Rubber composition and tire
The tire was solved by using a combination of a high weight average molecular weight and high hydrogenation hydrogenated diene polymer with a low weight average molecular weight and medium hydrogenation hydrogenated diene polymer with a high softening point resin in tire rubber The problems of rubber hardening and plasticizer escape have achieved more stable durability and fuel economy.
Patent Information
- Application Number
- CN202080068233.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-23
- Filing Date
- 2020-09-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-09-24
AI Technical Summary
The existing tire rubber hardens due to re-crosslinking during use, and plasticizers are prone to escape, resulting in unstable tire performance, especially the wet grip performance and durability performance.
The combination of hydrogenated conjugated diene polymer (A) with a high weight average molecular weight and a high hydrogenation degree and a hydrogenated conjugated diene polymer (B) with a low weight average molecular weight and a medium hydrogenation degree is used to combine resins with a softening point of 20°C or above , form a rubber composition, optimize the durability and fuel economy of the rubber.
The durability and wet grip properties of the rubber composition are significantly improved, and the hardness varies over time reduces the efficiency of the hardness, providing excellent fuel economy and stable tire performance.
Smart Images

Figure BDA0003570128880000191
Abstract
Description
Technical Field
[0001] The present invention relates to a rubber composition and a tire. Background Art
[0002] Typically, tire rubber containing a large number of double bonds tends to harden over time due to re-crosslinking. In addition, the plasticizer contained in the tire rubber is usually low in molecular weight and tends to escape from the rubber. The escape of the plasticizer accelerates the hardening of the rubber. The hardening of the rubber then leads to changes in tire performance (e.g., wet grip performance). Therefore, the tire rubber may not provide stable tire performance, and there is room for improvement in this regard.
[0003] Patent Document 1 discloses a technology for using a rubber (hydrogenated copolymer) that has been hydrogenated to reduce the number of double bonds in a tire. This technology can reduce the change in hardness over time to a certain extent. However, in recent years, as the life of tires has been extended, people expect to further improve the durability of tires.
[0004] Reference List
[0005] Patent Literature
[0006] Patent Document 1: WO 2016 / 039005 Summary of the invention
[0007] Technical issues
[0008] The present invention aims to solve the above-mentioned problems and provide a rubber composition and a tire having excellent durability performance as well as good fuel economy and wet grip performance.
[0009] Solutions to the problem
[0010] The present invention relates to a rubber composition, comprising: at least one hydrogenated conjugated diene polymer (A), the hydrogenated conjugated diene polymer (A) having a weight average molecular weight of 100,000 or more and a degree of hydrogenation of 75 mol% or more; at least one hydrogenated conjugated diene polymer (B), the hydrogenated conjugated diene polymer (B) having a weight average molecular weight of less than 100,000; and at least one resin, the softening point of the resin being 20° C. or more.
[0011] Preferably, the absolute value of the difference in degree of hydrogenation between the hydrogenated conjugated diene polymer (A) and the hydrogenated conjugated diene polymer (B) is 90 mol% or less.
[0012] Preferably, the degree of hydrogenation of the hydrogenated conjugated diene polymer (B) is 25 mol% or more.
[0013] Preferably, the hydrogenated conjugated diene polymer (B) is present in an amount of 5 parts by mass or more relative to 100 parts by mass of the rubber component in the rubber composition.
[0014] Preferably, the total amount of the hydrogenated conjugated diene polymer (B) and the resin is 40 parts by mass or less relative to 100 parts by mass of the rubber component in the rubber composition.
[0015] Preferably, the change in hardness of the rubber composition after immersion in acetone for 24 hours is 20% or less relative to the hardness before immersion.
[0016] Preferably, the mass of the rubber composition after being immersed in acetone for 24 hours is at least 80% of the mass before the immersion.
[0017] Preferably, the rubber composition comprises at least one filler selected from carbon black and silica.
[0018] Preferably, the resin is at least one selected from coumarone-indene resin, styrene resin and terpene resin.
[0019] Preferably, the hydrogenated conjugated diene polymer (A) has a weight average molecular weight of 200,000 to 1,000,000 and a hydrogenation degree of 90 to 98 mol %, and the hydrogenated conjugated diene polymer (B) has a weight average molecular weight of 1,000 to 6,000 and a hydrogenation degree of 40 to 98 mol %.
[0020] Preferably, the hydrogenated conjugated diene polymer (A) and the hydrogenated conjugated diene polymer (B) are each a copolymer of a conjugated diene compound and an aromatic vinyl compound; the hydrogenated conjugated diene polymer (A) contains 10% to 50% by mass of structural units derived from at least one aromatic vinyl compound; and the hydrogenated conjugated diene polymer (B) contains 10% to 50% by mass of structural units derived from at least one aromatic vinyl compound.
