Ceramic electronic device and method for manufacturing the same

By adding Sn and Au to the internal electrode layer of ceramic electronic devices, the diffusion of nickel is suppressed, the reliability and life problems caused by oxygen vacancies during the firing process of ceramic electronic devices are solved, and their durability and life characteristics are significantly improved.

CN114446645BActive Publication Date: 2024-10-18TAIYO YUDEN KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202111185883.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-12
Publication Date
2024-10-18
Estimated Expiration
2041-10-12

AI Technical Summary

Technical Problem

During the firing process of ceramic electronic devices, when a reducing atmosphere is used to prevent nickel from oxidizing, oxygen vacancies are easily generated, resulting in a decrease in the reliability and life characteristics of ceramic electronic devices.

Method used

Sn and Au are added to the internal electrode layer to form a Ni-Sn-Au alloy to inhibit the diffusion of nickel into the dielectric layer and improve the life characteristics of ceramic electronic devices.

Benefits of technology

By inhibiting the diffusion of nickel, the durability and reliability of ceramic electronic devices are improved, their lifespan is extended, and their lifespan differences are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114446645B_ABST
    Figure CN114446645B_ABST
Patent Text Reader

Abstract

The present invention relates to a ceramic electronic device and a manufacturing method thereof. The ceramic electronic device comprises a stacked chip, wherein a plurality of dielectric layers whose main component is ceramic are stacked with a plurality of internal electrode layers. The plurality of internal electrode layers contain Ni, Sn and Au.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] A certain aspect of the present invention relates to a ceramic electronic device and a method for manufacturing the ceramic electronic device. Background Art

[0002] Ni (nickel) is used as an internal electrode layer of ceramic electronic devices such as stacked ceramic capacitors. The atmosphere of the firing process may be a reducing atmosphere to prevent Ni oxidation. However, when a reducing atmosphere is used during the firing process, oxygen vacancies are generated in the dielectric layer. As a result, the reliability of the ceramic electronic device is reduced. Therefore, a technology that can improve the reliability of ceramic electronic devices by adding Sn to an internal electrode made of Ni is disclosed (for example, see International Publication No. 2014 / 024538 and Japanese Patent Application Publication No. 2005-505695). Summary of the invention

[0003] However, when Ni is used for internal electrodes, the life characteristics of ceramic electronic devices have room for improvement.

[0004] According to one aspect of the present invention, there is provided a ceramic electronic device including: a stacked chip in which a plurality of dielectric layers whose main component is ceramic are stacked with a plurality of internal electrode layers, wherein the plurality of internal electrode layers contain Ni, Sn, and Au.

[0005] According to another aspect of the present invention, there is provided a method for manufacturing a ceramic electronic device, comprising: forming respective stacking units by forming respective internal electrode patterns on respective dielectric green sheets, the respective internal electrode patterns comprising Ni, Sn and Au; forming a stacking structure by stacking the respective stacking units; and firing the stacking structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] Figure 1 A perspective view showing a stacked ceramic capacitor, wherein a partial cross section of the stacked ceramic capacitor is shown;

[0007] Figure 2 Shown along Figure 1 A cross-sectional view taken along line AA;

[0008] Figure 3 Shown along Figure 1 A cross-sectional view taken along line BB;

[0009] Figure 4 Shows the effect of additives in the inner electrode layer on Ni diffusion;

[0010] Figure 5A shows the Sn concentration in the internal electrode layer;

[0011] Figure 5B shows the Au concentration in the internal electrode layer;

[0012] Figure 6 A method for manufacturing a laminated ceramic capacitor is shown;

[0013] Fig. 7A and Figure 7B The lamination process is shown;

[0014] Figure 8 showing a Weibull plot showing the relationship between the time before failure and the cumulative failure rate of the embodiment and the comparative example; and

[0015] 9A to 9C The Ni concentration in the dielectric layer is shown. DETAILED DESCRIPTION

[0016] The embodiments will be described with reference to the drawings.

