Cyclic coating method, film layer and product
By forming a multi-layered, dense film on the substrate surface through a cyclic coating method, the problem of poor scratch resistance and durability of the film in traditional plasma chemical vapor deposition technology is solved, and better adhesion and waterproof performance are achieved. It is suitable for electronic products, glass products, ceramic products, etc.
Patent Information
- Application Number
- CN202011205084.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-02
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-11-02
AI Technical Summary
Traditional plasma chemical vapor deposition technology has unsatisfactory scratch resistance and durability when preparing polymer films, and it is not conducive to the formation of dense structures, which limits its large-scale industrial application.
A cyclic coating method is used to form a multi-layered, dense film on the substrate surface by alternating plasma discharge and off-discharge, combined with specific reactive materials. Intermittent plasma discharge is used to activate active sites, forming an even denser film.
It improves the scratch resistance, durability, and waterproof performance of the membrane, forms a dense structure, enhances the adhesion, acid and alkali resistance, and mechanical properties of the membrane, and solves the problem of membrane unevenness in traditional methods.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The invention relates to a surface modification technology, and in particular to a cyclic coating method, a film layer and a product. Background Art
[0002] The properties of the substrate itself can lead to some deficiencies in the performance of the substrate surface, thereby limiting the application of the substrate. The method of forming a film layer on the surface of the substrate is a common modification technology.
[0003] Plasma chemical vapor deposition (PCVD) technology has been widely used to deposit polymer films on the surface of substrates. It uses plasma to activate reactive gases, promote chemical reactions of reactive gases on the surface of substrates or in the space near the surface, and generate solid films.
[0004] Plasma chemical vapor deposition technology has the following advantages:
[0005] (1) It is a dry process, and the resulting film is uniform and pinhole-free; (2) The chemical and physical properties of the plasma polymerized film, such as solvent resistance, chemical corrosion resistance, and wear resistance, are stable; (3) The plasma polymerized film has good bonding performance with the substrate; (4) A uniform film can also be made on an extremely irregular substrate surface; (5) The film preparation temperature is low and can be carried out at room temperature, effectively avoiding the loss of temperature-sensitive devices; (6) The plasma process can not only prepare films with a thickness of micrometer level but also prepare ultra-thin nanometer-level films.
[0006] The traditional process uses plasma chemical vapor deposition technology to develop a method based on a specific small duty cycle pulse to prepare polymer film layers. The film layers obtained in this way have unsatisfactory scratch resistance and durability. In addition, the coating method based on a specific small duty cycle pulse is not conducive to the formation of dense structures, and may not even form a stable film structure. It is also not conducive to the high-speed growth of the film layer, which prolongs the preparation time and limits its large-scale application in industry. Summary of the invention
[0007] One advantage of the present invention is to provide a cyclic coating method, a film layer and a product, wherein the film layer obtained by the cyclic coating method can have better performance, such as scratch resistance and durability.
[0008] Another advantage of the present invention is to provide a cyclic coating method, a film layer and a product, wherein the film layer obtained by the cyclic coating method can have better waterproof performance.
[0009] Another advantage of the present invention is to provide a cyclic coating method, a film layer and a product, wherein the film layer obtained by the cyclic coating method can form a multi-layer dense structure.
[0010] Another advantage of the present invention is that it provides a cyclic coating method, film layer and product, wherein during the preparation process of the film layer, plasma discharge is intermittently turned on during the coating stage, and the above process is repeated to effectively activate active sites on the surface of the substrate, thereby forming a dense film layer.
[0011] According to one aspect of the present invention, the present invention provides a cyclic coating method, which comprises the following steps:
[0012] introducing reaction materials into a reaction chamber; and
[0013] Plasma enhanced chemical vapor deposition is performed on a substrate surface in the reaction chamber under cyclic coating conditions to form a film layer, wherein the plasma discharge is turned on for a preset time, and then the discharge is turned off for a preset time, which is one coating. The above process is cycled for cyclic coating, and the supply of reaction raw materials is maintained throughout the process.
[0014] According to one embodiment of the present invention, the duration of the plasma discharge during each cycle is t1, and t1 in the previous cycle and the next cycle is the same.
[0015] According to one embodiment of the present invention, the duration of the plasma discharge being turned off in each cycle is t2, and t2 in the previous cycle and the next cycle is the same.
[0016] According to one embodiment of the present invention, the reaction raw material is fluoride.
[0017] According to one embodiment of the present invention, the fluoride is a fluorinated alcohol and has the structural formula: n F 2n+1 -C m H 2m -OH, wherein n is an integer of 1-12, and m is an integer of 0-4.
[0018] According to one embodiment of the present invention, the reaction raw material has the general formula R 1 R 2 C=CR 3 R 4 , where R 1 , R 2 and R 3 are independently selected from hydrogen, alkyl, halogen, haloalkyl or aryl, wherein R 1 , R 2 and R 3At least one of them is a halogen, wherein R 4 It is a group XR 5 , R 5 is an alkyl or haloalkyl group and X is a bond; or X is a group -C(O)O(CH 2 ) n Y-, wherein n is an integer from 0 to 10, and Y is a bond or a sulfonamide group; or X is a group -OC(O)-(CH 2 ) i Z-, wherein i is an integer from 0 to 10, and Z is a bond or a sulfonamide group; or X is a group -(CH 2 ) x U-, wherein x is an integer from 0 to 10, and U is a bond or a sulfonamide group; or X is a group -(O) p R 6 (O) q (CH 2 ) t -, where R 6 is an aryl group optionally substituted with halogen, p is 0 or 1, q is 0 or 1, and t is 0 or an integer from 1 to 10, provided that when q is 1, t is non-0.
[0019] According to one embodiment of the present invention, the reaction raw material is an organosilicon compound and has the structural formula:
[0020]
[0021] Where R 8 , R 9 , R 10 , R 11 , R 12 , R 13 It is a group connected to an unsaturated carbon-carbon double bond and a Si atom, and can be independently selected from an alkyl group, an aryl group, a halogen group, a halogenated alkyl group, a halogenated aryl group, an alkoxy group or a vinyl group. K is an integer of 0-8.
[0022] According to one embodiment of the present invention, the reaction raw material is an epoxy compound and has the following structural formula:
[0023]
[0024] Among them, R 1 , R 2 , R 3 is independently selected from hydrogen, alkyl, aryl, halogen, haloalkyl or hydroxy; X is hydrogen or halogen, m is an integer of 0-8, and n is an integer of 1-15.
[0025] According to one embodiment of the present invention, the reaction raw material is an acrylamide compound, and has the following structural formula: Compound monomer 1, or monomer 2, or a mixture of monomer 1 and monomer 2:
[0026]
[0027] Among them, R 1 , R 2 , R 3 , R 6 , R 7 , R 8 are independently selected from hydrogen, alkyl, aryl, halogen, haloalkyl, alkenyl or haloalkenyl, X and Y are hydrogen or halogen; R 4 , R 5 Independently selected from hydrogen, alkyl, aryl, halogen, haloalkyl or having the following structure:
[0028]
[0029] Among them, R 11 is a straight chain or branched alkane subunit having 1 to 15 carbon atoms, R 12 , R 13 , R 14 , R 15 R is independently selected from hydrogen, alkyl, aryl, halogen or haloalkyl; 9 , R 10 is independently selected from a linear, branched alkyl subunit or an aryl subunit having 1 to 15 carbon atoms; or R 9 , R 10 is the connecting key; m, n, p, q are integers of 0-20, but m and n are not 0 at the same time, and p and q are not 0 at the same time.
[0030] According to one embodiment of the present invention, the plasma discharge mode is radio frequency discharge, microwave discharge, medium frequency discharge or spark discharge.
[0031] According to another aspect of the present invention, a film layer is formed on a substrate surface by a plasma chemical vapor deposition method using reaction raw materials in a cyclic coating manner, wherein the plasma discharge is turned on for a preset time, and then the discharge is turned off for a preset time, which is a single coating. The above process is cycled for cyclic coating, and the supply of reaction raw materials is maintained throughout the process.