[0021] Preferably, the hydrogenated conjugated diene polymer (A) is present in an amount of 80% by mass or more based on 100% by mass of the rubber component in the rubber composition.
[0022] Preferably, the softening point of the resin is 30°C to 130°C.
[0023] Preferably, the rubber composition contains 1 to 25 parts by mass of the resin, 1 to 30 parts by mass of carbon black, and 20 to 100 parts by mass of silica, relative to 100 parts by mass of the rubber component in the rubber composition.
[0024] The present invention also relates to a tire having a tire component, wherein the tire component includes the rubber composition.
[0025] Beneficial effects of the invention
[0026] The present invention relates to a rubber composition, comprising a hydrogenated conjugated diene polymer (A) having a weight average molecular weight of 100,000 or more and a degree of hydrogenation of 75 mol% or more, a hydrogenated conjugated diene polymer (B) having a weight average molecular weight of less than 100,000, and a resin having a softening point of 20° C. or more. Therefore, the rubber composition can provide excellent durability, fuel economy, and wet grip performance. DETAILED DESCRIPTION
[0027] The present invention relates to a rubber composition, comprising a hydrogenated conjugated diene polymer (A), a hydrogenated conjugated diene polymer (B), and a resin, wherein the hydrogenated conjugated diene polymer (A) has a weight average molecular weight of 100,000 or more and a degree of hydrogenation of 75 mol % or more, the hydrogenated conjugated diene polymer (B) has a weight average molecular weight of less than 100,000, and the resin has a softening point of 20° C. or more.
[0028] The rubber composition combines a hydrogenated conjugated diene polymer (A), a hydrogenated conjugated diene polymer (B) and a resin to provide excellent durability, fuel economy and wet grip performance.
[0029] The hydrogenated conjugated diene polymer (A) has a small number of double bonds and thus has an advantage that the hardness does not easily change over time. However, the hydrogenated conjugated diene polymer (A) has a lower polarity than the diene rubber generally used in tire rubber compositions and therefore has poor compatibility with conventional plasticizers (e.g., liquid rubber) and tends to bleed out.
[0030] In contrast, the hydrogenated conjugated diene polymer (B) used in the rubber composition has high compatibility with the hydrogenated conjugated diene polymer (A) and is less likely to bleed out. In addition, the presence of a resin having a softening point of 20° C. or higher can further suppress bleed out. It is believed that these effects provide excellent durability performance.
[0031] In addition, the combined use of the hydrogenated conjugated diene polymer (A) and the hydrogenated conjugated diene polymer (B) provides a sharp temperature dependence of tan δ, resulting in good overall performance in terms of fuel economy and wet grip performance. In addition, the presence of a resin having a softening point of 20° C. or more allows the Tg of the rubber composition to be within the temperature range under tire use conditions. It is believed that these effects provide excellent fuel economy and wet grip performance.
[0032] The rubber composition comprises at least one hydrogenated conjugated diene polymer (A) having a weight average molecular weight of 100,000 or more and a degree of hydrogenation of 75 mol % or more and at least one hydrogenated conjugated diene polymer (B) having a weight average molecular weight of less than 100,000.
[0033] A high molecular weight hydrogenated conjugated diene polymer (A) is used as a rubber component. On the other hand, a low molecular weight hydrogenated conjugated diene polymer (B) is used as a plasticizer. The hydrogenated conjugated diene polymer (B) is not contained in the rubber component.
[0034] Hydrogenated conjugated diene polymer (A) and (B) can be obtained by hydrogenating a polymer having a structural unit (conjugated diene unit) derived from at least one conjugated diene compound. Examples of hydrogenated polymers include: a homopolymer of a conjugated diene compound, a copolymer of two or more conjugated diene compounds, and a copolymer of a conjugated diene compound and other monomers (e.g., an aromatic vinyl compound). These can be used alone or in combination of two or more. Among these, a copolymer of a conjugated diene compound and an aromatic vinyl compound is preferred.
[0035] Examples of conjugated diene compounds include 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethylbutadiene, 2-phenyl-1,3-butadiene and 1,3-hexadiene. These can be used alone or in combination of two or more. 1,3-butadiene and isoprene are preferred, and 1,3-butadiene is more preferred.
[0036] Examples of aromatic vinyl compounds include styrene, α-methylstyrene, 1-vinylnaphthalene, 3-vinyltoluene, ethylvinylbenzene, divinylbenzene, 4-cyclohexylstyrene and 2,4,6-trimethylstyrene. These can be used alone or in combination of two or more. Styrene and α-methylstyrene are preferred, and styrene is more preferred.
[0037] In other words, the hydrogenated conjugated diene polymers (A) and (B) are each preferably a hydrogenated styrene-butadiene copolymer (hydrogenated SBR).
