A surface treatment method for titanium cathode roller
Through the combination of mechanical polishing pretreatment, chemical mechanical polishing and anodizing treatment, the problem of insufficient surface roughness uniformity of titanium cathode rollers is solved, and lower roller surface roughness and higher roughness uniformity are achieved , extends the production cycle and improves the quality of electrolytic copper foil.
Patent Information
- Application Number
- CN202210090821.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-01-26
AI Technical Summary
In the prior art, the roughness Ra index in the surface treatment method of titanium cathode rollers is single, and the roller surface roughness cannot be minimized, the roughness uniformity is improved, and the stable production time is extended.
Using a combination of mechanical polishing pretreatment, chemical mechanical polishing and anodizing treatment, oxidizing substances are removed through grinding wheels, and polished using nano-grinding materials and specific polishing liquid to generate a dense protective layer, improving the uniformity of roller surface roughness and Antioxidant properties.
It significantly reduces the roughness and uniformity of the roller surface of the titanium cathode roller, extends the stable production time, and improves the equipment production rate and the quality of electrolytic copper foil.
Smart Images

Figure CN114438551B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrolytic copper foil, and in particular relates to a surface treatment method for a titanium cathode roller. Background Art
[0002] Electrolytic copper foil is an indispensable key material for lithium-ion batteries and printed circuit boards, and plays a vital role in the fields of new energy and electronic circuits. In the production process of electrolytic copper foil, copper ions in the electrolyte are reduced to copper atoms by electrons on the surface of the titanium cathode roller, and are arranged according to a certain rule to form electrolytic copper foil. In this process, the surface state of the titanium cathode roller will directly affect the nucleation and growth process of copper atoms, thereby affecting the microscopic crystal structure of the copper foil, and ultimately affecting the macroscopic properties of the copper foil such as surface density uniformity, tensile strength, elongation, warping and appearance. However, in the process of electrolytic foil production, due to the influence of electrolyte, current and electrochemical reaction, a certain degree of oxidation or hydrogenation will occur on the surface of the titanium cathode roller. In particular, as the electrolysis time gradually increases, the oxide layer on the surface of the titanium cathode roller will gradually accumulate slowly, causing different degrees of oxidation on the roller surface, thereby affecting the quality of the copper foil. Therefore, after a period of continuous electrolytic foil production, the titanium cathode roller needs to be polished offline to remove the excessively grown oxide layer on the surface.
[0003] At present, the offline polishing of titanium cathode rollers mostly uses mechanical polishing to remove the surface oxide layer. The roughness Ra value of the roller surface after polishing is usually used as the criterion for judging the offline polishing effect of titanium cathode rollers. The Ra value of titanium cathode rollers after mechanical polishing is generally between 0.1 μm and 0.3 μm.
[0004] Traditional mechanical polishing will form different degrees of polishing marks on the roller surface, resulting in uneven roughness of the roller surface. After mechanical polishing, a very thin oxide film will be formed on the surface of the titanium roller in the atmosphere to protect the titanium material from corrosion. However, the thickness of the oxide film formed by oxidation in the natural state is uneven, which will lead to a certain degree of difference in the roughness and conductivity of the roller surface.
[0005] Among the common polishing methods: chemical polishing removes surface substances through chemical reactions between the polishing liquid and the material to be polished, and can obtain a polished surface with lower roughness. Mechanical polishing removes the components of the surface of the material to be polished through mechanical force, and can achieve rapid polishing of the workpiece. Chemical mechanical polishing combines the characteristics of chemical polishing and mechanical polishing, effectively improving the polishing efficiency while obtaining a polished surface with lower roughness; and during the chemical mechanical polishing process, the polishing liquid reacts chemically with the components on the surface of the workpiece to soften the surface material of the workpiece; the polishing disc transfers the energy required to break the weakly bonded molecular chains to the polishing particles, removing the softened layer on the surface of the workpiece.
[0006] Due to the above process reasons, the existing technology often uses mechanical polishing combined with chemical mechanical polishing to process the roller surface. However, the stable production cycle of titanium cathode rollers still needs to be improved.
[0007] According to existing research, the roughness uniformity of the titanium cathode roller surface will have a significant impact on the nucleation and growth of electrolytic copper foil. The inventors have also found through a large number of experiments that roughness uniformity can be used as a quantitative indicator of the polishing effect of titanium cathode rollers. Roughness uniformity refers to the ratio between the extreme difference in roughness and the average roughness in the measurement area.
[0008]
[0009] Among them, E R is the roughness uniformity, ΔR is the range of roughness, and R is the average roughness. R The smaller the value, the better the roughness uniformity, the easier it is for the nucleation and growth of the electrolytic copper foil, and the longer the stable production cycle of the titanium cathode roller.