[0032] According to another aspect of the present invention, a product is provided, wherein the product is provided with a film layer, wherein the film layer is formed on a surface of a substrate by a plasma chemical vapor deposition method using reaction raw materials in a cyclic coating manner, wherein the plasma discharge is turned on for a preset time, and then the discharge is turned off for a preset time, which is one coating, and the above process is cycled to form a cyclic coating, and the supply of reaction raw materials is maintained throughout the process. DETAILED DESCRIPTION
[0033] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be applied to other embodiments, variations, improvements, equivalents, and other technical solutions that do not deviate from the spirit and scope of the present invention.
[0034] It will be understood by those skilled in the art that, in the disclosure of the present invention, the term "halogen" or "halogen" refers to fluorine, chlorine, bromine and iodine. The term "hydrocarbon" includes alkyl, alkenyl or aryl. The term "aryl" refers to an aromatic cyclic group, such as phenyl or naphthyl, especially phenyl. The term "alkyl" refers to a straight or branched chain of carbon atoms, which is suitably up to 20 carbon atoms in length. The term "alkenyl" refers to a straight or branched unsaturated chain, suitably having 2 to 20 carbon atoms.
[0035] It is to be understood that the term "one" should be understood as "at least one" or "one or more", that is, in one embodiment, the number of an element may be one, while in another embodiment, the number of the element may be multiple, and the term "one" should not be understood as a limitation on the quantity.
[0036] The present invention provides a cyclic coating method, a film layer and a product. In some examples of the present invention, the product can be, but is not limited to, an electronic product, a silk product, a woven bag, a metal surface, a glass product or a ceramic product.
[0037] It is worth mentioning that the film layer has a good waterproof effect. When the product is an electronic product, the product can be, but is not limited to, a portable device, such as a keyboard. By coating the waterproof film layer, the keyboard can become a waterproof keyboard. The product can be, but is not limited to, LED display screens, smart fingerprint locks, hearing aids, Bluetooth headsets, sensors suitable for working in liquid environments or frequently exposed to water, mobile phones, notebooks, PSPs and other electronic devices that may be exposed to water in the working environment.
[0038] Further, according to at least one embodiment of the present invention, when water adheres to the film layer, the static contact angle of water is greater than 110°. The static contact angle may be greater than 120°, or 110° to 115°, or 115° to 120°.
[0039] The film layer is a nano film layer, and its thickness can be made thinner to be suitable for precision electronic equipment. For example, the thickness of the film layer can range from 10nm to 20nm, such as 15nm. The waterproof film layer can also be made thicker according to user needs. Optionally, the thickness of the film layer can range from 10nm to 2000nm, but is not limited to it.
[0040] The film layer is formed on the surface of the substrate by a plasma enhanced chemical vapor deposition (PECVD) process. That is, during the preparation process, the surface of the substrate is exposed to a chamber of a plasma enhanced chemical vapor deposition reaction device, plasma can be formed in the chamber, and the reaction raw material gas forms the film layer on the surface of the substrate through a chemical deposition reaction.
[0041] The plasma used in the preparation method provided by the present invention includes non-equilibrium plasma, such as those plasmas produced by radio frequency (Rf), microwave or direct current (DC). They can be operated at atmospheric pressure, or at a pressure lower than atmospheric pressure. It is worth noting that the plasma source can come from a monomer compound, i.e., there is no other gas, or other gases, such as inert gases, or mixed with other gases. The unit for providing plasma is called a plasma source, wherein the description of the plasma source can be seen in the corresponding part below. The plasma composed only of the monomer compound can be obtained in the following manner, first, the reaction device is evacuated as much as possible, and then, the reaction device is purged with the monomer compound for a sufficiently long time to discharge other gases in the reaction device.
[0042] In the plasma enhanced chemical vapor deposition (PECVD) process adopted in the present invention, plasma is generated by glow discharge, and the discharge method may be, but is not limited to, microwave discharge, radio frequency discharge, ultraviolet, spark discharge, and the like.
[0043] In the present invention, since cyclic coating is introduced in the coating process, it is beneficial to form the film layer of the multi-layer composite structure, providing multi-layer protection for the product itself. In addition, at the microscopic level, the film layer can be expressed as a denser film layer structure, and at the macroscopic level, it exhibits excellent hydrophobicity, adhesion, acid and alkali resistance, mechanical properties, and moisture and heat resistance.
[0044] It is worth mentioning that due to the introduction of intermittent coating in the coating process, sufficient energy plasma can be generated within a certain period of time to interrupt the introduced reaction monomer segments to form more excited state segments. The excited state segments are combined in the form of chemical bonds through the active sites with certain energy and activity in the monomer material and the active sites with corresponding energy on the substrate surface to produce more and more complex elementary reactions to form a denser network cross-linked structure.
[0045] In addition, during the intermittent coating process, the cessation of plasma discharge may be beneficial to the uniformity of the mutual reaction between the excited segments. For example, in at least one embodiment of the present invention, the substrate moves in the reaction chamber so that the coating thickness of the substrate at different positions tends to be consistent, so as to reduce the problem of uneven thickness of the film layer on the surface of the substrate due to different monomer densities in different regions in the reaction chamber. The reasons for the uneven monomer density may be various, for example, it may be caused by the arrangement position of a discharge device used for plasma discharge. If the plasma discharge is stopped for a period of time during the coating process, the problem of uneven monomer density caused by the discharge device may be weakened. At the same time, the movement of the substrate in the reaction chamber is beneficial to the uniformity of the film layer on the surface of the substrate.
[0046] According to some embodiments of the present invention, the movement of the substrate in the reaction chamber may be linear reciprocating motion or curved reciprocating motion, and the curved motion may include circular motion, elliptical motion, planetary motion, spherical motion or other irregular curved motion.
[0047] According to an embodiment of the present invention, the cyclic coating method may include the following steps:
[0048] (1) Substrate preparation
[0049] Before chemical vapor deposition is performed on the substrate, the substrate is cleaned to remove dust, moisture or grease on the surface of the substrate. The substrate can be cleaned with an organic solvent such as acetone or isopropanol, and then the substrate is placed in the reaction chamber of the reaction device.
[0050] (2) Preparing the waterproof film layer on the substrate surface using PECVD technology
[0051] The reaction chamber of the reaction device is continuously evacuated, and then the vacuum degree in the reaction chamber is reduced to 10-200 mTorr, and a plasma source gas is introduced;
[0052] The reaction raw materials are introduced until the vacuum degree is 30-300 mTorr, plasma discharge is started, chemical vapor deposition is performed, and the waterproof film layer is prepared on the surface of the substrate.
[0053] Then, the plasma discharge can be stopped, the introduction of the reaction raw materials can be stopped, and the vacuum can be continuously drawn to maintain the vacuum degree of the reaction chamber at 10 to 200 mTorr. After 1 to 5 minutes, the atmosphere can be introduced to normal pressure, and then the substrate can be taken out.
[0054] In the step (2), the reaction raw material can be a monomer compound or a mixture of a monomer compound and a cross-linking agent. Alternatively, the monomer compound can be a fluoride, and the low polarizability and strong electronegativity of the fluorine atoms in the fluorocarbon material give fluorocarbon polymers many unique properties, such as high hydrophobicity and oleophobicity, resistance to chemical reagent corrosion, so fluorocarbon materials are widely used in surface modification of architectural coatings, textile industry, and military fields. Alternatively, the monomer compound can be a silicide, and the bond energy of Si-O is higher than that of CC bond, and has good low temperature resistance. It will be appreciated by those skilled in the art that the reaction raw materials at this time are only for illustration, and the raw materials that can be subjected to plasma reaction under the cyclic coating conditions provided in the present embodiment can be selected according to demand.