[0038] Hydrogenated conjugated diene polymers (A) and (B) can be prepared by any polymerization method, including random polymerization and block polymerization, preferably random polymerization. Hydrogenation can also be carried out by any method under any reaction conditions (including known methods and known conditions). Typically, hydrogenation is carried out at an elevated hydrogen pressure of 0.1 MPa to 10 MPa and 20° C. to 150° C. in the presence of a hydrogenation catalyst. Other methods and conditions related to production are also not limited, for example, those described in WO2016 / 039005 above can be used.
[0039] Although it is sufficient that the weight average molecular weight (Mw) of the hydrogenated conjugated diene polymer (A) is 100,000 or more, it is preferably 120,000 or more, more preferably 200,000 or more, further preferably 300,000 or more, but is preferably 1,000,000 or less, more preferably 600,000 or less, further more preferably 400,000 or less. When Mw is within the above range, the beneficial effects tend to be better achieved.
[0040] The weight average molecular weight (Mw) can be measured by a gel permeation chromatograph (GPC) calibrated with a polystyrene standard (GPC-8000 series available from Tosoh Corporation, detector: differential refractometer, chromatographic column: TSKGELSUPERMULTIPORE HZ-M available from Tosoh Corporation). In addition, for a polymer having a modified group, the Mw of the polymer cannot be accurately determined due to the interaction between the modified group and the silica gel in the column, so the Mw is measured before the polymer is modified.
[0041] Although it is sufficient that the degree of hydrogenation of the hydrogenated conjugated diene polymer (A) is 75 mol% or more, the degree of hydrogenation is preferably 80 mol% or more, more preferably 90 mol% or more, but preferably 98 mol% or less, more preferably 95 mol% or less, based on the total amount of conjugated diene units before hydrogenation as 100 mol%. When the degree of hydrogenation is within the above range, a beneficial effect tends to be achieved better.
[0042] The degree of hydrogenation can be measured by 1 Calculation of the reduction rate of unsaturated bond signals in H-NMR spectra.
[0043] When the hydrogenated conjugated diene polymer (A) is a copolymer of a conjugated diene compound and an aromatic vinyl compound, the amount of the structural unit (aromatic vinyl unit) derived from at least one aromatic vinyl compound is preferably 10% by mass or more, more preferably 15% by mass or more, further preferably 20% by mass or more, but preferably 50% by mass or less, more preferably 45% by mass or less, further preferably 40% by mass or less, particularly preferably 33% by mass or less. When the amount is within the above range, a beneficial effect tends to be achieved better.
[0044] The amount of at least one hydrogenated conjugated diene polymer (A) is preferably 80% by mass or more, more preferably 90% by mass or more, further more preferably 95% by mass or more, based on 100% by mass of the rubber component, and may be 100% by mass. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0045] Although it is sufficient that the weight average molecular weight (Mw) of the hydrogenated conjugated diene polymer (B) is preferably less than 100,000, it is preferably 80,000 or less, more preferably 10,000 or less, further preferably 6,000 or less, particularly preferably 4,500 or less, but preferably 1,000 or more, more preferably 2,000 or more. When Mw is within the above range, the beneficial effects tend to be better achieved.
[0046] The degree of hydrogenation of the hydrogenated conjugated diene polymer (B) is preferably 25 mol% or more, more preferably 40 mol% or more, and further preferably 50 mol% or more, but preferably 98 mol% or less, and more preferably 95 mol% or less, based on the total amount of conjugated diene units before hydrogenation as 100 mol%. When the degree of hydrogenation is within the above range, the compatibility between the hydrogenated copolymer (A) and the hydrogenated copolymer (B) is better, thereby tending to further suppress exudation.
[0047] The absolute value of the difference in degree of hydrogenation between the hydrogenated conjugated diene polymer (A) and the hydrogenated conjugated diene polymer (B) is preferably 90 mol% or less, more preferably 60 mol% or less, further preferably 45 mol% or less, particularly preferably 15 mol% or less, and may be 0 mol% (the degree of hydrogenation is substantially the same). When the absolute value is within the above range, the compatibility between the hydrogenated copolymer (A) and the hydrogenated copolymer (B) is better, thereby tending to further suppress bleeding.
[0048] When the hydrogenated conjugated diene polymer (B) is a copolymer of a conjugated diene compound and an aromatic vinyl compound, the amount of the structural unit (aromatic vinyl unit) derived from at least one aromatic vinyl compound is preferably 10% by mass or more, more preferably 15% by mass or more, further preferably 20% by mass or more, particularly preferably 25% by mass or more, but preferably 50% by mass or less, more preferably 45% by mass or less, further preferably 40% by mass or less. When the amount is within the above range, a beneficial effect tends to be achieved better.
[0049] The amount of at least one hydrogenated conjugated diene polymer (B) is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, and further preferably 25 parts by mass or more, but is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and further preferably 35 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0050] In addition to the hydrogenated conjugated diene polymer (A), examples of rubber components that can be used in the rubber composition include diene rubbers such as natural rubber (NR), styrene-butadiene rubber (SBR), polybutadiene rubber (BR), acrylonitrile-butadiene rubber (NBR) and styrene-isoprene-butadiene copolymer rubber (SIBR). These can be used alone or in combination of two or more.