[0010] Based on the above new research and development direction and the lack of supporting treatment methods for experimental results, the present invention proposes a surface treatment technology for titanium cathode rollers. Summary of the invention
[0011] The purpose of the present invention is to provide a surface treatment method for a titanium cathode roller to solve the problem that the surface treatment method for a titanium cathode roller in the prior art uses a single roughness Ra index as a judgment, and is unable to reduce the roughness of the titanium cathode roller surface to the greatest extent, improve the uniformity of the roughness of the titanium cathode roller surface, and extend the stable production time of the titanium cathode roller.
[0012] In order to solve the above problems, the technical solution of the present invention is:
[0013] A surface treatment method for a titanium cathode roller, the method comprising the following steps:
[0014] Step A, mechanical polishing pretreatment of the titanium cathode roller;
[0015] Use a crane to hoist the titanium cathode roller that needs surface treatment to the grinder, set the rotation speed of the grinding wheel on the polishing disc, the cylinder pressure and the lateral movement speed, respectively start the rotating motors of the grinding wheel and the titanium cathode roller, and perform mechanical polishing pretreatment on the roller surface of the titanium cathode roller;
[0016] Step B, chemical mechanical polishing of the titanium cathode roller;
[0017] The mechanical grinding wheel is replaced with polishing discs symmetrically distributed on both sides of the horizontal diameter of the cathode roller, and the flow rate of the polishing liquid nozzle and the rotation speed of the cathode roller are set to start chemical mechanical polishing of the titanium cathode roller;
[0018] Step C, anodizing the polished titanium cathode roller;
[0019] 1. Use deionized water to remove impurities remaining on the surface of the titanium cathode roller after chemical mechanical polishing;
[0020] 2. Use compressed air to dry the residual moisture on the surface of the titanium cathode roller;
[0021] 3. Using a metal titanium plate as the cathode, a polished titanium cathode roller as the anode, and a deionized water-ethylene glycol solution containing ammonium fluoride as the electrolyte, anodizing treatment is performed at a certain voltage to form a thin and dense protective layer on the roller surface of the titanium cathode roller.
[0022] Furthermore, the polishing liquid in step B is composed of nano-abrasive material, etchant, pH regulator, surfactant and deionized water; and its preparation process is as follows:
[0023] Add an appropriate amount of deionized water to the polishing liquid preparation tank, add surfactant, etchant, pH stabilizer and nano-abrasive material under mechanical stirring, continue stirring to make the components in the polishing liquid fully mixed, and then transport the polishing liquid to a polishing liquid storage tank with a stirring function, continue stirring for standby use.
[0024] Furthermore, the electrolyte solute used in the anodizing treatment in step C-3 includes but is not limited to ammonium fluoride and ammonium chloride, the solvent is deionized water-ethylene glycol, the voltage is between 35 V and 50 V, and the treatment time is between 3 minutes and 5 minutes.
[0025] Furthermore, in the chemical mechanical polishing operation of step B, a polishing disc is used to polish the titanium cathode roller, and the polishing discs are symmetrically distributed on both sides of the titanium cathode roller. During the polishing process, the polishing disc is in direct contact with the titanium cathode roller, and the polishing liquid is delivered to the nozzle just above the highest point of the titanium cathode roller and above the contact point between the titanium cathode roller and the polishing disc by a delivery pump;
[0026] During the whole process, the polishing liquid passing through the polishing disc finally collects into the low-level tank along the roller surface of the titanium cathode roller. The lower roller surface of the titanium cathode roller is immersed in the polishing liquid in the low-level tank. The height of the titanium cathode roller immersed in the low-level tank is greater than 1 / 6 of the diameter of the cathode roller.
[0027] During the process, the linear speeds of the titanium cathode roller and the polishing disc are different, and the linear speed of the polishing disc is greater than the linear speed of the titanium cathode roller.
[0028] Furthermore, the mesh number of the grinding wheel for mechanical polishing in step A is 120 meshes to 300 meshes.
[0029] Furthermore, the nano-abrasive material in the polishing liquid is spherical with a diameter between 20-200 nm; the nano-abrasive material is one or more of colloidal alumina (Al2O3), colloidal silicon dioxide (SiO2), silicon nitride (Si3N4) or cerium oxide (CeO2); the mass concentration of the nano-abrasive material in the polishing liquid is between 1wt%-4wt%.
[0030] Furthermore, the etching agent in the polishing liquid is two or more of lactic acid, chloroacetic acid, hydrogen peroxide, hydrofluoric acid, oxalic acid, citric acid, and ethylenediaminetetraacetic acid-2 sodium (EDTA-2Na); the mass concentration of the etching agent in the polishing liquid is between 5wt% and 10wt%.
[0031] Furthermore, the pH value of the polishing liquid is between 3-5.
[0032] Further, the pH regulator in the polishing liquid is composed of an inorganic-organic composite component;
[0033] The inorganic pH regulator is at least two or more of acetic acid, hydrochloric acid, nitric acid, ammonia water, and sodium hydroxide;
[0034] The organic pH regulator is two or more of tetramethylammonium hydroxide, tetraethylammonium hydroxide, salicylic acid, and ascorbic acid;
[0035] The mass concentration of the pH regulator in the polishing liquid is between 1wt% and 1.5wt%.