[0055] In step (2), the plasma discharge mode is implemented as cyclic coating, wherein cyclic coating means turning on the plasma discharge for t1 (for example, 30 seconds), then turning off the discharge for t2 (for example, 60 seconds), taking this as a cycle T, and then repeating the above process n times, and in the whole process, the reaction raw materials are continuously supplied. t1, t2 and n can be adjusted according to actual production needs. n can be 2 or more.
[0056] It is understandable that the time t1 may be longer than the time t2, or shorter than the time t2, or equal to the time t2, and the user may adjust it according to needs.
[0057] It is understood that in two adjacent cycles, t1 of the previous cycle and t1 of the next cycle can be the same or different. t2 of the previous cycle and t2 of the next cycle can be the same or different. It is understood by those skilled in the art that "cyclic coating" does not require all conditions of the previous coating process to be completely repeated.
[0058] According to an embodiment of the present invention, the substrate may be subjected to bombardment pretreatment before the reaction raw materials are introduced.
[0059] It is worth mentioning that when the plasma source gas is an inert gas or a gas that is not easy to react, the plasma source gas will not be deposited to form the hydrophobic surface film layer, that is, the plasma source gas will not become a component of the hydrophobic surface film layer, but through the interaction of the plasma source on the surface, tiny etching phenomena will occur, thereby being able to clean the surface of the substrate well, and provide good deposition conditions for the deposition of the reaction gas raw materials, so that the deposited hydrophobic surface film layer is more firmly bonded to the surface of the substrate.
[0060] The cyclic coating periodically introduces a high-power pretreatment activation stage during the process. The cyclic introduction of this stage is beneficial to introduce more active sites on the surface of the substrate at this stage, increase the effective coating, make the film structure denser, and provide better protection against corrosive environments.
[0061] The reaction gas raw material can be introduced simultaneously with the plasma source, or the substrate can be pretreated for 1 to 1200 seconds after the plasma source is introduced, and then the reaction gas raw material and the cross-linking agent are introduced according to the process parameter requirements.
[0062] Optionally, the plasma source gas is an inert gas or nitrogen, such as helium.
[0063] Further, optionally, the operating power range of the reaction chamber may be 1-500W, the pressure range may be 10 mTorr-500 mTorr, and the temperature range may be 30°C-60°C.
[0064] According to an embodiment of the present invention, the substrate in the preparation method is a solid material, such as an electronic component or an electrical component, and the waterproof film layer prepared on the surface of the substrate can be exposed to the environment described in the international industrial waterproof grade standard IPX1-IPX8.
[0065] According to an embodiment of the present invention, the volume of the reaction chamber in the preparation method is 50-1000L, and the temperature of the reaction chamber is controlled at 30-60°C; the flow rate of the inert gas or nitrogen is 5-300sccm, and the inert gas is one of argon or helium, or a mixture of argon and helium.
[0066] According to an embodiment of the present invention, the reaction raw materials in the preparation method are introduced into the reaction chamber by atomization and volatilization through a feeding pump at a low pressure of 10-200 mTorr, and the flow rate of the reaction raw materials is 10-1000 μL / min.
[0067] According to an embodiment of the present invention, the substrate is subjected to bombardment pretreatment before the reaction raw materials are introduced.
[0068] According to an embodiment of the present invention, in the preparation method, the power of starting plasma discharge is 2-500W, and the discharge is cyclic. The plasma discharge mode can be radio frequency discharge, microwave discharge, medium frequency discharge or spark discharge.
[0069] According to an embodiment of the present invention, in the preparation method, the energy output mode of the plasma RF is controlled to be pulsed or continuous output during the plasma RF discharge process. When the energy output mode of the plasma RF is pulsed output, the pulse width is 2μs-1ms and the repetition frequency is 20Hz-10kHz.
[0070] The reaction raw material may be a fluoride, or a fluoride and a cross-linking agent, and the cross-linking agent may be a multifunctional compound containing an ester group, an ether group, an epoxy group, or a cyano group.
[0071] The reaction raw material may be a general structure C n F 2n+1 -C m H 2m A fluorinated alcohol compound containing -OH, wherein n is an integer of 1 to 12, and m is an integer of 0 to 4. Furthermore, n is an integer of 1 to 8, and m is an integer of 2 to 3.
[0072] For example, the fluorinated alcohol compound reaction raw material is selected from: one or more of perfluorohexylethanol, perfluorobutylethanol, and perfluorohexylethanol.
[0073] According to one embodiment of the present invention, there are methylene weak sites in the fluorinated alcohol compound reaction raw material.
[0074] According to one embodiment of the present invention, the fluorinated alcohol compound reaction raw material is a primary alcohol.
[0075] The crosslinker compound may be a compound having the following structure:
[0076]
[0077] Among them, R 1 , R 2 , R 3 , R 5 , R 6 , R 7 R is independently selected from hydrogen, alkyl, aryl, halogen, alkyl halide, aryl halide. j and k are integers of 0-10 and cannot be 0 at the same time. 4 It can be a bond, -CO-, -COO-, an aromatic subunit, an alicyclic subunit, or an aliphatic alkyl subunit substituted with a hydroxyl group. The crosslinking agent can also be a multifunctional compound containing an ester group, an ether group, an epoxy group, or a cyano group.
[0078] According to one embodiment of the present invention, the crosslinking agent is selected from the group consisting of glycidyl methacrylate, allyl glycidyl ether, 1,2-epoxy-4-vinylcyclohexane, 3-(2,3-epoxypropoxy)propyl vinyldimethoxysilane, and enbutoxide.
[0079] The reaction raw material may be a saturated fluoride or an unsaturated fluoride. 1 R 2 C=CR 3 R 4 A compound wherein R 1 , R 2 and R 3 are independently selected from hydrogen, alkyl, halogen, haloalkyl or aryl, wherein R 1 , R 2 and R 3 At least one of them is a halogen, wherein R 4 It is a group XR 5 , R 5 is an alkyl or haloalkyl group and X is a bond; or X is a group -C(O)O(CH 2 ) n Y-, wherein n is an integer from 0 to 10, and Y is a bond or a sulfonamide group; or X is a group -OC(O)-(CH 2 ) i Z-, wherein i is an integer from 0 to 10, and Z is a bond or a sulfonamide group; or X is a group -(CH 2 ) x U-, wherein x is an integer from 0 to 10, and U is a bond or a sulfonamide group; or X is a group -(O) p R 6 (O) q (CH 2 ) t -, where R 6 is an aryl group optionally substituted with halogen, p is 0 or 1, q is 0 or 1, and t is 0 or an integer from 1 to 10, provided that when q is 1, t is non-0.
[0080] The reaction raw material may be a general formula R 1 CH=CHR 4 A compound wherein R 1 is a halogen, where R 4 The group -C(O)O(CH 2 ) n C m F 2m+1 ; or R 4 The group -OC(O)-(CH2 ) i C m F 2m+1 ; or R 4 The group -(CH 2 ) x C m F 2m+1 , wherein n, i or x is an integer from 1 to 8, and m is an integer from 1 to 12. Optionally, C m F 2m+1 It can be a linear fluoroalkyl group, a branched fluoroalkyl group, or a cyclic structure. Optionally, m is less than 8, for example, not more than 6.
[0081] The reaction raw material may be a general formula CH 2 =CHR 4 A compound wherein R 4 The group -C(O)O(CH 2 ) n C m F 2m+1 ; or R 4 The group -OC(O)-(CH 2 ) i C m F 2m+1 ; or R 4 The group -(CH 2 ) x C m F 2m+1 , wherein n, i or x is an integer from 1 to 8, and m is an integer from 1 to 12. Optionally, C m F 2m+1 It can be a linear fluoroalkyl group, a branched fluoroalkyl group, or a cyclic structure. Optionally, m is less than 8, for example, not more than 6.