[0017] (First Embodiment) Figure 1 A perspective view showing a stacked ceramic capacitor 100 according to an embodiment is shown, in which a partial cross section of the stacked ceramic capacitor 100 is shown. Figure 2 Shown along Figure 1 Cross-sectional view taken along line AA. Figure 3 Shown along Figure 1 The cross-sectional view taken along line BB. Figures 1 to 3 As shown, the laminated ceramic capacitor 100 includes: a laminated chip 10 having a rectangular parallelepiped shape; and a pair of external electrodes 20a and 20b respectively arranged on two end faces of the laminated chip 10 that are opposite to each other. Among the four faces other than the two end faces of the laminated chip 10, the two faces other than the upper and lower faces of the laminated chip 10 in the stacking direction are called side faces. The external electrodes 20a and 20b extend to the upper and lower faces and two side faces of the laminated chip 10. However, the external electrodes 20a and 20b are separated from each other. Figure 1 In the figure, the X-axis direction (first direction) is the length direction of the stacked chip 10. In the X-axis direction, the two end faces of the stacked chip 10 are opposite to each other. In addition, in the X-axis direction, the external electrode 20a is opposite to the external electrode 20b. The Y-axis direction (second direction) is the width direction of the internal electrode layer. The Z-axis direction is the stacking direction. The X-axis direction, the Y-axis direction, and the Z-axis direction are perpendicular to each other.

[0018] The laminated chip 10 has a structure designed to have dielectric layers 11 and internal electrode layers 12 that are alternately laminated. The dielectric layer 11 includes a ceramic material used as a dielectric material. The internal electrode layer 12 includes a base metal material. The end edges of the internal electrode layer 12 are alternately exposed to the first end face of the laminated chip 10 and the second end face of the laminated chip 10 that is different from the first end face. In the present embodiment, the first end face is opposite to the second end face. The external electrode 20a is provided on the first end face. The external electrode 20b is provided on the second end face. Therefore, the internal electrode layer 12 is alternately electrically connected to the external electrode 20a and the external electrode 20b. Therefore, the laminated ceramic capacitor 100 has a structure in which a plurality of dielectric layers 11 are laminated and each two dielectric layers 11 sandwich the internal electrode layer 12. In the laminated structure of the dielectric layer 11 and the internal electrode layer 12, the outermost layers in the lamination direction are two internal electrode layers 12. The upper and lower surfaces of the laminated structure as the internal electrode layer 12 are covered by the cover layer 13. The main component of the cover layer 13 is a ceramic material. For example, the main component of the cover layer 13 is the same as the main component of the dielectric layer 11.

[0019] For example, the stacked ceramic capacitor 100 may have a length of 0.25 mm, a width of 0.125 mm, and a height of 0.125 mm. The stacked ceramic capacitor 100 may have a length of 0.4 mm, a width of 0.2 mm, and a height of 0.2 mm. The stacked ceramic capacitor 100 may have a length of 0.6 mm, a width of 0.3 mm, and a height of 0.3 mm. The stacked ceramic capacitor 100 may have a length of 1.0 mm, a width of 0.5 mm, and a height of 0.5 mm. The stacked ceramic capacitor 100 may have a length of 3.2 mm, a width of 1.6 mm, and a height of 1.6 mm. The stacked ceramic capacitor 100 may have a length of 4.5 mm, a width of 3.2 mm, and a height of 2.5 mm. However, the size of the stacked ceramic capacitor 100 is not limited.

[0020] The dielectric layer 11 is mainly composed of a ceramic material represented by the general formula ABO3 and having a perovskite structure. The perovskite structure includes ABO3 having a non-stoichiometric composition. 3-α For example, such ceramic materials include BaTiO3 (barium titanate), CaZrO3 (calcium zirconate), CaTiO3 (calcium titanate), SrTiO3 (strontium titanate), Ba with a perovskite structure, and 1-x-y Ca x Sr y Ti 1-z Zr zO3 (0≤x≤1, 0≤y≤1, 0≤z≤1). The average thickness of each dielectric layer 11 may be, for example, 0.05 μm or more and 5 μm or less. The average thickness may be 0.1 μm or more and 3 μm or less. The average thickness may be 0.2 μm or more and 1 μm or less.