[0036] Furthermore, the surfactant in the polishing liquid is one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, polyvinyl pyrrolidone, and polyethylene glycol; and the mass concentration of the surfactant in the polishing liquid is between 0.01wt% and 0.1wt%.
[0037] The beneficial effects of the present invention are as follows:
[0038] (1) The present invention introduces the roughness uniformity E based on the roughness Ra of the roller surface after polishing. RAs another quantitative indicator of the polishing effect of the titanium cathode roller, in this research and development direction, mechanical polishing pretreatment, chemical mechanical polishing, and anodizing processes are used. First, the titanium cathode roller is mechanically polished and pretreated with a grinding wheel to remove the outermost oxidizing substances on the roller surface; then the pretreated titanium cathode roller is further polished by chemical mechanical polishing to reduce the roughness of the roller surface while improving the roughness uniformity of the roller surface; finally, a dense protective layer is generated on the polished titanium cathode roller surface with the help of anodizing. While reducing the roughness of the roller surface, the roughness uniformity of the roller surface can be improved. Further anodizing treatment can make the surface oxide layer of the titanium cathode roller more uniform and more resistant to oxidation. While reducing the roughness of the roller surface, the roughness uniformity of the roller surface can be improved, and a uniform protective oxide layer can be quickly generated on the surface of the titanium cathode roller, which can effectively extend the stable production cycle of the titanium cathode roller, improve the production utilization rate of the equipment, and improve the quality of the electrolytic copper foil.
[0039] (2) The present invention has concluded through a large number of experiments and production verifications that the roughness Sa can be reduced by 27%, the roughness Sq can be reduced by 42%, and the roughness uniformity E R It can be improved by 40%, and the stable production time after polishing is extended by 33%. Therefore, compared with the traditional surface treatment process, it has a very significant improvement effect in reducing the roughness of the titanium cathode roller surface, improving the uniformity of the roughness of the titanium cathode roller surface, and extending the stable production time of the titanium cathode roller, which has important economic significance in production. Therefore, the application of the present invention has considerable economic value and excellent promotion prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 It is a schematic diagram of the structure of a chemical mechanical polishing device for a titanium cathode roller;
[0041] Figure 2 This is a comparison diagram of the effects of the microscopic image analysis of the smooth surface of the electrolytic green foil produced by the titanium cathode roller after being processed by the method of the present invention and the conventional mechanical polishing method. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention as claimed but is merely representative of selected embodiments of the present invention.
[0044] Implementation
[0045] A surface treatment method for a titanium cathode roller comprises the following steps:
[0046] Step A, mechanical polishing pretreatment of the titanium cathode roller;
[0047] Use a crane to hoist the titanium cathode roller that needs surface treatment to the grinder, select a grinding wheel with a mesh size of 120-300, set the rotation speed of the grinding wheel on the polishing disc, the cylinder pressure and the lateral movement speed, respectively start the rotating motors of the grinding wheel and the titanium cathode roller, and perform mechanical polishing pretreatment on the roller surface of the titanium cathode roller.
[0048] Step B, chemical mechanical polishing of the titanium cathode roller;
[0049] like Figure 1 As shown, the mechanical grinding wheel is replaced with polishing discs symmetrically distributed on both sides of the horizontal diameter of the cathode roller. After setting the flow rate of the polishing liquid nozzle and the rotation speed of the cathode roller, the titanium cathode roller is subjected to chemical mechanical polishing.
[0050] Specifically: the polishing discs are symmetrically distributed on both sides of the titanium cathode roller. During the polishing process, the polishing discs are in direct contact with the titanium cathode roller. The polishing liquid is delivered to the nozzle just above the highest point of the titanium cathode roller and above the contact point between the titanium cathode roller and the polishing disc through a delivery pump.
[0051] During the whole process, the polishing liquid passing through the polishing disk finally gathers into the low-level tank along the roller surface of the titanium cathode roller. The lower roller surface of the titanium cathode roller is immersed in the polishing liquid in the low-level tank. The height of the titanium cathode roller immersed in the low-level tank is greater than 1 / 6 of the diameter of the cathode roller.
[0052] During the process, the linear speeds of the titanium cathode roller and the polishing disc are different, and the linear speed of the polishing disc is greater than the linear speed of the titanium cathode roller.
[0053] In the above steps, the polishing liquid is composed of nano-abrasive material, etching agent, pH regulator, surfactant and deionized water.
[0054] The nano-abrasive material is spherical with a diameter between 20-200 nm; the nano-abrasive material is one or more of colloidal alumina (Al2O3), colloidal silicon dioxide (SiO2), silicon nitride (Si3N4) or cerium oxide (CeO2); the mass concentration of the nano-abrasive material in the polishing liquid is between 1wt% and 4wt%.
[0055] The etchant is composed of two or more of lactic acid, chloroacetic acid, hydrogen peroxide, hydrofluoric acid, oxalic acid, citric acid and EDTA-2Na with a mass concentration of 5wt%.