[0082] The reaction raw material may be a general formula CH 2 =CR 3 R 4 of fluoride, where R 3 is a halogen, where R 4 The group -C(O)O(CH 2 ) n C m F 2m+1 ; or R 4 The group -OC(O)-(CH 2 ) i C m F 2m+1 ; or R 4 The group -(CH 2 )x C m F 2m+1 , wherein n, i or x is an integer from 1 to 8, and m is an integer from 1 to 12. Optionally, C m F 2m+1 It can be a linear fluoroalkyl group, a branched fluoroalkyl group, or a cyclic structure. Optionally, m is less than 8, for example, not more than 6.
[0083] The reaction raw material may be a general formula R 1 R 2 C=CHR 4 , where R 1 and R 2 , independently selected from hydrogen, alkyl, halogen, haloalkyl or aryl, wherein R 1 and R 2 At least one of them is a halogen, wherein R 4 The group -C(O)O(CH 2 ) n C m F 2m+1 ; or R 4 The group -OC(O)-(CH 2 ) i C m F 2m+1 ; or R 4 The group -(CH 2 ) x C m F 2m+1 , wherein n, i or x is an integer from 1 to 8, and m is an integer from 1 to 12. Optionally, C m F 2m+1 It can be a linear fluoroalkyl group, a branched fluoroalkyl group, or a cyclic structure. Optionally, m is less than 8, for example, not more than 6.
[0084] The reaction raw material may be a general formula R 2 CH=CR 3 R 4 , where R 2 and R 3 are independently selected from hydrogen, alkyl, halogen, haloalkyl or aryl, wherein R 2 and R 3 At least one of them is a halogen, wherein R 4 The group -C(O)O(CH 2 ) n C m F 2m+1 ; or R 4 The group -OC(O)-(CH 2 )i C m F 2m+1 ; or R 4 The group -(CH 2 ) x C m F 2m+1 , wherein n, i or x is an integer from 1 to 8, and m is an integer from 1 to 12. Optionally, C m F 2m+1 It can be a linear fluoroalkyl group, a branched fluoroalkyl group, or a cyclic structure. Optionally, m is less than 8, for example, not more than 6.
[0085] The crosslinking agent is a compound with a multi-functional crosslinking structure. During plasma glow discharge, low-temperature plasma breaks the active groups with higher energy in the crosslinking agent to form active points, and the introduced additional active points crosslink and polymerize with each other in the plasma environment to form a dense network structure.
[0086] According to an embodiment of the present invention, the crosslinking agent may be a multifunctional unsaturated hydrocarbon derivative, which may be selected from one or more of a combination of ethoxylated trimethylolpropane triacrylate, tripropylene glycol diacrylate, divinylbenzene, polyethylene glycol diacrylate, 1,6-hexanediol diacrylate, ethylene glycol diacrylate, diethylene glycol divinyl ether, and neopentyl glycol diacrylate. The crosslinking agent accounts for 30 to 50% of the reaction raw materials.
[0087] The reaction raw material may be an organosilicon compound, such as epoxysilane or an organosilicon compound having the following structural formula:
[0088]
[0089] Where R 8 , R 9 , R 10 , R 11 , R 12 , R 13 It is a group connected to an unsaturated carbon-carbon double bond and a Si atom, and can be independently selected from an alkyl group, an aryl group, a halogen group, a halogenated alkyl group, a halogenated aryl group, an alkoxy group or a vinyl group. K is an integer of 0-8.
[0090] The organosilicon compound may be hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane and / or decamethylcyclopentasiloxane.
[0091] The reaction raw material can be a mixture of the above-mentioned organosilicon compound and unsaturated hydrocarbons, and the unsaturated hydrocarbons can be selected from one or more of ethoxylated trimethylolpropane triacrylate, tripropylene glycol diacrylate, divinylbenzene, polyethylene glycol diacrylate, 1,6-hexanediol diacrylate, ethylene glycol diacrylate, diethylene glycol divinyl ether, and neopentyl glycol diacrylate. Si-O in the organosilicon compound can be opened in a plasma environment to react with the unsaturated bond to form a C-Si bond or a CO bond.
[0092] The reaction raw material may be an epoxy compound, for example, an epoxy compound having the following structural formula:
[0093]
[0094] Wherein, R1, R2, and R3 are independently selected from hydrogen, alkyl, aryl, halogen, halogenated alkyl or hydroxyl; X is hydrogen or halogen, m is an integer of 0-8, and n is an integer of 1-15.
[0095] The reaction raw material may be an acrylamide compound, for example, an acrylamide compound monomer 1, or a monomer 2, or a mixture of monomer 1 and monomer 2 having the following structural formula:
[0096]
[0097] Among them, R 1 , R 2 , R 3 , R 6 , R 7 , R 8 are independently selected from hydrogen, alkyl, aryl, halogen, haloalkyl, alkenyl or haloalkenyl, X and Y are hydrogen or halogen; R 4 , R 5 Independently selected from hydrogen, alkyl, aryl, halogen, haloalkyl or having the following structure:
[0098]
[0099] Among them, R 11 is a straight chain or branched alkane subunit having 1 to 15 carbon atoms, R 12 , R 13 , R 14 , R 15 R is independently selected from hydrogen, alkyl, aryl, halogen or haloalkyl; 9 , R 10 is independently selected from a linear, branched alkyl subunit or an aryl subunit having 1 to 15 carbon atoms; or R 9 , R 10is the connecting key; m, n, p, q are integers of 0-20, but m and n are not 0 at the same time, and p and q are not 0 at the same time.
[0100] Example 1
[0101] Step (1) placing the substrate in the reaction chamber of the reaction device, continuously evacuating the reaction chamber to a vacuum degree of 150 mTorr, and introducing nitrogen;
[0102] The substrate is a solid material, the solid material is an electrical component, and after the waterproof film layer is prepared on the surface of the substrate, any interface thereof can be exposed to the environment described in the international industrial waterproof grade standard IPX6 for use.
[0103] The volume of the reaction chamber is 560 L, the temperature of the reaction chamber is controlled at 50° C., and the flow rate of nitrogen gas introduced as a plasma source is 220 sccm.
[0104] Step (2) introducing the reaction raw materials until the vacuum degree is 220 mTorr and starting the plasma discharge;
[0105] The process of introducing the reaction raw materials is to atomize and volatilize the reaction raw materials through a feed pump, and introduce them into the reaction chamber at a low pressure of 150 mTorr, and the flow rate of the reaction raw materials is 320 μL / min;
[0106] The composition of the reaction raw materials is as follows:
[0107] The reaction raw material is a saturated fluorocarbon compound: perfluorohexylethanol.
[0108] The power of starting the plasma discharge in step (2) is 240 W, and the plasma discharge mode is microwave discharge. During the plasma discharge process, the discharge can be started for 10 seconds, and then the discharge is continuously turned off for 20 seconds, and the above process is repeated. The total time of the plasma discharge process is 3000 seconds.
[0109] Step (3) The vacuum degree of the reaction chamber is maintained at 160 mTorr, and after 4 minutes, the vacuum is introduced into the reaction chamber to an atmospheric pressure.
[0110] Example 2
[0111] Step (1) placing the substrate in the reaction chamber of the reaction device, continuously evacuating the reaction chamber to a vacuum degree of 160 mTorr, and introducing argon gas;
[0112] The substrate is a solid material, the solid material is an electrical component, and after the waterproof film layer is prepared on the surface of the substrate, any interface thereof can be exposed to the environment described in the international industrial waterproof grade standard IPX5 for use.
[0113] The volume of the reaction chamber is 550 L, the temperature of the reaction chamber is controlled at 45° C., and the flow rate of argon gas introduced as a plasma source is 200 sccm.
[0114] Step (2) introducing the reaction raw materials until the vacuum degree is 200 mTorr and starting the plasma discharge;
[0115] The process of introducing the reaction raw materials is to atomize and volatilize the reaction raw materials through a feed pump, and introduce them into the reaction chamber at a low pressure of 150 mTorr;
[0116] The composition of the reaction raw materials is as follows:
[0117] The fluoride in the reaction raw material is saturated fluoride-perfluorohexylethanol, and the cross-linking agent is 1,2-epoxy-4-vinylcyclohexane.
