant compositions. In this case, the content of the thickener can be appropriately adjusted according to its intended use, and can contain known additional components.
[0070] Implementation
[0071] Below, the present invention will be described in detail by examples. The following examples are only used to illustrate the present invention, and the scope of the present invention is not limited to the following examples. This embodiment is provided to make the disclosure of the present invention complete and to fully inform the scope of the invention to those of ordinary skill in the art to which the present invention belongs. The present invention is only defined by the scope of the claims.
[0072] Example
[0073] Comparative Example 1.
[0074] 17g of 2-acrylamidopropylmethyl sulfonic acid and 6.5g of ammonium bicarbonate were put into 100g of tert-butanol as a solvent and fully dissolved at 70°C, and then 1.6g of trimethylolpropane triacrylate as a crosslinking agent was dissolved in 6.4g of tert-butanol and added. Finally, 0.2g of dilauryl peroxide was added, reacted for 2 hours, and the thickener was precipitated with acetone to obtain.
[0075] Example 1.
[0076] Aqueous phase: 17 g of 2-acrylamido-2-methylpropanesulfonic acid and 0.5 g of trimethylolpropane ethoxylate triacrylate were dissolved in 63 g of distilled water, and then neutralized to pH 7-9 with ammonia water.
[0077] Oil phase: 10 g of polyoxyethylene (3) oleyl ether and 10 g of polyoxyethylene (6) oleyl ether were added to 80 g of hepane and mixed thoroughly.
[0078] The aqueous phase and the oil phase were placed in a reactor and heated to 70° C., and then 0.1 g of an initiator 4,4′-azobis(4-cyanovaleric acid) was added and reacted for 3 hours. The thickener was precipitated with acetone to obtain the thickener.
[0079] Example 2.
[0080] Aqueous phase: 17 g of 2-acrylamido-2-methylpropanesulfonic acid and 1.0 g of trimethylolpropane ethoxylated triacrylate were dissolved in 63 g of distilled water and then neutralized to pH 7-9 with aqueous ammonia.
[0081] Oil phase: 10 g of polyoxyethylene (3) oleyl ether and 10 g of polyoxyethylene (6) oleyl ether were added to 80 g of heptane and mixed thoroughly.
[0082] The aqueous phase and the oil phase were placed in a reactor and heated to 70° C., and then 0.1 g of an initiator 4,4′-azobis(4-cyanovaleric acid) was added and reacted for 3 hours. The thickener was precipitated with acetone to obtain the thickener.
[0083] Example 3.
[0084] Aqueous phase: 17 g of 2-acrylamido-2-methylpropanesulfonic acid and 1.5 g of trimethylolpropane ethoxylated triacrylate were dissolved in 63 g of distilled water and then neutralized to pH 7-9 with aqueous ammonia.
[0085] Oil phase: 10 g of polyoxyethylene (3) oleyl ether and 10 g of polyoxyethylene (6) oleyl ether were added to 80 g of heptane and mixed thoroughly.
[0086] The aqueous phase and the oil phase were placed in a reactor and heated to 70° C., and then 0.1 g of an initiator 4,4′-azobis(4-cyanovaleric acid) was added and reacted for 3 hours. The thickener was precipitated with acetone to obtain the thickener.
[0087] Comparative Example 2.
[0088] Aqueous phase: 17 g of 2-acrylamido-2-methylpropanesulfonic acid and 1.0 g of trimethylolpropane ethoxylated triacrylate were dissolved in 63 g of distilled water and then neutralized to pH 7-9 with aqueous ammonia.
[0089] Oil phase: 10 g of polyoxyethylene (3) oleyl ether and 5 g of polyoxyethylene (6) oleyl ether were respectively added into 80 g of hexane and mixed thoroughly.
[0090] The aqueous phase and the oil phase were placed in a reactor and heated to 70° C., and then 0.1 g of an initiator 4,4′-azobis(4-cyanovaleric acid) was added and reacted for 3 hours. The thickener was precipitated with acetone to obtain the thickener.