[0056] The pH regulator is composed of inorganic-organic composite components with a mass concentration between 1wt% and 1.5wt%; the inorganic regulator is at least two or more of acetic acid, hydrochloric acid, nitric acid, ammonia water, and sodium hydroxide; the organic regulator is two or more of tetramethylammonium hydroxide, tetraethylammonium hydroxide, salicylic acid, and ascorbic acid.
[0057] The surfactant is composed of one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, polyvinyl pyrrolidone and polyvinyl alcohol with a mass concentration of 0.1wt%.
[0058] During preparation: first add an appropriate amount of deionized water to the polishing liquid preparation tank, add surfactant, etchant, pH stabilizer and nano-abrasive material under mechanical stirring, continue stirring to make the components in the polishing liquid fully mixed, then transport the polishing liquid to a polishing liquid storage tank with a stirring function, continue stirring for standby use.
[0059] The pH value of the final polishing liquid is between 3-5.
[0060] During polishing:
[0061] Polishing liquid temperature: 25 ℃; polishing liquid nozzle pressure: 0.2-0.5 MPa; polishing time: 60-90 min; titanium cathode roller speed: 2 m / min.
[0062] Step C, anodizing the polished titanium cathode roller;
[0063] 1. Use deionized water to remove impurities remaining on the surface of the titanium cathode roller after chemical mechanical polishing;
[0064] 2. Use compressed air to dry the residual moisture on the surface of the titanium cathode roller;
[0065] 3. Using a metal titanium plate as the cathode, a polished titanium cathode roller as the anode, and a deionized water-ethylene glycol solution containing ammonium fluoride or ammonium chloride as the electrolyte, anodizing treatment is performed at a voltage between 35 V and 50 V for 3 minutes to 5 minutes to form a thin and dense protective layer on the roller surface of the titanium cathode roller.
[0066] Example 1
[0067] Use a crane to hoist the titanium cathode roller with oxidized surface to the grinder and perform the following treatments in sequence:
[0068] Step A, mechanical polishing pretreatment of the titanium cathode roller;
[0069] Grinding wheel size: 120 mesh;
[0070] Grinding wheel speed: 20 m / min;
[0071] Grinding wheel lateral movement speed: 50 mm / min
[0072] Cathode roller speed: 2 m / min;
[0073] Polishing time: 30 min;
[0074] Step B, chemical mechanical polishing of the titanium cathode roller;
[0075] Polishing disc material: short-pile Micro Met synthetic fiber;
[0076] The polishing liquid is composed of abrasive materials, etchants, pH regulators, and surfactants. The specific ingredients are as follows:
[0077] Colloidal SiO2: diameter 50 nm, concentration 4wt%; Colloidal Al2O3: diameter 200 nm, concentration 1wt%;
[0078] H2O2 concentration: 5wt%; Lactic acid concentration: 5wt%;
[0079] Acetic acid concentration: 1wt%; Ammonia concentration: 1wt%;
[0080] Tetramethylammonium hydroxide concentration: 1.5wt%; Ascorbic acid concentration: 1.5wt%;
[0081] Polyvinyl pyrrolidone concentration: 0.1wt%;
[0082] Polishing liquid temperature: 25℃;
[0083] Polishing fluid nozzle pressure: 0.4 MPa;
[0084] Polishing disc speed: 25 m / min;
[0085] Chemical mechanical polishing time: 60 min;
[0086] Titanium cathode roller speed: 2 m / min;
[0087] Step C, anodizing the polished titanium cathode roller;
[0088] The electrolyte solute is ammonium fluoride, and the solvent is deionized water-ethylene glycol. The specific ingredients are as follows:
[0089] NH4F concentration: 0.3wt%;
[0090] Deionized water content: 10vol%;
[0091] Ethylene glycol content: 90vol%;
[0092] Electrolyte temperature: 25 °C;
[0093] Voltage: 50 V;
[0094] Processing time: 5 min;
[0095] Results: The surface roughness S of the titanium cathode roller treated by this embodiment a =0.207 μm, S q =0.281 μm, E R =8.1%, and the continuous stable production time is 60 days.
[0096] Example 2
[0097] The difference between this embodiment and embodiment 1 is that the ratio of the grinding material in step B is changed.
[0098] Step B, chemical mechanical polishing of the titanium cathode roller;
[0099] Polishing disc material: short-pile Micro Met synthetic fiber;
[0100] The polishing liquid is composed of abrasive materials, etchants, pH regulators, and surfactants. The specific ingredients are as follows:
[0101] Colloidal SiO2: diameter 20 nm, concentration 3wt%; Colloidal Al2O3: diameter 200 nm, concentration 2wt%;
[0102] H2O2 concentration: 5wt%; Chloroacetic acid concentration: 10wt%;
[0103] Hydrochloric acid concentration: 1wt%; Ammonia concentration: 1wt%;
[0104] Tetramethylammonium hydroxide concentration: 1.5wt%; Ascorbic acid concentration: 1.5wt%;
[0105] Polyvinyl pyrrolidone concentration: 0.1wt%;
[0106] Polishing liquid temperature: 25℃;
[0107] Polishing liquid nozzle pressure: 0.2 MPa;
[0108] Polishing disc speed: 25 m / min;
[0109] Chemical mechanical polishing time: 90 min;
[0110] Titanium cathode roller speed: 2 m / min;
[0111] Results: The surface roughness S of the titanium cathode roller treated by this embodiment a =0.243 μm, S q =0.324 μm, ER =8.5%, and the continuous stable production time is 55 days.