[0118] In the step (2), 1,2-epoxy-4-vinylcyclohexane (cross-linking agent) can be introduced first, with a flow rate of 320 μL / min and an introduction time of 2000 s; after completion, the reaction gas raw material perfluorohexylethanol is vaporized and introduced into the reaction chamber, with a flow rate of 150 μL / min and an introduction time of 3000 s, and chemical vapor deposition is performed on the surface of the substrate to prepare a nanofilm layer.
[0119] It is understood that the crosslinking agent and the fluoride can be introduced simultaneously or separately, or the order of introduction can be reversed.
[0120] The power of starting the plasma discharge in step (2) is 200 W, and the plasma discharge mode is microwave discharge. The plasma discharge mode is implemented as cyclic coating. During the plasma discharge process, the discharge can be turned on for 20 seconds, and then the discharge is turned off for 20 seconds. The above process is repeated, and the total cyclic coating time is 5000 seconds.
[0121] Step (3) The vacuum degree of the reaction chamber is maintained at 160 mTorr, and after 4 minutes, the vacuum is introduced into the reaction chamber to an atmospheric pressure.
[0122] Example 3
[0123] Step (1) placing the substrate in the reaction chamber of the reaction device, continuously evacuating the reaction chamber to a vacuum degree of 150 mTorr, and introducing helium;
[0124] The substrate is a solid material, the solid material is an electrical component, and after the waterproof film layer is prepared on the surface of the substrate, any interface thereof can be exposed to the environment described in the international industrial waterproof grade standard IPX4 for use.
[0125] The volume of the reaction chamber is 550 L, the temperature of the reaction chamber is controlled at 40° C., and the flow rate of helium gas introduced as a plasma source is 200 sccm.
[0126] Step (2) introducing the reaction raw materials until the vacuum degree is 200 mTorr and starting the plasma discharge;
[0127] The process of introducing the reaction raw materials is to atomize and volatilize the reaction raw materials through a feeding pump, and introduce them into the reaction chamber at a low pressure of 120 mTorr;
[0128] The composition of the reaction raw materials is as follows:
[0129] The fluoride in the reaction raw material is saturated fluoride-perfluorohexyl butanol, and the cross-linking agent is allyl glycidyl ether.
[0130] In the step (2), allyl glycidyl ether (cross-linking agent) can be introduced first at a flow rate of 300 μL / min for a time of 2000 s; after completion, the reaction gas raw material perfluorohexyl butanol is vaporized and introduced into the reaction chamber at a flow rate of 200 μL / min for a time of 3000 s, and chemical vapor deposition is performed on the surface of the substrate to prepare a hydrophobic surface film layer.
[0131] The power of starting the plasma discharge in step (2) is 250 W, and the plasma discharge mode is microwave discharge. In the cyclic coating process, the plasma discharge process can be first discharged for 30 seconds, and then continuously turned off for 20 seconds, and the above process is repeated, and the total time is 5000 seconds.
[0132] Step (3) The vacuum degree of the reaction chamber is maintained at 150 mTorr, and after 4 minutes, the vacuum is introduced into the chamber to an atmospheric pressure.
[0133] Example 4
[0134] In the step (1), the fabric substrate is first cleaned with acetone or isopropanol, wiped dry with a dust-free cloth, and then placed in a drying oven for 24 hours.
[0135] In the step (2), the dried fabric is placed in a 1000L plasma vacuum reaction chamber, and the reaction chamber is continuously evacuated to a vacuum degree of 80 mTorr.
[0136] Helium plasma source gas was introduced at a flow rate of 40 sccm, and radio frequency discharge was turned on to pre-treat the fabric. The discharge power in the pre-treatment stage was 50 W, and the discharge time was 300 s.
[0137] First, 1,2-epoxy-4-vinylcyclohexane (cross-linking agent) was introduced at a flow rate of 320μL / min for 2000s; after that, the reaction gas raw material perfluorohexylethanol was vaporized and introduced into the reaction chamber at a flow rate of 150μL / min for 3000s, and a nano-film layer was prepared by chemical vapor deposition on the surface of the substrate. During the film preparation process, the plasma discharge mode was plasma pulse discharge, and the pulse width was 200μs. A cyclic coating process was adopted. During the plasma discharge process, the discharge could be turned on for 30 seconds, and then the discharge could be turned off for 20 seconds. The above process was repeated, and the total cyclic coating time was 5000s.
[0138] After the film layer is prepared, compressed air is introduced to restore the reaction chamber to normal pressure, the chamber is opened, and the fabric is taken out. That is, a hydrophobic surface film layer is plated on the fabric.
[0139] Example 5
[0140] Step (1) placing the substrate in the reaction chamber of the reaction device, continuously evacuating the reaction chamber to a vacuum degree of 150 mTorr, and introducing nitrogen;
[0141] The substrate is a solid material, the solid material is an electrical component, and after the waterproof film layer is prepared on the surface of the substrate, any interface thereof can be exposed to the environment described in the international industrial waterproof grade standard IPX6 for use.
[0142] The volume of the reaction chamber is 560 L, the temperature of the reaction chamber is controlled at 50° C., and the flow rate of nitrogen gas introduced as a plasma source is 220 sccm.
[0143] Step (2) introducing the reaction raw materials until the vacuum degree is 220 mTorr and starting the plasma discharge;
[0144] The reaction raw materials are introduced by atomizing and volatilizing the reaction raw materials through a feed pump, and then introduced into the reaction chamber at a low pressure of 150 mTorr, and the flow rate of the reaction raw materials is 320 μL / min;
[0145] The composition of the reaction raw materials is as follows:
[0146] The unsaturated fluorocarbon compound in the reaction raw material is: CH 2 =CR 3 R 4 , where R 3 Cl, R 4 -OCO-(CH 2 ) 2 C 6 F 13 .
[0147] The power of starting plasma discharge in step (2) is 240 W, and the plasma discharge mode is microwave discharge. Cyclic coating is adopted, and during the plasma discharge process, the discharge can be turned on for 60 seconds, and then the discharge is turned off for 20 seconds, and the above process is repeated, and the total time is 3200 seconds.
[0148] Step (3) The vacuum degree of the reaction chamber is maintained at 160 mTorr, and after 4 minutes, the vacuum is introduced into the reaction chamber to an atmospheric pressure.
[0149] Example 6
[0150] Step (1) placing the substrate in the reaction chamber of the reaction device, continuously evacuating the reaction chamber to a vacuum degree of 160 mTorr, and introducing argon gas;
[0151] The substrate is a solid material, the solid material is an electrical component, and after the waterproof film layer is prepared on the surface of the substrate, any interface thereof can be exposed to the environment described in the international industrial waterproof grade standard IPX5 for use.
[0152] The volume of the reaction chamber is 550 L, the temperature of the reaction chamber is controlled at 45° C., and the flow rate of argon gas introduced as a plasma source is 200 sccm.
[0153] Step (2) introducing the reaction raw materials until the vacuum degree is 200 mTorr and starting the plasma discharge;
[0154] The reaction raw material steam is introduced by atomizing and volatilizing the reaction raw material through a feed pump, and introducing the reaction raw material into the reaction chamber at a low pressure of 150 mTorr. The reaction raw material is a mixture of an unsaturated fluorocarbon compound and a cross-linking agent, and the flow rate of the reaction raw material is 300 μL / min;
[0155] The composition of the reaction raw materials is as follows:
[0156] The unsaturated fluorocarbon compound in the reaction raw material is R 2 CH=CHR 4 , where R 2 Cl, R 4 For-OCOCH 2 C 6 F 13 .
[0157] The crosslinking agent in the reaction raw material can be tripropylene glycol diacrylate, wherein the mass fraction ratio of the unsaturated fluorocarbon compound to the crosslinking agent is 55%:45%.