[0021] like Figure 2 As shown in FIG. 1 , a region where one group of internal electrode layers 12 connected to the external electrode 20 a faces another group of internal electrode layers 12 connected to the external electrode 20 b is a region where capacitance is generated in the multilayer ceramic capacitor 100. Therefore, this region is referred to as a capacitance region 14. That is, the capacitance region 14 is a region where mutually adjacent internal electrode layers connected to different external electrodes face each other.

[0022] The region where the internal electrode layers 12 connected to the external electrode 20a are opposed to each other without sandwiching the internal electrode layer 12 connected to the external electrode 20b is referred to as an edge 15. The region where the internal electrode layers 12 connected to the external electrode 20b are opposed to each other without sandwiching the internal electrode layer 12 connected to the external electrode 20a is another edge 15. That is, the edge 15 is a region where a group of internal electrode layers 12 connected to one external electrode are opposed to each other without sandwiching the internal electrode layer 12 connected to the other external electrode. The edge 15 is a region where no capacitance is generated in the multilayer ceramic capacitor 100.

[0023] like Figure 3 As shown, the area of ​​the laminated chip 10 from both sides thereof to the internal electrode layer 12 is called the side edge 16. That is, the side edge 16 is an area covering the edge of the laminated internal electrode layer 12 in the direction extending toward both side surfaces. The side edge 16 does not generate capacitance.

[0024] When Ni is used for the internal electrode layer 12 in the laminated ceramic capacitor 100, the reliability of the dielectric layer 11 may be reduced due to the generation of oxygen vacancies in the dielectric layer 11. For example, when the atmosphere during firing is reducing to suppress oxidation of Ni, oxygen vacancies may be easily generated in the dielectric layer 11. When the thickness of the dielectric layer 11 containing vacancies is reduced and a voltage with a high field strength is applied to the dielectric layer 11, the durability of the dielectric layer 11 may be insufficient. In this case, the life of the laminated ceramic capacitor 100 may be short. Or, there is a difference in the life. That is, the life characteristics may be deteriorated. Therefore, the laminated ceramic capacitor 100 has a structure for improving the life characteristics.

[0025] In addition to Ni, the internal electrode layer 12 also includes Sn. When the internal electrode layer 12 includes Ni and Sn, the life of the laminated ceramic capacitor 100 can be improved. For example, when Ni and Sn form an alloy, the interface state between the internal electrode layer 12 and the dielectric layer 11 changes. In this case, it is considered that the life of the laminated ceramic capacitor 100 can be improved.

[0026] Next, when Ni in the internal electrode layer 12 diffuses into the dielectric layer 11, a sufficient life of the multilayer ceramic capacitor 100 may not be achieved. The mechanism is not clear. Therefore, it is advantageous to suppress the diffusion of Ni from the internal electrode layer 12 to the dielectric layer 11. Therefore, the present inventors studied the effect of additives added to the internal electrode layer 12 on the diffusion of Ni.

[0027] Four samples were prepared. A sample in which an internal electrode pattern (thickness of 200 nm) made of Ni was formed on a dielectric green sheet whose main component was barium titanate by sputtering was prepared as a first sample. A sample in which 3.3 μg of Ni paste was printed on a dielectric green sheet whose main component was barium titanate was prepared as a second sample. A sample in which an internal electrode pattern (Sn concentration of 3.2 at%, thickness of 200 nm) was formed on a dielectric green sheet whose main component was barium titanate by sputtering was prepared as a third sample. A sample in which an internal electrode pattern (Au concentration of 1.0 at%, thickness of 200 nm) was formed on a dielectric green sheet whose main component was barium titanate by sputtering was prepared as a fourth sample.

[0028] Each sample was heated at an oxygen partial pressure of 10 -5 atm to 10 -8 The samples were fired at 1100°C to 1300°C in a reducing atmosphere of 200 atm. The Ni concentration in the dielectric layer was measured using La-ICP (Laser Ablation Inductively Coupled Plasma Mass Spectrometry). The relationship between the distance from the internal electrode layer and the Ni concentration ratio (Ni / Ti) at% was measured.