[0112] Example 3
[0113] The difference between this embodiment and embodiment 1 is that the size of one of the grinding materials in step B is changed.
[0114] Step B, chemical mechanical polishing of the titanium cathode roller;
[0115] Polishing disc material: short-pile Micro Met synthetic fiber;
[0116] The polishing liquid is composed of abrasive materials, etchants, pH regulators, and surfactants. The specific ingredients are as follows:
[0117] Colloidal SiO2: diameter 100 nm, concentration 4wt%; Colloidal Al2O3: diameter 200 nm, concentration 1wt%;
[0118] H2O2 concentration: 5wt%; Hydrofluoric acid concentration: 5wt%;
[0119] Nitric acid concentration: 1wt%; Ammonia concentration: 1wt%;
[0120] Tetramethylammonium hydroxide concentration: 1.5wt%; Ascorbic acid concentration: 1.5wt%;
[0121] Polyvinyl pyrrolidone concentration: 0.1wt%;
[0122] Polishing liquid temperature: 25℃;
[0123] Polishing fluid nozzle pressure: 0.4 MPa;
[0124] Polishing disc speed: 25 m / min;
[0125] Chemical mechanical polishing time: 60 min;
[0126] Titanium cathode roller speed: 2 m / min;
[0127] Results: The surface roughness S of the titanium cathode roller treated by this embodiment a =0.282 μm, S q =0.356 μm, E R =9.2%, and the continuous stable production time is 54 days.
[0128] Example 4
[0129] The difference between this embodiment and embodiment 1 is that the ratio of the grinding material in step B is changed, and the colloidal Al2O3 is replaced by nano CeO2 particles of the same size.
[0130] Step B, chemical mechanical polishing of the titanium cathode roller;
[0131] Polishing disc material: short-pile Micro Met synthetic fiber;
[0132] The polishing liquid is composed of abrasive materials, etchants, pH regulators, and surfactants. The specific ingredients are as follows:
[0133] Colloidal SiO2: diameter 50 nm, concentration 4wt%; Nano CeO2: diameter 200 nm, concentration 1wt%;
[0134] H2O2 concentration: 5wt%; Oxalic acid concentration: 5wt%;
[0135] Glacial acetic acid concentration: 1wt%; sodium hydroxide concentration: 1wt%;
[0136] Tetramethylammonium hydroxide concentration: 1.5wt%; Ascorbic acid concentration: 1.5wt%;
[0137] Hexadecyltrimethylammonium bromide concentration: 0.1wt%;
[0138] Polishing liquid temperature: 25℃;
[0139] Polishing liquid nozzle pressure: 0.4 MPa;
[0140] Polishing disc speed: 25 m / min;
[0141] Chemical mechanical polishing time: 60 min;
[0142] Titanium cathode roller speed: 2 m / min;
[0143] Results: The surface roughness S of the titanium cathode roller treated by this embodiment a =0.225 μm, S q =0.303 μm, E R =8.7%, and the continuous stable production time is 58 days.
[0144] Example 5
[0145] The difference between this embodiment and embodiment 1 is that one of the grinding materials in step B and the components of the etchant in the polishing liquid are changed, the colloidal Al2O3 is replaced by colloidal Si3N4, and the lactic acid is replaced by EDTA-2Na of the same concentration.
[0146] Step B, chemical mechanical polishing of the titanium cathode roller;
[0147] Polishing disc material: short-pile Micro Met synthetic fiber;
[0148] The polishing liquid is composed of abrasive materials, etchants, pH regulators, and surfactants. The specific ingredients are as follows:
[0149] Colloidal SiO2: diameter 50 nm, concentration 4wt%; Colloidal Si3N4: diameter 200 nm, concentration 1wt%;
[0150] H2O2 concentration: 5wt%; EDTA-2Na concentration: 10wt%;
[0151] Glacial acetic acid concentration: 1wt%; ammonia concentration: 1wt%;
[0152] Tetramethylammonium hydroxide concentration: 1.5wt%; Ascorbic acid concentration: 1.5wt%;
[0153] Sodium dodecyl sulfate concentration: 0.1wt%
[0154] Polishing liquid temperature: 25℃;
[0155] Polishing fluid nozzle pressure: 0.4 MPa;
[0156] Polishing disc speed: 25 m / min;
[0157] Chemical mechanical polishing time: 60 min;
[0158] Titanium cathode roller speed: 2 m / min;
[0159] Results: The surface roughness S of the titanium cathode roller treated by this embodiment a =0.314 μm, S q =0.401 μm, E R =9.5%, and the continuous stable production time is 50 days.