[0091] Experimental Example 1. Transparency Comparison
[0092] The compositions (thickeners) prepared in Comparative Example 1 and Example 2 were compared in terms of transparency.
[0093] The results are shown in Figure 1 .
[0094] exist Figure 1 , the left container shows a container containing a 1% (w / v) aqueous solution of the thickener polymerized in Comparative Example 1, and the right container shows a container containing a 1% aqueous solution of the thickener polymerized in Example 2.
[0095] As mentioned above Figure 1 As shown, it can be confirmed that the thickener prepared in Comparative Example 1 is opaque, while the thickener prepared in the example is transparent in the aqueous solution phase.
[0096] Experimental Example 2. Spherical Particle Morphology Measurement
[0097] The morphologies of the spherical particles prepared in Examples and Comparative Examples were measured.
[0098] Figure 2 is a particle of the thickener prepared in Example 2, specifically, Figure 2 (a) shows the droplet state (70°C) of the oil-in-water emulsion formed during the polymerization reaction in Example 2, (b) shows the hydrodynamic volume size of the polymerized fine particle thickener, and (c) shows an optical image of an aqueous solution containing the thickener.
[0099] As mentioned above Figure 2 As shown, it can be confirmed that the thickener prepared in Example 2 exists in the form of spherical particles.
[0100] Figure 3 The results (optical images) of comparing particles of thickeners prepared in Comparative Example 1(a) and Example 2(b) are shown.
[0101] As mentioned above Figure 3 As shown, fine particles could not be confirmed in the thickener polymerized in Comparative Example 1. When polymerization was performed by the method according to Example 2, the presence of fine particles of the thickener in the aqueous solution was confirmed.
[0102] on the other hand, Figure 4 Comparative results of the hydrodynamic volume sizes of the fine particle thickeners polymerized in Example 2 and Comparative Example 2 are shown.
[0103] As mentioned above Figure 4 As shown, it can be confirmed that the thickener of Example 2 using heptane as the organic solvent has a larger volume size than that using hexane.
[0104] Experimental Example 3. Viscosity Comparison
[0105] The viscosity of the thickeners prepared in Example 2 and Comparative Example 2 was measured using a Brookefield LVT (Brookefield, MA) at 64 spindles and 10 to 30 rpm.
[0106] The above viscosity was measured for a 1% (w / v) aqueous solution containing a thickener.
[0107] As a result, the viscosity of the aqueous solution including the thickener of Comparative Example 2 was measured to be 2,000 cPs, and the viscosity of the aqueous solution including the thickener of Example 2 was measured to be 14,000 cPs.
[0108] From the above measurement results, it can be confirmed that the viscosity of the thickener according to the present invention is improved compared with the comparative example.
[0109] Experimental Example 4. Comparison of Rheological Properties
[0110] The rheological properties of the prepared thickeners were measured. The rheological properties were measured using a Discovery hr-3 hybrid rheometer (TA Instruments).
[0111] The results are shown in Figure 5 .
[0112] Figure 5 (a) and (b) show the rheological property measurement results of the thickeners prepared in Comparative Example 1 and Example 2, respectively.
[0113] In rheology, polymer chains in polymer solutions have entangled structures, so under high shear stress, the entangled structure is untied, and resistance occurs before the structure is completely untied. This is called overshooting, and it can be confirmed that this phenomenon occurs in Comparative Example 1 in an amorphous state.
[0114] In contrast, it can be confirmed that the thickener exists in the form of fine particles in Example 2, so the structure collapses under high shear stress and there is almost no overshoot. Due to this rheological characteristic, it is judged that the thickener according to the present invention improves the feel in use, especially the spreadability, in the cosmetic dosage form.
[0115] Preparation Example 1. Emulsion cream dosage form
[0116] A cream was prepared using the ingredients and contents in Table 1 below.
[0117] [Table 1]
[0118]
[0119] Experimental Example 4: Evaluation of the user experience panelists
[0120] (1) Methods
[0121] 20 trained panelists were selected to conduct the usage evaluation.
[0122] The above-mentioned feeling during use was evaluated with a full score of 5 points for each of softness, thickness, moisture and stickiness.