[0029] Figure 4 The results are shown. Figure 4 As shown in the figure, in the first, second and third samples, the Ni concentration becomes higher in places far from the internal electrode layer. It is believed that this is because Ni diffuses during the firing process. On the other hand, in the fourth sample, the Ni concentration becomes lower in places far from the internal electrode layer. It is believed that this is because the diffusion of Ni is suppressed during the firing process. According to this result, it is confirmed that the diffusion of Ni into the dielectric layer is suppressed by adding Au to the internal electrode layer.

[0030] Therefore, the internal electrode layer 12 includes Sn and Au in addition to Ni. When the internal electrode layer 12 includes Au, Au acts as a barrier to prevent the diffusion of Ni. The diffusion of Ni into the dielectric layer 11 is further suppressed. Therefore, the durability of the dielectric layer 11 to an applied voltage with a high field strength is improved. Therefore, the life of the stacked ceramic capacitor 100 is improved. When the life is improved, capacitors with a short life are no longer included. Therefore, the life difference is suppressed. Therefore, the life characteristics of the stacked ceramic capacitor 100 are improved.

[0031] The thickness of each internal electrode layer 12 may be, for example, 0.01 μm to 5 μm. The thickness of each internal electrode layer 12 may be 0.05 μm to 3 μm. The thickness of each internal electrode layer 12 may be 0.1 μm to 1 μm.

[0032] When the amount of Sn in the internal electrode layer 12 is small, it may be difficult to control the interface state between the internal electrode layer 12 and the dielectric layer 11. When the amount of Au is small, it may be difficult to sufficiently suppress the diffusion of Ni. Therefore, the total amount of Sn and Au preferably has a lower limit. For example, in the internal electrode layer 12, the ratio of the total amount of Sn and Au to the amount of Ni is preferably 0.01at% or more. More preferably, the ratio is 0.05at% or more. More preferably, the ratio is 0.1at% or more. Even more preferably, the ratio is 0.2at% or more.

[0033] On the other hand, when the total amount of Sn and Au is large, the melting point of the internal electrode layer 12 may decrease or the cost may increase. Therefore, the total amount of Sn and Au preferably has an upper limit. For example, in the internal electrode layer 12, the ratio of the total amount of Sn and Au relative to the amount of Ni is preferably 95at% or less. The ratio is more preferably 50at% or less. It is even more preferable that the ratio is 10at% or less.

[0034] When the ratio of the total amount of Sn and Au to the amount of Ni is 0.2 at% or more and 10 at% or less, even if the amount of Au is less than the amount of Sn, the interface state between the internal electrode layer 12 and the dielectric layer 11 can be controlled and the diffusion of Ni can be suppressed. Therefore, when the ratio of the total amount of Sn and Au to the amount of Ni is 0.2 at% or more and 10 at% or less, from the viewpoint of reducing the amount of Au and reducing costs, it is preferred that the amount of Au is smaller than the amount of Sn.

[0035] It is preferable that the Sn concentration near the interface between the internal electrode layer 12 and the dielectric layer 11 is high. This is because the internal electrode layer as a whole does not have a great influence on the reliability, but only the interface between the dielectric layer 11 and the internal electrode layer 12 has a great influence on the reliability. Figure 5AAs shown in FIG. 1 , the internal electrode layer 12 preferably has a concentration gradient in which the Sn concentration is low in the center portion in the thickness direction of the internal electrode layer 12 and high in the vicinity of the interface between the internal electrode layer 12 and the dielectric layer 11. Figure 5B As shown, it is preferred that the Au concentration in the internal electrode layer 12 is high near the interface between the internal electrode layer 12 and the dielectric layer 11. This is because diffusion of Ni into the dielectric layer 11 is effectively suppressed. Therefore, the internal electrode layer 12 preferably has a concentration gradient in which the Au concentration is low in the central portion in the stacking direction of the internal electrode layer 12 and the Au concentration is high near the interface between the dielectric layer 11 and the internal electrode layer 12.