[0160] Example 6
[0161] The difference between this embodiment and embodiment 1 is that the organic component of the pH adjuster in the polishing liquid of step B is changed: 1.5 wt% tetramethylammonium hydroxide-1.5 wt% ascorbic acid is replaced by tetraethylammonium hydroxide-salicylic acid of the same concentration.
[0162] Step B, chemical mechanical polishing of the titanium cathode roller;
[0163] Polishing disc material: short-pile Micro Met synthetic fiber;
[0164] The polishing liquid is composed of abrasive materials, etchants, pH regulators, and surfactants. The specific ingredients are as follows:
[0165] Colloidal SiO2: diameter 50 nm, concentration 4wt%; Colloidal Al2O3: diameter 200 nm, concentration 1wt%;
[0166] H2O2 concentration: 5wt%; citric acid concentration: 5wt%;
[0167] Glacial acetic acid concentration: 1wt%; ammonia concentration: 1wt%;
[0168] Tetraethylammonium hydroxide concentration: 1.5wt%; salicylic acid concentration: 1.5wt%;
[0169] Polyvinyl pyrrolidone concentration: 0.1wt%;
[0170] Polishing liquid temperature: 25℃;
[0171] Polishing fluid nozzle pressure: 0.5 MPa;
[0172] Polishing disc speed: 25 m / min;
[0173] Chemical mechanical polishing time: 60 min;
[0174] Titanium cathode roller speed: 2 m / min;
[0175] Results: The surface roughness S of the titanium cathode roller treated by this embodiment a =0.271 μm, S q =0.358 μm, E R =9.1%, and the continuous stable production time is 54 days.
[0176] Example 7
[0177] The difference between this embodiment and embodiment 1 is that the composition of the surfactant in the polishing liquid in step B is changed, and polyvinyl pyrrolidone (PVP) is replaced by sodium dodecylbenzene sulfonate (SDBS) of the same concentration.
[0178] Step B, chemical mechanical polishing of the titanium cathode roller;
[0179] Polishing disc material: short-pile Micro Met synthetic fiber;
[0180] The polishing liquid is composed of abrasive materials, etchants, pH regulators, and surfactants. The specific ingredients are as follows:
[0181] Colloidal SiO2: diameter 50 nm, concentration 5wt%; Colloidal Al2O3: diameter 200 nm, concentration 1wt%;
[0182] H2O2 concentration: 5wt%; Lactic acid concentration: 5wt%;
[0183] Glacial acetic acid concentration: 1wt%; ammonia concentration: 1wt%;
[0184] Tetramethylammonium hydroxide concentration: 1.5wt%; Ascorbic acid concentration: 1.5wt%;
[0185] Sodium dodecylbenzenesulfonate concentration: 0.1wt%;
[0186] Polishing liquid temperature: 25℃;
[0187] Polishing liquid nozzle pressure: 0.4 MPa;
[0188] Polishing disc speed: 25 m / min;
[0189] Chemical mechanical polishing time: 60 min;
[0190] Titanium cathode roller speed: 2 m / min;
[0191] Results: The surface roughness S of the titanium cathode roller treated by this embodiment a =0.257 μm, S q =0.339 μm, E R =8.9%, and the continuous stable production time is 56 days.
[0192] Example 8
[0193] The difference between this embodiment and embodiment 1 is that the time of chemical mechanical polishing in step B is changed.
[0194] Step B, chemical mechanical polishing of the titanium cathode roller;
[0195] Polishing disc material: short-pile Micro Met synthetic fiber;
[0196] The polishing liquid is composed of abrasive materials, etchants, pH regulators, and surfactants. The specific ingredients are as follows:
[0197] Colloidal SiO2: diameter 50 nm, concentration 5wt%; Colloidal Al2O3: diameter 200 nm, concentration 1wt%;
[0198] H2O2 concentration: 5wt%; Lactic acid concentration: 5wt%;
[0199] Glacial acetic acid concentration: 1wt%; ammonia concentration: 1wt%;
[0200] Tetramethylammonium hydroxide concentration: 1.5wt%; Ascorbic acid concentration: 1.5wt%;
[0201] Polyethylene glycol concentration: 0.1wt%;
[0202] Polishing liquid temperature: 25℃;
[0203] Polishing fluid nozzle pressure: 0.4 MPa;
[0204] Polishing disc speed: 25 m / min;
[0205] Chemical mechanical polishing time: 60 min;
[0206] Titanium cathode roller speed: 2 m / min;
[0207] Results: The surface roughness S of the titanium cathode roller treated by this embodiment a =0.406 μm, S q =0.482 μm, E R =10.3%, and the continuous stable production time is 50 days.