[0158] In step (2), the power of starting plasma discharge is 200 W, the plasma discharge mode is radio frequency discharge, the output mode is pulse, the pulse width is 2 μs, and the repetition frequency is 500 Hz. In the cyclic coating process, the plasma discharge process can be discharged for 60 seconds, and then the discharge is continuously turned off for 20 seconds, and the above process is repeated 13 times.
[0159] Step (3) The vacuum degree of the reaction chamber is maintained at 160 mTorr, and after 4 minutes, the vacuum is introduced into the reaction chamber to an atmospheric pressure.
[0160] Example 7
[0161] Step (1) placing the substrate in the reaction chamber of the reaction device, continuously evacuating the reaction chamber to a vacuum degree of 150 mTorr, and introducing helium;
[0162] The substrate is a solid material, the solid material is an electrical component, and after the waterproof film layer is prepared on the surface of the substrate, any interface thereof can be exposed to the environment described in the international industrial waterproof grade standard IPX4 for use.
[0163] The volume of the reaction chamber is 550 L, the temperature of the reaction chamber is controlled at 40° C., and the flow rate of helium gas introduced as a plasma source is 200 sccm.
[0164] Step (2) introducing the reaction raw materials until the vacuum degree is 200 mTorr and starting the plasma discharge;
[0165] The reaction raw material steam is introduced by atomizing and volatilizing the reaction raw material through a feed pump, and then introduced into the reaction chamber at a low pressure of 120 mTorr, and the flow rate of the reaction raw material is 250 μL / min;
[0166] The composition of the reaction raw materials is as follows:
[0167] The unsaturated fluorocarbon compound in the reaction raw material is R 2 CH=CHR 4 , where R 2 Cl, R 4 -OCO(CH 2 ) 2 C 5 F 11 .
[0168] In step (2), the power of starting plasma discharge is 250W, the plasma discharge mode is radio frequency discharge, the output mode is pulse, the pulse width is 200μs, and the repetition frequency is 600Hz. In the cyclic coating process, the plasma discharge process can be discharged for 50 seconds, and then the discharge is continuously turned off for 20 seconds, and the above process is repeated 50 times.
[0169] Step (3) The vacuum degree of the reaction chamber is maintained at 150 mTorr, and after 4 minutes, the vacuum is introduced into the chamber to an atmospheric pressure.
[0170] Example 8
[0171] Step (1) placing the substrate in the reaction chamber of the reaction device, continuously evacuating the reaction chamber to a vacuum degree of 120 mTorr, and introducing a mixture of argon and helium;
[0172] The substrate is a solid material, the solid material is an electrical component, and after the waterproof film layer is prepared on the surface of the substrate, any interface thereof can be exposed to the environment described in the international industrial waterproof grade standard IPX5 for use.
[0173] The volume of the reaction chamber is 500 L, and the temperature of the reaction chamber is controlled at 35° C.; a mixture of argon and helium is introduced as a plasma source with a flow rate of 200 sccm.
[0174] Step (2) introducing the reaction raw materials until the vacuum degree is 200 mTorr and starting the plasma discharge;
[0175] The reaction raw material steam is introduced by atomizing and volatilizing the reaction raw material through a feed pump, and introducing the reaction raw material into the reaction chamber at a low pressure of 150 mTorr, and the flow rate of the reaction raw material is 300 μL / min;
[0176] The composition of the reaction raw materials is as follows:
[0177] The unsaturated fluorocarbon compound in the reaction raw material is R 2 CH=CHR 4 , where R 2 Cl, R 4 -C(O)OCH 2 C 5 F 11 .
[0178] The power of starting the plasma discharge in step (2) is 300 W, and the plasma discharge mode is medium frequency discharge. In the cyclic coating process, the plasma discharge process can be first discharged for 60 seconds, and then continuously turned off for 20 seconds, and the above process can be repeated 10 times.
[0179] Step (3) The vacuum degree of the reaction chamber is maintained at 160 mTorr, and after 4 minutes, the vacuum is introduced into the reaction chamber to an atmospheric pressure.
[0180] Example 9
[0181] Step (1) placing the substrate in the reaction chamber of the reaction device, continuously evacuating the reaction chamber to a vacuum degree of 100 mTorr, and introducing argon gas;
[0182] The substrate is a solid material, the solid material is an electrical component, and after the waterproof film layer is prepared on the surface of the substrate, any interface thereof can be exposed to the environment described in the international industrial waterproof grade standard IPX5 for use.
[0183] The volume of the reaction chamber is 1000 L, the temperature of the reaction chamber is controlled at 50° C., and the flow rate of argon gas introduced as a plasma source is 200 sccm.
[0184] Step (2) introducing the reaction raw materials until the vacuum degree is 200 mTorr and starting the plasma discharge;
[0185] The reaction raw material steam is introduced by atomizing and volatilizing the reaction raw material through a feed pump, and then introduced into the reaction chamber at a low pressure of 200 mTorr, and the flow rate of the reaction raw material is 100 μL / min;
[0186] The composition of the reaction raw materials is as follows:
[0187] The unsaturated fluorocarbon compound in the reaction raw material is R 2 CH=CHR 4 , where R 2 Cl, R 4 For -(CH 2 ) 2 C 6 F 13 .
[0188] The power of starting the plasma discharge in step (2) is 200 W, and the plasma discharge mode is electric spark discharge. In the cyclic coating process, the plasma discharge process can be discharged for 100 seconds first, and then the discharge is continuously turned off for 50 seconds, and the above process is repeated 20 times.
[0189] Step (3) The vacuum degree of the reaction chamber is maintained at 160 mTorr, and after 4 minutes, the vacuum is introduced into the chamber to an atmospheric pressure.
[0190] Example 10
[0191] Step (1) placing the substrate in the reaction chamber of the reaction device, continuously evacuating the reaction chamber to a vacuum degree of 150 mTorr, and introducing nitrogen;
[0192] The substrate is a solid material, the solid material is an electrical component, and after the waterproof film layer is prepared on the surface of the substrate, any interface thereof can be exposed to the environment described in the international industrial waterproof grade standard IPX6 for use.
[0193] The volume of the reaction chamber is 560 L, the temperature of the reaction chamber is controlled at 50° C., and the flow rate of nitrogen gas introduced as a plasma source is 220 sccm.
[0194] Step (2) introducing the reaction raw materials until the vacuum degree is 220 mTorr and starting the plasma discharge;
[0195] The reaction raw material steam is introduced by atomizing and volatilizing the reaction raw material through a feed pump, and then introduced into the reaction chamber at a low pressure of 150 mTorr, and the flow rate of the reaction raw material is 320 μL / min;
[0196] The composition of the reaction raw materials is as follows:
[0197] The unsaturated fluorocarbon compound in the reaction raw material is R 2 CH=CHR 4 , where R 2 Cl, R 4 -C(O)O(CH 2 ) 2 C 5 F 11 .
[0198] The power of starting the plasma discharge in step (2) is 240 W, and the plasma discharge mode is microwave discharge. In the cyclic coating process, during the plasma discharge process, the discharge can be started for 10 seconds (t1), and then the discharge can be turned off for 5 seconds (t2), and the above process can be repeated 50 times.
[0199] Step (3) The vacuum degree of the reaction chamber is maintained at 160 mTorr, and after 4 minutes, the vacuum is introduced into the chamber to an atmospheric pressure.
[0200] Comparative Example 10A is different from Example 10 in that the plasma discharge is first started for 500 seconds and then the discharge is stopped for 250 seconds, and the raw materials are kept flowing in the whole process.
[0201] Comparative Example 10B is different from Example 10 in that the plasma discharge is continuously turned on during the entire coating process until the coating is completed, and the discharge time is 750 s.
[0202] The thickness of the film layer was measured using an American Filmetrics F20-UV-film thickness measuring instrument.
[0203] The water contact angle of hydrophobic surface coating is tested according to GB / T 30447-2013 standard.
[0204] Salt spray resistance test is carried out according to GB / T 2423.18-2000 Environmental testing methods for electrical and electronic products.