[0051] The rubber component and the hydrogenated conjugated diene polymer (B) may each be modified to introduce a functional group that interacts with a filler (eg, silica) into the polymer.
[0052] The example of functional group comprises: amino, amide, silyl, alkoxysilyl, isocyanate, imino, imidazolyl, urea, ether, carbonyl, oxycarbonyl, sulfydryl, thioether, disulfide, sulfonyl, sulfinyl, thiocarbonyl, ammonium, imido, hydrazine, azo, diazo, carboxyl, nitrile, pyridyl, alkoxy, hydroxyl, oxygen base and epoxy group.These functional groups can be substituted.In these, preferably amino (preferably hydrogen atom is replaced by C1-C6 alkyl amino), alkoxy (preferably C1-C6 alkoxy) and alkoxysilyl (preferably C1-C6 alkoxysilyl).
[0053] Specific examples of compounds (modifiers) having these functional groups include: 2-dimethylaminoethyltrimethoxysilane, 3-dimethylaminopropyltrimethoxysilane, 2-dimethylaminoethyltriethoxysilane, 3-dimethylaminopropyltriethoxysilane, 2-diethylaminoethyltrimethoxysilane, 3-diethylaminopropyltrimethoxysilane, 2-diethylaminoethyltriethoxysilane and 3-diethylaminopropyltriethoxysilane.
[0054] The rubber composition contains at least one resin having a softening point of 20° C. or higher.
[0055] Examples of resins include coumarone-indene resins, styrene resins, terpene resins, C5 / C9 resins, and phenolic resins. These can be used alone or in combination of two or more. Among these, coumarone-indene resins, styrene resins, and terpene resins are preferred.
[0056] The term "coumarone-indene resin" refers to a polymer having structural units mainly derived from coumarone and indene. Examples include copolymers of coumarone and indene, and copolymers of coumarone and indene and other monomers (e.g., terpenes, conjugated diene compounds). Of these, coumarone-indene resins (copolymers of coumarone and indene) are preferred.
[0057] The term "styrene resin" refers to a liquid polymer having a structural unit mainly derived from styrene. Examples include homopolymers of styrene (e.g., styrene, α-methylstyrene), copolymers of two or more styrenes, and copolymers of styrene with other monomers (e.g., terpenes, conjugated diene compounds). Among these, copolymers of α-methylstyrene and styrene are preferred.
[0058] The term "terpene resin" refers to a liquid polymer having a structural unit mainly derived from terpene. Examples include homopolymers of terpenes (e.g., α-pinene, β-pinene, farnesene, myrcene), copolymers of two or more terpenes, and copolymers of terpenes with other monomers (e.g., aromatic vinyl compounds, conjugated diene compounds), such as terpene-styrene copolymers and farnesene-butadiene copolymers. Among these, β-pinene resin (homopolymer of β-pinene) is preferred.
[0059] Although it is sufficient that the softening point of the resin is 20° C. or higher, it is preferably 30° C. or higher, but is preferably 130° C. or lower, more preferably 116° C. or lower, further preferably 85° C. or lower. When the softening point is within the above range, the overall performance in terms of fuel economy and wet grip performance tends to be better.
[0060] The softening point is measured using a ring and ball softening point measuring apparatus as described in JIS K 6220-1:2001, and is defined as the temperature at which a ball falls.
[0061] The resin can be purchased from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemical Company, BASF, Arizona Chemical Company, Nitto Chemical Co., Ltd., Nippon Shokubai Co., Ltd., JXTG Nippon Oil & Energy Co., Ltd., Arakawa Chemical Industries, Ltd., Taoka Chemical Co., Ltd., ExxonMobil, and the like.
[0062] The amount of at least one resin is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and further preferably 5 parts by mass or more, but is preferably 25 parts by mass or less, more preferably 20 parts by mass or less, and further preferably 15 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, bleeding tends to be further suppressed.
[0063] The total amount of at least one hydrogenated conjugated diene polymer (B) and at least one resin is preferably 6 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 30 parts by mass or more, but is preferably 40 parts by mass or less, and more preferably 35 parts by mass or less, relative to 100 parts by mass of the rubber component. When the total amount is within the above range, bleeding tends to be further suppressed.
[0064] The rubber composition may comprise at least one filler selected from carbon black and silica, preferably a combination of carbon black and silica.
[0065] Any carbon black can be used, examples include N134, N110, N220, N234, N219, N339, N330, N326, N351, N550 and N762. Available commercial products can be purchased from Asahi Carbon Co., Ltd., Cabot (Japan) Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Co., Ltd., Lion Co., Ltd., Shin Nichika Carbon Co., Ltd., Columbia Carbon Co., Ltd., etc. These can be used alone or in combination of two or more.