[0208] Comparative Example 1
[0209] The titanium cathode roller is mechanically polished using a conventional grinding wheel. The specific polishing process is as follows:
[0210] (1) Coarse grinding
[0211] Grinding wheel size: 120 mesh;
[0212] Grinding wheel speed: 20 m / min;
[0213] Grinding wheel lateral movement speed: 50 mm / min;
[0214] Cathode roller speed: 2 m / min;
[0215] Polishing time: 30 min;
[0216] (2) Fine grinding
[0217] Grinding wheel size: 300 mesh;
[0218] Grinding wheel speed: 20 m / min;
[0219] Grinding wheel lateral movement speed: 25 mm / min;
[0220] Cathode roller speed: 2 m / min;
[0221] Polishing time: 120 min;
[0222] (3) Washing-drying
[0223] After the mechanical polishing treatment, the titanium cathode roller surface is cleaned with deionized water, and then the residual moisture on the roller surface is removed under the blowing of compressed air.
[0224] Results: The surface roughness S of the titanium cathode roller treated by this embodimenta =0.324 μm, S q =0.541 μm, E R =13.5%, and the continuous stable production time is 45 days.
[0225] Comparative Example 2
[0226] The titanium cathode roller is mechanically polished using a conventional grinding wheel. The specific polishing process is as follows:
[0227] (1) Coarse grinding
[0228] Grinding wheel size: 120 mesh;
[0229] Grinding wheel speed: 20 m / min;
[0230] Grinding wheel lateral movement speed: 25 mm / min;
[0231] Cathode roller speed: 2 m / min;
[0232] Polishing time: 60 min;
[0233] (2) Fine grinding
[0234] Grinding wheel size: 300 mesh;
[0235] Grinding wheel speed: 20 m / min;
[0236] Grinding wheel lateral movement speed: 50 mm / min;
[0237] Cathode roller speed: 2 m / min;
[0238] Polishing time: 90 min;
[0239] (3) Washing-drying
[0240] After the mechanical polishing treatment, the titanium cathode roller surface is cleaned with deionized water, and then the residual moisture on the roller surface is removed under the blowing of compressed air.
[0241] Results: The surface roughness S of the titanium cathode roller treated by this embodiment a =0.283 μm, S q =0.484 μm, E R =12.7%, and the continuous stable production time is 40 days.
[0242] From the observations of Examples 1-8 and Comparative Examples 1-2, it can be clearly seen that:
[0243] 1. Introducing E R rationality.
[0244] Comparison of Example 8 and the comparative example shows that even when the chemical mechanical polishing time is only 30 min, S a =0.406 μm, the data is obviously inferior to the comparative example; S q =0.482 μm, the data is comparable to that of Comparative Example 2; but E R =10.3%, which is significantly lower than the two comparative examples. The direct difference in production brought about by this data is that the titanium cathode roller in Example 8 can be produced stably and continuously for 50 days; while the titanium cathode rollers in Comparative Examples 1 and 2 can be produced stably and continuously for 50 days respectively.
[0245] It can be seen that the roughness uniformity E R As another quantitative indicator of the polishing effect of titanium cathode rollers, it is feasible. Both production data and production cycle show that once the improvement of roller surface roughness uniformity is carried out simultaneously with the control of reducing roller surface roughness, it will have an unexpected technical effect on the polishing effect of titanium cathode rollers.
[0246] 2. Within the conventional polishing time, the Sa and Sq of the method of the present invention are significantly reduced.
[0247] Taking Example 1 and Comparative Example 1 as examples, Sa decreased by 16.4%, Sq decreased by 18%, and E R Reduced by 40%. Lower surface roughness and higher roughness uniformity not only help reduce the consumption of leveling agent, but also suppress tip discharge and improve the uniformity of copper foil.
[0248] 3. The continuous and stable production time is significantly extended.
[0249] Taking Example 1 and Comparative Example 1 as examples, the continuous stable production time was extended by 1 / 3, which significantly improved the production utilization rate of the titanium cathode roller.
[0250] In order to visually verify the effect, a microscopic image analysis was performed on the smooth surface of the first roll of electrolytic green foil after surface treatment. Since the smooth surface morphology of the electrolytic green foil is a mirror image of the roller surface state of the titanium cathode roller, the effect of the surface treatment can be compared by analyzing the smooth surface of the first roll of electrolytic green foil after surface treatment.
[0251] Figure 2 (a) shows a microscopic image of the polished surface of electrolytic green foil after being treated by the method of the present invention;
[0252] Figure 2(b) shows a microscopic image of the polished surface of electrolytic green foil after conventional mechanical polishing.
[0253] It can be clearly observed from the figure that the roller surface roughness and uniformity of the titanium cathode roller after the treatment of the present invention are significantly better than those after the traditional mechanical polishing treatment.