[0036] Next, a method for manufacturing the multilayer ceramic capacitor 100 will be described. Figure 6 A method for manufacturing the multilayer ceramic capacitor 100 is shown.

[0037] (Process for producing raw material powder) A dielectric material for forming the dielectric layer 11 is prepared. The dielectric material includes a ceramic which is a main component of the dielectric layer 11. The A-site element and the B-site element are usually contained in the dielectric layer 11 in the form of a sintered phase of ABO3 particles. For example, BaTiO3 is a tetragonal compound having a perovskite structure and a high dielectric constant. BaTiO3 can usually be obtained by reacting a titanium material such as titanium dioxide with a barium material such as barium carbonate and synthesizing barium titanate. Various methods can be used as a method for synthesizing the ceramic constituting the dielectric layer 11. For example, a solid phase method, a sol-gel method, a hydrothermal method, etc. are known. Any of the above methods can be used in this embodiment.

[0038] An additive compound may be added to the obtained ceramic powder according to the purpose. The additive compound may be an oxide of Mg (magnesium), Mn (manganese), V (vanadium), Cr (chromium) or a rare earth element (Y (yttrium), Sm (samarium), Eu (europium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium) and Yb (ytterbium)), or an oxide of Co (cobalt), Ni, Li (lithium), B (boron), Na (sodium), K (potassium) and Si (silicon). The additive compound may be a glass including cobalt, nickel, lithium, boron, sodium, potassium or silicon.

[0039] For example, the obtained ceramic raw material powder is wet mixed with an additive and dried and crushed. Thus, a ceramic material is obtained. For example, the particle size can be adjusted by crushing the obtained ceramic material as needed. Alternatively, the particle size of the obtained ceramic powder can be adjusted by combining crushing and classification. Through this process, a dielectric material is obtained.

[0040] (Lamination process) Next, a binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer are added to the obtained dielectric material and wet mixed. Using the obtained slurry, a dielectric green sheet 52 having a thickness of 0.5 μm or more and 1.0 μm or less is applied to a substrate 51 by, for example, a die coater method or a doctor blade method, and then dried. The substrate 51 is, for example, a PET (polyethylene terephthalate) film.

[0041] Next, if Fig. 7A As shown in FIG. 5 , an internal electrode pattern 53 is formed on a dielectric green sheet 52. Fig. 7A In the embodiment, as an example, four internal electrode patterns 53 are formed on the dielectric green sheet 52 and are spaced apart from each other. The formation method is not limited. For example, an electrode paste including a mixture of Ni, Sn and Au can be used. A Ni metal powder paste including Au and Sn can be used. A vacuum deposition method such as a sputtering method using an alloy target can be performed. Simultaneous sputtering using separate targets can be performed. The dielectric green sheet 52 on which the internal electrode pattern 53 is formed is a stacked unit.

[0042] Next, the dielectric green sheet 52 is peeled off from the substrate 51. Figure 7B , the stacking units are stacked.

[0043] A predetermined number (e.g., 2 to 10) of cover sheets are stacked on both upper and lower surfaces of the ceramic laminate structure of the stacked laminate unit and thermally clamped. The resulting ceramic laminate structure is cut into chips having a predetermined size (e.g., 1.0 mm×0.5 mm). Figure 7B The laminated structure is cut along the dotted line in FIG. 5 . The composition of the cover sheet may be the same as that of the dielectric green sheet 52. The additives of the cover sheet may be different from those of the dielectric green sheet 52.

[0044] (Firing process) The binder is removed from the ceramic laminate structure in an N2 atmosphere. A metal paste as a base layer of the external electrodes 20a and 20b is applied to the ceramic laminate structure by an immersion method. The obtained ceramic laminate structure is heated to 10°C in an oxygen partial pressure of 10°C. -5 atm to 10 -8 The ceramic capacitor 100 is fired in a reducing atmosphere of 100° C. to 1300° C. for 10 minutes to 2 hours.

[0045] (Reoxidation Process) After that, a reoxidation process may be performed in a N2 gas atmosphere at a temperature range of 600°C to 1000°C.