[0066] Nitrogen adsorption specific surface area of carbon black (N 2 SA) is preferably 80m 2 / g or more, more preferably 100m 2 / g or more, more preferably 114m 2 / g or more, but preferably 160m 2 / g or less, more preferably 140m 2 / g or less, more preferably 125m 2 / g or less. 2 When SA is within the above range, the beneficial effects tend to be better achieved.
[0067] Carbon black N 2 SA is measured based on JIS K6217-2:2001.
[0068] The amount of carbon black is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and further preferably 5 parts by mass or more, but is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and further more preferably 10 parts by mass or less relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0069] Examples of silicon dioxide include dry process silicon dioxide (anhydrous silicic acid) and wet process silicon dioxide (hydrous silicic acid). Wet process silicon dioxide is preferred because it has a large amount of silanol groups. Available commercial products can be purchased from Evonik, Tosoh Silica Co., Ltd., Solvay (Japan) Co., Ltd., Tokuyama Co., Ltd., etc. These can be used alone or in combination of two or more.
[0070] The nitrogen adsorption specific surface area of silicon dioxide (N 2 SA) is preferably 100m 2 / g or more, more preferably 150m 2 / g or more, more preferably 180m 2 / g or more, but preferably 250m 2 / g or less, more preferably 220m2 / g or less, more preferably 200m 2 / g or less. 2 When SA is within the above range, the beneficial effects tend to be better achieved.
[0071] The nitrogen adsorption specific surface area of silica is measured by the BET method according to ASTM D3037-81.
[0072] The amount of silica is preferably 20 parts by mass or more, more preferably 40 parts by mass or more, and further preferably 50 parts by mass or more, and is preferably 100 parts by mass or less, more preferably 80 parts by mass or less, and further more preferably 60 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0073] Silica is preferably used together with a silane coupling agent.
[0074] Any silane coupling agent can be used, and examples include sulfide-based silane coupling agents such as bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(trimethoxysilylbutyl) trisulfide, bis(3-triethoxysilylpropyl) disulfide, bis(2-triethoxysilylethyl) disulfide, bis(4-triethoxysilylbutyl) disulfide, bis(3-trimethoxysilylpropyl) disulfide, bis(2-trimethoxysilylethyl) disulfide, bis(4-trimethoxysilylbutyl) disulfide, 3-trimethoxysilylpropyl-N,N-dimethylsulfide 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, and 3-triethoxysilylpropyl methacrylate monosulfide; mercapto-based silane coupling agents, such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, NXT and NXT-Z (both can be purchased from Momentive); vinyl-based silane coupling agents, such as vinyltriethoxysilane and vinyltrimethoxysilane; amino silane coupling agents such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy silane coupling agents such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro silane coupling agents such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chlorine silane coupling agents such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. Available commercial products can be purchased from Evonik, Momentive, Shin-Etsu Silicone, Tokyo Chemical Industry Co., Ltd., Azmax, Dow Corning Toray Co., Ltd., etc. These can be used alone or in combination of two or more.
[0075] The amount of the silane coupling agent is preferably 3 parts by mass or more, more preferably 6 parts by mass or more, but is preferably 12 parts by mass or less, more preferably 9 parts by mass or less, relative to 100 parts by mass of silica. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0076] The rubber composition may contain wax.
[0077] Any wax may be used, examples of which include: petroleum waxes such as paraffin wax and microcrystalline wax; naturally occurring waxes such as vegetable wax and animal wax; and synthetic waxes such as polymers of ethylene, propylene or other similar monomers. Usable commercial products may be purchased from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., Seiko Chemical Co., Ltd., etc. These may be used alone or in combination of two or more.
[0078] The amount of the wax is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, but is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0079] The rubber composition may contain oil.
[0080] The example of oil includes: process oil, vegetable oil and their mixture. The example of process oil includes paraffin process oil, aromatic process oil and cycloparaffin process oil. The example of vegetable oil includes: castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice bran oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia oil and tung oil. Available commercial products can be purchased from Idemitsu Kosan Co., Ltd., Sankyo Oil Chemical Industry Co., Ltd., JXTG Japan Oil Energy Co., Ltd., Orison, H&R, Toyokuni Oil Manufacturing Co., Ltd., Showa Shell Oil Co., Ltd., Fuji Kosan Co., Ltd., etc. These can be used alone or in combination of two or more.
[0081] The amount of oil is preferably 25 parts by mass or less, more preferably 10 parts by mass or less, further more preferably 5 parts by mass or less, relative to 100 parts by mass of the rubber component, and may be 0 parts by mass (the rubber composition contains substantially no oil). Since the hydrogenated conjugated diene polymer (B) acts as a plasticizer in the rubber composition, the amount of oil can be reduced to provide better fuel economy.