Claims
1. A surface treatment method for a titanium cathode roller, Features: The method is as follows: Step A, mechanical polishing pretreatment of the titanium cathode roller; Use a crane to hoist the titanium cathode roller that needs surface treatment to the grinder, set the rotation speed of the grinding wheel on the polishing disc, the cylinder pressure and the lateral movement speed, respectively start the rotating motors of the grinding wheel and the titanium cathode roller, and perform mechanical polishing pretreatment on the roller surface of the titanium cathode roller; Step B, chemical mechanical polishing of the titanium cathode roller; The mechanical grinding wheel is replaced with polishing discs symmetrically distributed on both sides of the horizontal diameter of the cathode roller, and the flow rate of the polishing liquid nozzle and the rotation speed of the cathode roller are set to start chemical mechanical polishing of the titanium cathode roller; The polishing liquid used in this step is composed of nano-abrasive material, etchant, pH adjuster, surfactant and deionized water; The nano-abrasive material in the polishing liquid is colloidal aluminum oxide (Al 2 O 3 ), colloidal silicon dioxide (SiO 2 ), silicon nitride (Si 3 N 4 ) or cerium oxide (CeO 2 ) one or more; the mass concentration of the nano-abrasive material in the polishing liquid is between 1wt%-4wt%; The etchant in the polishing liquid is two or more of lactic acid, chloroacetic acid, hydrogen peroxide, hydrofluoric acid, oxalic acid, citric acid, and ethylenediaminetetraacetic acid-2 sodium (EDTA-2Na); the mass concentration of the etchant in the polishing liquid is between 5wt% and 10wt%; The pH adjusting agent in the polishing liquid adjusts the pH value of the polishing liquid to between 3 and 5; The surfactant in the polishing liquid is one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, polyvinyl pyrrolidone, and polyethylene glycol; the mass concentration of the surfactant in the polishing liquid is between 0.01wt% and 0.1wt%; Step C, anodizing the polished titanium cathode roller; 1. Use deionized water to remove impurities remaining on the surface of the titanium cathode roller after chemical mechanical polishing; 2. Use compressed air to dry the residual moisture on the surface of the titanium cathode roller; 3. Using a metal titanium plate as the cathode, a polished titanium cathode roller as the anode, and a deionized water-ethylene glycol solution containing ammonium fluoride as the electrolyte, anodizing treatment is performed at a certain voltage to form a thin and dense protective layer on the roller surface of the titanium cathode roller.
2. A surface treatment method for a titanium cathode roller as claimed in claim 1, Features: The polishing liquid preparation process in step B is as follows: Add an appropriate amount of deionized water to the polishing liquid preparation tank, add surfactant, etchant, pH stabilizer and nano-abrasive material under mechanical stirring, continue stirring to make the components in the polishing liquid fully mixed, and then transport the polishing liquid to a polishing liquid storage tank with a stirring function, continue stirring for standby use.
3. A surface treatment method for a titanium cathode roller as claimed in claim 2, Features: The electrolyte solute used in the anodizing treatment in step C-3 includes ammonium fluoride, the solvent is deionized water-ethylene glycol, the voltage is between 35 V and 50 V, and the treatment time is between 3 minutes and 5 minutes.
4. A method for surface treatment of a titanium cathode roller as claimed in claim 2 or 3, Features: In the chemical mechanical polishing operation of step B, polishing discs are used to polish the titanium cathode roller. The polishing discs are symmetrically distributed on both sides of the titanium cathode roller. During the polishing process, the polishing discs are in direct contact with the titanium cathode roller. The polishing liquid is delivered to the nozzle just above the highest point of the titanium cathode roller and above the contact point between the titanium cathode roller and the polishing disc by a delivery pump. During the whole process, the polishing liquid passing through the polishing disc finally collects into the low-level tank along the roller surface of the titanium cathode roller. The lower roller surface of the titanium cathode roller is immersed in the polishing liquid in the low-level tank. The height of the titanium cathode roller immersed in the low-level tank is greater than 1 / 6 of the diameter of the cathode roller. During the process, the linear speeds of the titanium cathode roller and the polishing disc are different, and the linear speed of the polishing disc is greater than the linear speed of the titanium cathode roller.
5. A surface treatment method for a titanium cathode roller as claimed in claim 4, Features: The mesh number of the grinding wheel for mechanical polishing in step A is 120 mesh to 300 mesh.
6. A surface treatment method for a titanium cathode roller as claimed in claim 1, Features: The nano-abrasive material in the polishing liquid is spherical, and the diameter is between 20-200 nm.
7. A surface treatment method for a titanium cathode roller as claimed in claim 1, Features: The pH regulator in the polishing liquid is composed of an inorganic-organic composite component; The inorganic pH regulator is at least two or more of acetic acid, hydrochloric acid, nitric acid, ammonia water, and sodium hydroxide; The organic pH regulator is two or more of tetramethylammonium hydroxide, tetraethylammonium hydroxide, salicylic acid, and ascorbic acid; The mass concentration of the pH regulator in the polishing liquid is between 1wt% and 1.5wt%.
Citation Information
Patent Citations
Chemical mechanical polishing liquid for titanium
CN104593776A
Cathode roller polishing process for reducing 4.5 mu m copper foil defects