[0123] (2) Results
[0124] The results are shown in Table 2 below.
[0125] [Table 2]
[0126] soft Thickness Moisture feeling Sticky feeling Frost 1 3.2 3.5 3.7 1.3 Frost 2 3.2 2.8 3.8 1.2 Frost 3 4.1 3.7 3.7 1.0 Frost 4 3.0 3.4 3.6 1.2 Frost 5 3.0 1.5 4.2 1.0
[0127] As shown in Table 2 above, it can be confirmed that Cream 3 received the highest evaluation in the softness and thickness feeling items.
[0128] Specifically, it can be confirmed that the viscosity of the thickener of Comparative Example 1 in a 0.4% (w / v) aqueous solution is 5,500 cPs, but when applied to the <Cream 1> dosage form, it is reduced to 4,000 cPs. In contrast, the viscosity of the thickener of Example 2 in a 0.4% (w / v) aqueous solution is 1,500 cPs, but when applied to the <Cream 3> dosage form, it is increased to 6,500 cPs.
[0129] on the other hand, Figure 6 Optical images of frost 1 (a) and frost 3 (b) are shown.
[0130] like Figure 6 As shown, the results of testing the dosage form using an optical microscope confirmed that the spherical particles of the thickener coexist in the dosage form, affecting the fluidity of the dosage form and forming a more stable dosage form.
[0131] For the thickener of Comparative Example 1, the entangled structure in the dosage form shrinks due to the emulsifier, thereby reducing the viscosity. On the contrary, for the thickener of Example 2, as a particle form, it has a hydrodynamic volume, so it is not greatly affected by the emulsifier while maintaining a certain volume in the dosage form. Moreover, since the emulsified particles and fine particles that hinder fluidity coexist in the dosage form, it is judged that the thickening effect is doubled.
[0132] Industrial Availability
[0133] In the present invention, the polymerization reaction is carried out in a uniform reverse emulsion phase with a small particle size by using the PIT (phase inversion temperature) polymerization method, so that a thickener in the form of homogeneous fine particles can be prepared. The thickener in the form of spherical particles prepared by the present invention has the following advantages: even if it swells in a water phase, the particle shape is not only maintained, but also the particles are uniformly dispersed, transparent in appearance, and highly stable.
Claims
1. A method for preparing a thickener, comprising: The step of preparing an oil-in-water emulsion composition, the oil-in-water emulsion composition comprising an aqueous phase including a compound represented by the following Chemical Formula 1 and a cross-linking monomer, and an oil phase including heptane; The step of heating to above 60° C. to prepare a water-in-oil type reverse emulsion composition; and The step of preparing a cross-linked polymer by adding a reaction initiator to carry out a polymerization reaction, [Chemical formula 1] 2. The method for preparing a thickener according to claim 1, wherein: The compound represented by Chemical Formula 1 may be included in an amount of 95 to 99.5 parts by weight relative to 100 parts by weight of the total weight of the compound represented by Chemical Formula 1 and the cross-linking monomer.
3. The method for preparing a thickener according to claim 1, wherein: The crosslinking monomer is a compound having two or more acrylate groups, two or more acrylamide groups, or two or more vinyl groups.
4. The method for preparing a thickener according to claim 1, wherein: The content of the cross-linking monomer is 0.5 to 5 parts by weight relative to 100 parts by weight of the total weight of the compound represented by Chemical Formula 1 and the cross-linking monomer.
5. The method for preparing a thickener according to claim 1, wherein: The oil phase further comprises one or more surfactants, and the total HLB value of the surfactants is 6 to 14.
6. The method for preparing a thickener according to claim 5, wherein: Two surfactants, a surfactant having an HLB value of 3 to 8 and a surfactant having an HLB value of 8 to 16, are used.
7. The method for preparing a thickener according to claim 1, wherein: The reaction initiator is one or more selected from the group consisting of peroxides and azo compounds.
8. The method for preparing a thickener according to claim 1, wherein: The polymerization reaction is carried out at above 60°C for 2 to 6 hours.
9. A composition comprising a thickener prepared by the preparation method according to claim 1.