[0082] The rubber composition may contain an antioxidant.
[0083] Examples of antioxidants include naphthylamine antioxidants such as phenyl-α-naphthylamine; diphenylamine antioxidants such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; p-phenylenediamine antioxidants such as N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and N,N'-di-2-naphthyl-p-phenylenediamine; quinoline antioxidants such as 2,2,4-trimethyl-1,2-dihydroquinoline polymers; monophenol antioxidants such as 2,6-di-tert-butyl-4-methylphenol and styrenated phenol; and bisphenol antioxidants, triphenol antioxidants or polyphenol antioxidants such as tetrakis[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane. Commercially available products that can be used are commercially available from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., Flex Corporation, etc. These can be used alone or in combination of two or more.
[0084] The amount of the antioxidant is preferably 1 part by mass or more, more preferably 2 parts by mass or more, but is preferably 6 parts by mass or less, more preferably 4 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0085] The rubber composition may contain stearic acid.
[0086] Stearic acid may be conventional stearic acid. Commercially available products that can be used may be purchased from NOF Corporation, Kao Corporation, Fujifilm Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., etc. These may be used alone or in combination of two or more.
[0087] The amount of stearic acid is preferably 1 part by mass or more, more preferably 2 parts by mass or more, but is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0088] The rubber composition may include zinc oxide.
[0089] Zinc oxide may be conventional zinc oxide. Commercially available products that can be used may be purchased from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Industry Co., Ltd., Shiraishi Techno Co., Ltd., Shodo Chemical Industry Co., Ltd., Sakai Chemical Co., Ltd., etc. These may be used alone or in combination of two or more.
[0090] The amount of zinc oxide is preferably 1 part by mass or more, more preferably 2 parts by mass or more, but is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0091] The rubber composition may contain sulfur.
[0092] Examples of sulfur include those commonly used in the rubber industry, such as powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, and soluble sulfur. Available commercial products can be purchased from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flex Corporation, Nippon Innolux Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These can be used alone or in combination of two or more.
[0093] The amount of sulfur is preferably 0.5 parts by mass or more, more preferably 1.2 parts by mass or more, but is preferably 6 parts by mass or less, more preferably 3 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0094] The rubber composition may contain a vulcanization accelerator.
[0095] Examples of vulcanization accelerators include: thiazole vulcanization accelerators, such as 2-benzothiazole, di-2-benzothiazolyl disulfide; thiuram vulcanization accelerators, such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD) and tetrakis (2-ethylhexyl) thiuram disulfide (TOT-N); sulfenamide vulcanization accelerators, such as N-cyclohexyl-2-benzothiazole sulfenamide (CBS), N-tert-butyl-2-benzothiazole sulfenamide (TBBS), N-oxyethylene-2-benzothiazole sulfenamide, N, N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine vulcanization accelerators, such as diphenylguanidine, di-o-tolylguanidine and o-tolylbiguanide. Commercially available products that can be used can be purchased from Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., etc. These can be used alone or in combination of two or more.
[0096] The amount of the vulcanization accelerator is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and further preferably 3.8 parts by mass or more, and preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and further preferably 6 parts by mass or less, relative to 100 parts by mass of the rubber component. When the amount is within the above range, the beneficial effects tend to be better achieved.
[0097] In addition to the above components, the rubber composition may also contain additives commonly used in the tire industry, including, for example, organic peroxides and fillers such as calcium carbonate, talc, alumina, clay, aluminum hydroxide and mica. The amount of each of these additives is preferably 0.1 to 200 parts by mass relative to 100 parts by mass of the rubber component.
[0098] For example, the rubber composition can be prepared by kneading the above-mentioned components using a rubber kneading machine such as an open roll mill or a Banbury mixer, and then vulcanizing the kneaded mixture.
[0099] The kneading conditions are as follows. In the basic kneading step of kneading additives other than the vulcanizing agent and the vulcanization accelerator, the kneading temperature is generally 100°C to 180°C, preferably 120°C to 170°C. In the final kneading step of kneading the vulcanizing agent and the vulcanization accelerator, the kneading temperature is generally 120°C or less, preferably 850°C to 110°C. Then, the composition obtained after kneading the vulcanizing agent and the vulcanization accelerator is generally vulcanized by, for example, press vulcanization. The vulcanization temperature is generally 140°C to 190°C, preferably 150°C to 185°C. The vulcanization time is generally 5 to 15 minutes.
[0100] The change in hardness of the rubber composition after immersion in acetone for 24 hours can be used as an index of the change in hardness over time.
[0101] The hardness change relative to the hardness before immersion is preferably 20% or less, more preferably 10% or less, further preferably 5% or less, particularly preferably 4% or less, and may be 3% or less, 2% or less, or 0% (the hardness before and after immersion in acetone is substantially the same). When the change is within the above range, the change in hardness over time tends to be small, resulting in good durability.