[0046] (Plating Step) After that, a metal layer such as Cu, Ni, Sn, etc. is plated on the external electrodes 20a and 20b by a plating method.

[0047] In the manufacturing method of the present embodiment, the internal electrode layer 12 includes Sn and Au in addition to Ni. Therefore, the life of the laminated ceramic capacitor is improved. When the life is improved, capacitors with short life are no longer included. In this case, the difference in life becomes smaller. Therefore, the life characteristics of the laminated ceramic capacitor 100 are improved.

[0048] In the embodiments, a laminated ceramic capacitor is described as an example of a ceramic electronic device. However, the embodiments are not limited to the laminated ceramic capacitor. For example, the embodiments may be applied to other electronic devices such as a varistor or a thermistor.

[0049] Example

[0050] The multilayer ceramic capacitor according to the embodiment was manufactured and its characteristics were measured.

[0051] (Example 1) Additives were added to barium titanate powder. The additives and barium titanate powder were fully wet mixed and crushed in a ball mill. Thus, a dielectric material was prepared. A butyral-based material used as an organic binder and toluene and ethanol used as solvents were added to the dielectric material. And, a dielectric green sheet was prepared on a PET substrate by a doctor blade method. The thickness of the dielectric green sheet was 1.0 μm.

[0052] Next, an internal electrode pattern was formed on the dielectric green sheet using a paste containing a Ni-Sn-Au alloy. The atomic concentration ratio of Ni / Sn / Au was 96 / 2 / 2.

[0053] Next, the dielectric green sheet is peeled off from the substrate. Multiple stacking units are stacked. The temperature of the stacking process is 80°C. The resulting ceramic stacking structure is pressed at 4MPa. The pressing time is 5 seconds. Next, a predetermined number of cover sheets are stacked on the upper and lower surfaces of the ceramic stacking structure of the stacked stacking units and hot clamped by fluid static pressure. The pressure of the fluid static pressure is 120MPa. The pressing temperature is 100°C. The pressing time is 25 seconds. Afterwards, the resulting ceramic stacking structure is cut into chips with predetermined dimensions (1.0mm×0.5mm×0.5mm).

[0054] The binder is removed from the ceramic laminate structure in an N2 atmosphere. A metal paste as a base layer of an external electrode is applied to the ceramic laminate structure by an impregnation method. The ceramic laminate structure is fired in a reducing atmosphere.

[0055] (Example 2) The atomic concentration ratio of Ni / Sn / Au is 99.6 / 0.2 / 0.2. Other conditions are the same as those in Example 1.

[0056] (Example 3) The atomic concentration ratio of Ni / Sn / Au is 80 / 10 / 10. Other conditions are the same as those in Example 1.

[0057] (Comparative Example 1) Neither Sn nor Au was added to the internal electrode layer. Other conditions were the same as in Example 1.

[0058] (Comparative Example 2) The Au concentration in the internal electrode layer is the same as that in Example 1. However, Sn is not added to the internal electrode layer. Other conditions are the same as those in Example 1.

[0059] (Comparative Example 3) The Sn concentration in the internal electrode layer is the same as that in Example 1. However, Au is not added to the internal electrode layer. Other conditions are the same as those in Example 1.

[0060] (Life Test) The time until failure occurred was measured for each sample of Examples 1 to 3 and Comparative Examples 1 to 3. In the test, the time until the leakage current under a DC electric field of 18 V / μm at 150° C. became 10 times the minimum leakage current was measured.

[0061] Figure 8 A Weibull plot is shown, which shows the relationship between the time to failure occurrence and the cumulative failure rate in Examples 1 to 3 and the Comparative Example. Table 1 shows Figure 8 Table 1 shows the time at which 50% of the number of samples fail for each of Examples 1 to 3 and Comparative Example.