[0205] Appendix 1: Performance parameters of Examples 1-10
[0206]
[0207]
[0208] Note: Example 4 is a fabric and no salt spray resistance test was performed.
[0209] The film thickness was measured using an American Filmetrics F20-UV-film thickness measuring instrument.
[0210] The water contact angle of the film layer is tested according to GB / T 30447-2013 standard.
[0211] The test-related data of the film layers obtained in Example 10, Comparative Example 10A and Comparative Example 10B are as follows:
[0212]
[0213] Example 11a
[0214] Step (1) placing a 5 cm x 5 cm piece of aluminum in a 100-liter plasma vacuum reaction chamber, pumping the vacuum degree in the reaction chamber to 0.1 mTorr, and introducing nitrogen;
[0215] The temperature of the reaction chamber is controlled at 50° C. The flow rate of nitrogen as a plasma source is 220 sccm. Radio frequency plasma discharge is turned on to pretreat the metal aluminum. The discharge power in the pretreatment stage is 80 W, and the discharge is continued for 500 s.
[0216] In step (2), monomer 1 and then monomer 2 are introduced at a flow rate of 150 μL / min, and the introduction time is 600 s and 400 s respectively.
[0217] The composition of the reaction raw materials is as follows:
[0218] Monomer 1 is:
[0219]
[0220] Monomer 2 is:
[0221]
[0222] The power of starting plasma discharge in step (2) is 50W, the plasma discharge mode is radio frequency discharge, the output mode is pulse, the pulse width is 2μs, the repetition frequency is 1000Hz, and the discharge time is 500s. During the plasma discharge process, the discharge can be turned on for 10 seconds, and then the discharge can be turned off for 10 seconds, and the above process can be repeated 50 times.
[0223] After the preparation in step (3) is completed, nitrogen is introduced to restore the reaction chamber to normal pressure, and then the metal block is taken out.
[0224] Comparative Example 11b is different from Example 11a in that the plasma discharge is first started for a period of 500 seconds, and then the discharge is stopped and the introduction of the raw material is maintained within 500 seconds.
[0225] Comparative Example 11c is different from Example 11a in that the plasma discharge is continuously turned on during the entire coating process until the coating is completed, and the discharge time is 1000 s.
[0226] Example 12a
[0227] (1) An iron block was placed in a 200 L plasma vacuum reaction chamber, and the reaction chamber was continuously evacuated to a vacuum degree of 0.8 mTorr.
[0228] (2) Helium gas is introduced at a flow rate of 50 sccm, and radio frequency plasma discharge is turned on to pretreat the iron block substrate (i.e., radio frequency pretreatment plasma discharge is turned on). The discharge power in the pretreatment stage is 20 W, and the discharge is continued for 100 seconds.
[0229] (3) Monomer s is introduced to the surface of the substrate for chemical vapor deposition to prepare a nano coating. The monomer flow rate is 150 μL / min. After being vaporized, it is introduced into the reaction chamber for 1500 seconds. The plasma discharge used for pretreatment is adjusted to the plasma discharge used for deposition. The power of the plasma discharge in the cavity during the deposition stage is 250W, and the plasma discharge method is microwave discharge. Cyclic coating is used in the deposition process, and the discharge time is 900 seconds. During the plasma discharge process, the discharge can be turned on for 30 seconds, and then the discharge can be turned off for 20 seconds. The above process is repeated 30 times.
[0230] Monomer s is:
[0231]
[0232] Comparative Example 12b is different from Example 12a in that the plasma discharge is first started for 900 seconds, and then the discharge is stopped and the raw material is continuously introduced for 600 seconds.
[0233] Comparative Example 12c is different from Example 12a in that the plasma discharge is continuously turned on for 1500 seconds during the entire coating process until the coating is completed.
[0234] Example 13a
[0235] (1) A copper sheet was placed in a 100 L plasma vacuum reaction chamber, and the reaction chamber was continuously evacuated to a vacuum degree of 100 mTorr.
[0236] (2) Argon gas was introduced at a flow rate of 100 sccm, and microwave plasma discharge was started to pre-treat the metal copper sheet (i.e., microwave pre-treatment plasma discharge was started). The discharge power in the pre-treatment stage was 200 W, the microwave discharge frequency was 100 MHz, and the discharge lasted for 200 s.
[0237] (3) The monomer x is vaporized and introduced into the reaction chamber to prepare the nano coating by chemical vapor deposition on the surface of the substrate. During the coating preparation process, the monomer flow rate is 80 μL / min, the introduction time is 1000 s, and the pretreatment plasma discharge is adjusted to the deposition plasma discharge. The plasma discharge in the deposition stage is a cyclic microwave discharge with a total discharge time of 500 s. The discharge can be turned on for 10 seconds and then turned off for 10 seconds. The above process is repeated 50 times.
[0238] Monomer x is:
[0239]
[0240] Comparative Example 13b is different from Example 13a in that the plasma discharge is first started for a period of 500 seconds, and then the discharge is stopped and other coating conditions such as raw material concentration are maintained for 500 seconds.
[0241] Comparative Example 13c is different from Example 13a in that the plasma discharge is continuously turned on during the entire coating process until the coating is completed, and the discharge time is 1000 s.
[0242] The film thickness was measured using an American Filmetrics F20-UV-film thickness measuring instrument.
[0243] The water contact angle of the film layer is tested according to GB / T 30447-2013 standard.
[0244] Salt spray resistance test is carried out according to GB / T 2423.18-2000 Environmental testing methods for electrical and electronic products.
[0245] The film layers obtained in Examples 11a, 12a, and 13a and Comparative Examples 11b, 11c, 12b, 12c, 13b, and 13c, the test-related data are as follows:
[0246]
[0247] It should be understood by those skilled in the art that the above description and the embodiments of the present invention are only examples and do not limit the present invention. The purpose of the present invention has been fully and effectively achieved. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments, and the embodiments of the present invention may be deformed or modified in any way without departing from the principles.
Claims
1. A cyclic coating method, characterized in that: The steps include: introducing reaction materials into a reaction chamber; and Plasma enhanced chemical vapor deposition is performed on a substrate surface in the reaction chamber under cyclic coating conditions to form a film layer, wherein the plasma discharge is turned on for a preset time, and then the discharge is turned off for a preset time, which is a coating cycle, and the above process is repeated for cyclic coating, and the supply of reaction raw materials is maintained during the whole process; The duration of plasma discharge in each cycle is t1, and the duration of plasma discharge being turned off in each cycle is t2, wherein t1 is 10 seconds and t2 is 5 seconds, t1 is 10 seconds and t2 is 10 seconds, t1 is 10 seconds and t2 is 20 seconds, t1 is 20 seconds and t2 is 20 seconds, t1 is 30 seconds and t2 is 20 seconds, t1 is 50 seconds and t2 is 20 seconds, t1 is 60 seconds and t2 is 20 seconds, or t1 is 100 seconds and t2 is 50 seconds.
2. The cyclic coating method according to claim 1, wherein the duration of the plasma discharge during each cycle is t1, and t1 in the previous cycle and the next cycle is the same.
3. The cyclic coating method according to claim 1, wherein the duration of the plasma discharge being shut down during each cycle is t2, and t2 in the previous cycle and the next cycle is the same.
4. A cyclic coating method according to any one of claims 1 to 3, wherein the reaction raw material is fluoride.
5. The cyclic coating method according to claim 4, wherein the fluoride is a fluorinated alcohol and has the structural formula: n F 2n+1 -C m H 2m -OH, wherein n is an integer of 1-12, and m is an integer of 0-4.