[0102] The change in hardness can be measured as described below in the Examples.
[0103] The mass of the rubber composition after immersion in acetone for 24 hours can also be used as an index of the change in hardness over time.
[0104] The mass is preferably 80% or more of the mass before immersion, more preferably 90% or more, further preferably 91% or more, particularly preferably 92% or more, and may be 94% or more, 96% or more, 98% or more, or 100% (the mass before and after immersion in acetone is substantially the same). When the mass is within the above range, the change in hardness over time tends to be small, resulting in good durability.
[0105] The mass can be measured as described below in the Examples.
[0106] The rubber composition can be used for tire components (i.e., as a tire rubber composition), including tread (coasting surface), sidewall, base tread, undertread, shoulder, clinch, bead apex, cushion rubber, carcass cord topping rubber, insulation layer, bead filler and inner liner, as well as side reinforcement layers of run flat tires.
[0107] The tire of the present invention can be produced from the above-mentioned rubber composition by a conventional method.
[0108] Specifically, the rubber composition before vulcanization can be extruded into the shape of a tire component (such as a tread), then assembled with other tire components in a conventional manner on a tire building machine to form an unvulcanized tire, which is then heated and pressurized in a vulcanizer to produce a tire.
[0109] Here, it is sufficient that a tire component (eg, tread) of the tire at least partially comprises the rubber composition. The entire tire component may comprise the rubber composition.
[0110] The tire (e.g., pneumatic tire) can be used as: a tire for a passenger car; a tire for a truck and a bus; a tire for a two-wheeled vehicle; a high-performance tire; a winter tire, such as a studless winter tire; a run-flat tire with a side reinforcing layer; a tire with a sound-absorbing component, which has a sound-absorbing component such as a sponge in the inner cavity of the tire; a tire with a sealant, which includes a sealant capable of sealing a puncture in the interior of the tire or on the inner cavity of the tire; a tire equipped with an electronic component, which includes an electronic component (e.g., a sensor or a radio tag) in the interior of the tire or on the inner cavity of the tire; etc. The tire is suitable for a passenger car.
[0111] Example
[0112] The present invention will be specifically described below with reference to Examples, but the present invention is not limited to the Examples.
[0113] Chemicals used in Examples and Comparative Examples are listed below.
[0114] SBR: HPR850 purchased from JSR Corporation
[0115] Hydrogenated copolymer (1): Preparation Example 1-1 below (hydrogenated SBR, degree of hydrogenation: 95 mol%, aromatic vinyl (styrene) unit: 33 mass%, Mw: 300,000)
[0116] Hydrogenated copolymer (2): Preparation Example 1-2 below (hydrogenated SBR, degree of hydrogenation: 80 mol%, aromatic vinyl (styrene) unit: 33 mass%, Mw: 300,000)
[0117] Hydrogenated copolymer (3): Preparation Example 1-3 below (hydrogenated SBR, degree of hydrogenation: 95 mol%, aromatic vinyl (styrene) unit: 33 mass%, Mw: 120,000)
[0118] Carbon black: N220 (N220) purchased from Cabot (Japan) 2 SA: 114m 2 / g)
[0119] Silicon dioxide: ULTRASIL VN3 (N 2 SA: 180m 2 / g)
[0120] Silane coupling agent: Si266 (bis(3-triethoxysilylpropyl) disulfide) purchased from Evonik
[0121] Oil: Diana Process NH-70S (aromatic process oil) purchased from Idemitsu Kosan Co., Ltd.
[0122] Liquid SBR: RICON 100 (Mw: 4,500) purchased from Cray Valley
[0123] Liquid hydrogenated SBR (1): hydrogenated product of RICON 100 available from Cray Valley (Mw: 4,500, degree of hydrogenation: 50 mol%, aromatic vinyl (styrene) unit: 25 mass%)
[0124] Liquid hydrogenated SBR (2): hydrogenated product of RICON 100 available from Cray Valley (Mw: 4,500, degree of hydrogenation: 95 mol%, aromatic vinyl (styrene) unit: 25 mass%)
[0125] Liquid hydrogenated SBR (3): Preparation Example 2 below (Mw: 80,000, degree of hydrogenation: 95 mol%, aromatic vinyl (styrene) unit: 25 mass%)
[0126] Resin (1): NOVARES C10 (coumarone-indene resin, softening point: 10°C) purchased from Rutgers Chemical Company
[0127] Resin (2): NOVARES C30 (coumarone-indene resin, softening point: 30° C.) purchased from Rutgers Chemical Company
[0128] Resin (3): Sylvares SA85 (copolymer of α-methylstyrene and styrene, softening point: 85° C.) purchased from Arizona Chemical Company
[0129] Resin (4): Sylvatraxx 4150 (β-pinene resin, softening point: 116° C.) purchased from Arizona Chemical Company
[0130] Antioxidant: NOCRAC 6C (N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine) purchased from Ouchi Shinko Chemical Industry Co., Ltd.