[0062] Table 1

[0063]

[0064] like Figure 8 As shown in Table 1, in Comparative Example 1, the slope of the Weibull plot is small. The number of samples with short lifespan is large. The lifespan difference between the samples is large. It is believed that this is because the internal electrode layer contains neither Sn nor Au. In Comparative Example 2, the lifespan is longer than that of Comparative Example 1. However, a sufficient lifespan is not achieved. It is believed that this is because Sn is added to the Ni of the internal electrode layer but Au is not added to the Ni of the internal electrode layer, so the diffusion of Ni is not sufficiently suppressed. In Comparative Example 3, the lifespan is longer than that of Comparative Example 1. However, a sufficient lifespan is not achieved. It is believed that this is because Au is added to the Ni of the internal electrode layer but Sn is not added to the Ni of the internal electrode layer, so the interface between the internal electrode layer and the dielectric layer cannot be fully controlled.

[0065] In contrast, the samples of Examples 1 to 3 each have a long lifespan. The slope of the Weibull plot is large. The difference in lifespan is small. This is considered to be due to the addition of Sn and Au to Ni of the internal electrode layer.

[0066] For Example 1 and Comparative Examples 2 and 3, the Ni concentration of the dielectric layer was measured using La-ICP. Fig. 9A The results of Comparative Example 3 are shown. Fig. 9B The results of Comparative Example 2 are shown. Fig. 9CThe results of Example 1 are shown. Fig. 9A As shown in FIG. 1 , when Au is not added to the internal electrode layer, a large amount of Ni diffuses into the dielectric layer. Fig. 9B As shown in FIG. 1 , when Au is added to the internal electrode layer instead of Sn, the amount of Ni diffused into the dielectric layer is small. Fig. 9C As shown, when both Sn and Au are added to the inner electrode layer, the amount of Ni diffused into the dielectric layer is smaller. It is believed that these results contribute to the results of Table 1.

[0067] Although the embodiments of the present invention have been described in detail, it should be understood that the various changes, substitutions, and alterations could be made hereto without departing from the spirit and scope of the invention.

Claims

1. A ceramic electronic device comprising: A laminated chip in which a plurality of dielectric layers whose main component is ceramic are laminated with a plurality of internal electrode layers. wherein the plurality of internal electrode layers comprise Ni, Sn and Au, In an interface portion where the dielectric layer contacts the adjacent internal electrode layer, a Sn concentration is higher than an Au concentration. 2 . The ceramic electronic device according to claim 1 , wherein the total amount of Ni, Sn and Au in the plurality of internal electrode layers is 0.01 at % or more and 95 at % or less. 3 . The ceramic electronic device according to claim 2 , wherein the total amount of Ni, Sn and Au in the plurality of internal electrode layers is 0.2 at % or more and 10 at % or less. 4 . The ceramic electronic device according to claim 1 , wherein an amount of Au is smaller than an amount of Sn in the plurality of internal electrode layers. 5 . The ceramic electronic device according to claim 1 , wherein a Sn concentration near each interface between the plurality of internal electrode layers and the plurality of dielectric layers is greater than a Sn concentration at each central portion in a thickness direction of the plurality of internal electrode layers. 6 . The ceramic electronic device according to claim 1 , wherein the Au concentration near each interface between the plurality of internal electrode layers and the plurality of dielectric layers is greater than the Au concentration in each center portion in a thickness direction of the plurality of internal electrode layers.

7. A method for manufacturing a ceramic electronic device, comprising the following steps: forming each stacked unit by forming each internal electrode pattern on each dielectric green sheet, the each internal electrode pattern comprising Ni, Sn and Au; forming a stacked structure by stacking the respective stacking units; and The stacked structure is fired so that the Sn concentration is higher than the Au concentration in an interface portion where a dielectric layer is in contact with an adjacent internal electrode layer formed of a dielectric green sheet and the internal electrode layer is formed of an internal electrode pattern.

8. The manufacturing method according to claim 7, wherein when forming each stacked unit, each of the internal electrode patterns is formed on each of the dielectric green sheets by a vacuum deposition process.

Citation Information

Patent Citations

  • Powder for use inside multilayer ceramic capacitor electrodes

    JP2005505695A

  • Powder for laminated ceramic capacitor internal electrode

    US20040256603A1