6. The cyclic coating method according to any one of claims 1 to 3, wherein the reaction raw materials have the general formula R1R2C=CR3R4, wherein R1, R2 and R3 are independently selected from hydrogen, alkyl, halogen, halogenated alkyl or aryl, wherein at least one of R1, R2 and R3 is halogen, wherein R4 is a group X-R5, R5 is an alkyl or halogenated alkyl group, and X is a bond; or X is a group -C(O)O(CH2)nY-, wherein n is an integer from 0 to 10, and Y is a bond or a sulfonamide group; or X is a group -OC(O)-(CH2)iZ-, wherein i is an integer from 0 to 10, and Z is a bond or a sulfonamide group; or X is a group -(CH2)xU-, wherein x is an integer from 0 to 10, and U is a bond or a sulfonamide group; or X is a group -(O) p R6(O) q (CH2)t-, wherein R6 is aryl optionally substituted with halogen, p is 0 or 1, q is 0 or 1, and t is 0 or an integer from 1 to 10, provided that when q is 1, t is non-0.
7. The cyclic coating method according to any one of claims 1 to 3, wherein the reaction raw material is an organic silicon compound having the structural formula: Among them, R8, R9, R 10 , R 11 , R 12 , R 13 It is a group connected to unsaturated carbon-carbon double bonds and Si atoms and can be independent is independently selected from alkyl, aryl, halogen, halogenated alkyl, halogenated aryl, alkoxy or vinyl, and K is an integer of 0-8.
8. The cyclic coating method according to any one of claims 1 to 3, wherein the reaction raw material is an epoxy compound and has the following structural formula: in, R1, R2, and R3 are independently selected from hydrogen, alkyl, aryl, halogen, halogenated alkyl, or hydroxyl; X is hydrogen or halogen, m is an integer of 0-8, and n is an integer of 1-15.
9. The cyclic coating method according to any one of claims 1 to 3, wherein the reaction raw material is an acrylamide compound, and has the following structural formula: Compound monomer 1, or monomer 2, or a mixture of monomer 1 and monomer 2: Monomer 1 Monomer 2 in, R1, R2, R3, R6, R7, R8 are independently selected from hydrogen, alkyl, aryl, halogen, haloalkyl, alkenyl or haloalkenyl, X, Y are hydrogen or halogen; R4, R5 are independently selected from hydrogen, alkyl, aryl, halogen, haloalkyl or have the following structure: Among them, R 11 is a straight chain or branched alkane subunit having 1 to 15 carbon atoms, R 12 , R 13 , R 14 , R 15 are independently selected from hydrogen, alkyl, aryl, halogen or haloalkyl; R9, R 10 are independently selected from a linear, branched alkyl subunit or an aryl subunit having 1 to 15 carbon atoms; or R9, R 10 is the connecting key; m, n, p, q are integers of 0-20, but m and n are not 0 at the same time, and p and q are not 0 at the same time.
10. The cyclic coating method according to any one of claims 1 to 3, wherein the plasma discharge mode is radio frequency discharge, microwave discharge, medium frequency discharge or spark discharge.
11. A film layer, characterized in that Using the reaction raw materials to form a film on the surface of a substrate by a plasma chemical vapor deposition method in a cyclic coating manner, wherein the plasma discharge is turned on for a preset time, and then the discharge is turned off for a preset time, which is a coating cycle, and the above process is repeated for a cyclic coating, and the reaction raw materials are kept supplied during the whole process; The duration of plasma discharge in each cycle is t1, and the duration of plasma discharge being turned off in each cycle is t2, wherein t1 is 10 seconds and t2 is 5 seconds, t1 is 10 seconds and t2 is 10 seconds, t1 is 10 seconds and t2 is 20 seconds, t1 is 20 seconds and t2 is 20 seconds, t1 is 30 seconds and t2 is 20 seconds, t1 is 50 seconds and t2 is 20 seconds, t1 is 60 seconds and t2 is 20 seconds, or t1 is 100 seconds and t2 is 50 seconds. 12 . The film layer according to claim 11 , wherein the duration of the plasma discharge during each cycle is t1 , and t1 in a previous cycle and a next cycle is the same.
13. The film layer according to claim 11, wherein the duration of the plasma discharge being turned off during each cycle is t2, and t2 in a previous cycle and a next cycle is the same.
14. The film layer according to any one of claims 11 to 13, wherein the reaction raw material is a fluoride.
15. The film layer according to claim 14, wherein the fluoride is a fluorinated alcohol and has the structural formula: n F 2n+1 -C m H 2m -OH, wherein n is an integer of 1-12, and m is an integer of 0-4.
16. The film layer according to any one of claims 11 to 13, wherein the reaction raw materials have the general formula R1R2C=CR3R4, wherein R1, R2 and R3 are independently selected from hydrogen, alkyl, halogen, haloalkyl or aryl, wherein at least one of R1, R2 and R3 is a halogen, wherein R4 is a group X-R5, R5 is an alkyl or haloalkyl group, and X is a bond; or X is a group -C(O)O(CH2)nY-, wherein n is an integer from 0 to 10, and Y is a bond or a sulfonamide group; or X is a group -OC(O)-(CH2)iZ-, wherein i is an integer from 0 to 10, and Z is a bond or a sulfonamide group; or X is a group -(CH2)xU-, wherein x is an integer from 0 to 10, and U is a bond or a sulfonamide group; or X is a group -(O) p R6(O) q (CH2)t-, wherein R6 is aryl optionally substituted with halogen, p is 0 or 1, q is 0 or 1, and t is 0 or an integer from 1 to 10, provided that when q is 1, t is non-0.
17. The film layer according to any one of claims 11 to 13, wherein the reaction raw material is an organosilicon compound having the structural formula: Among them, R8, R9, R 10 , R 11 , R 12 , R 13 It is a group connected to an unsaturated carbon-carbon double bond and a Si atom, and can be independently selected from an alkyl group, an aryl group, a halogen group, a halogenated alkyl group, a halogenated aryl group, an alkoxy group or a vinyl group, and K is an integer of 0-8.
18. The film layer according to any one of claims 11 to 13, wherein the reaction raw material is an epoxy compound and has the following structural formula: in, R1, R2, and R3 are independently selected from hydrogen, alkyl, aryl, halogen, halogenated alkyl, or hydroxyl; X is hydrogen or halogen, m is an integer of 0-8, and n is an integer of 1-15.
19. The film layer according to any one of claims 11 to 13, wherein the reaction raw material is an acrylamide compound, and has the following structural formula: Compound monomer 1, or monomer 2, or a mixture of monomer 1 and monomer 2: Monomer 1 Monomer 2 in, R1, R2, R3, R6, R7, R8 are independently selected from hydrogen, alkyl, aryl, halogen, haloalkyl, alkenyl or haloalkenyl, X, Y are hydrogen or halogen; R4, R5 are independently selected from hydrogen, alkyl, aryl, halogen, haloalkyl or have the following structure: Among them, R 11 is a straight chain or branched alkane subunit having 1 to 15 carbon atoms, R 12 , R 13 , R 14 , R 15 are independently selected from hydrogen, alkyl, aryl, halogen or haloalkyl; R9, R 10 are independently selected from a linear, branched alkyl subunit or an aryl subunit having 1 to 15 carbon atoms; or R9, R 10 is the connecting key; m, n, p, q are integers of 0-20, but m and n are not 0 at the same time, and p and q are not 0 at the same time.
20. A product, characterized in that The product is provided with a film layer, wherein the film layer is formed on a substrate surface by a plasma chemical vapor deposition method using a reaction raw material in a cyclic coating manner, wherein the plasma discharge is turned on for a preset time, and then the discharge is turned off for a preset time, which is a coating cycle, and the above process is repeated for cyclic coating, and the reaction raw material supply is maintained during the whole process; The duration of plasma discharge in each cycle is t1, and the duration of plasma discharge being turned off in each cycle is t2, wherein t1 is 10 seconds and t2 is 5 seconds, t1 is 10 seconds and t2 is 10 seconds, t1 is 10 seconds and t2 is 20 seconds, t1 is 20 seconds and t2 is 20 seconds, t1 is 30 seconds and t2 is 20 seconds, t1 is 50 seconds and t2 is 20 seconds, t1 is 60 seconds and t2 is 20 seconds, or t1 is 100 seconds and t2 is 50 seconds.