[0131] Stearic acid: stearic acid "TSUBAKI" purchased from NOF Corporation
[0132] Zinc oxide: Zinc oxide #1 purchased from Mitsui Mining and Smelting Co., Ltd.
[0133] Wax: Ozoace 0355 purchased from Nippon Seiro Co., Ltd.
[0134] Sulfur: HK-200-5 (powdered sulfur containing 5% by mass of oil) purchased from Hosoi Chemical Industry Co., Ltd.
[0135] Vulcanization accelerator (1): NOCCELER NS (N-tert-butyl-2-benzothiazole sulfenamide, TBBS) purchased from Ouchi Shinko Chemical Industry Co., Ltd.
[0136] Vulcanization accelerator (2): NOCCELER D (N, N'-diphenylguanidine, DPG) purchased from Ouchi Shinko Chemical Industry Co., Ltd.
[0137] <Production Example 1-1: Production of Hydrogenated Copolymer (1)>
[0138] n-Hexane, styrene, 1,3-butadiene, N,N,N',N'-tetramethylethylenediamine (TMEDA) and n-butyllithium are placed in a heat-resistant reaction vessel fully purged with nitrogen, and then stirred at 50°C for 5 hours to carry out a polymerization reaction. Afterwards, the reaction solution is stirred for 20 minutes, while hydrogen is supplied at a gauge pressure of 0.4 MPa to react the unreacted polymer terminal lithium with hydrogen to form lithium hydride. Hydrogenation is carried out using a dichlorodipentadienyl titanocene catalyst at a hydrogen supply pressure of 0.7 MPa gauge and a reaction temperature of 90°C. Once the cumulative amount of absorbed hydrogen reaches an amount corresponding to the target degree of hydrogenation, the reaction temperature is raised to room temperature and the hydrogen pressure is restored to normal pressure. Then, the reaction solution is extracted from the reaction vessel and introduced into water under stirring. The solvent is removed by steam stripping to obtain a hydrogenated copolymer (1). The polymerization conversion rate is almost 100%.
[0139] <Production Example 1-2: Production of Hydrogenated Copolymer (2)>
[0140] The preparation of hydrogenated copolymer (2) was the same as in Preparation Example 1, except that the amount of chemicals and the cumulative amount of absorbed hydrogen were changed. The polymerization conversion was almost 100%.
[0141] <Production Example 1-3: Production of Hydrogenated Copolymer (3)>
[0142] The preparation of hydrogenated copolymer (3) was the same as in Preparation Example 1 except that the amounts of chemicals were changed. The polymerization conversion was almost 100%.
[0143] <Production Example 2: Production of Liquid Hydrogenated SBR (3)>
[0144] Hexane, butadiene and styrene are introduced into a heat-resistant reaction vessel fully purged with nitrogen together with TMEDA. Next, a small amount of n-butyl lithium solution in hexane is introduced into the polymerization vessel as a scavenger to preliminarily remove impurities that inactivate the polymerization initiator. Then, a hexane solution of n-butyl lithium is added and the polymerization reaction is carried out at 50°C for 3 hours. After 3 hours, 1M isopropanol / hexane solution is added dropwise to terminate the reaction. Subsequently, the polymerization solution is evaporated at room temperature for 24 hours and then vacuum dried at 80°C for 24 hours to obtain a copolymer.
[0145] Next, the copolymer, n-hexane and 10% palladium carbon were placed in a pressure vessel, the vessel was purged with nitrogen, and then heated at 5.0 kg / cm 2The reaction mixture was stirred for 24 hours at room temperature and then dried under vacuum at 80°C for 24 hours to obtain liquid hydrogenated SBR (3). The polymerization conversion rate was almost 100%.
[0146] <Examples and Comparative Examples>
[0147] According to the formulation shown in Table 1, materials other than sulfur and vulcanization accelerator were kneaded at 150° C. for 5 minutes in a 1.77 L Banbury mixer (Kobe Steel) to obtain a kneaded mixture. Then, sulfur and vulcanization accelerator were added to the kneaded mixture, and they were kneaded at 80° C. for 5 minutes in an open roll mill to obtain an unvulcanized rubber composition. The unvulcanized rubber composition was vulcanized at 170° C. for 10 minutes to obtain a vulcanized rubber composition.
[0148] The test tires prepared as above were evaluated as described below. Table 1 shows the results.
[0149] It should be noted that all measurements were performed within 3 days after vulcanization.
[0150] (Mass Change)
[0151] The mass of a sample of each vulcanized rubber composition was measured.
[0152] Furthermore, the measured sample was immersed in acetone for 24 hours, dried, and then the mass was measured again.
[0153] Then, the mass change after immersion in acetone is expressed as an index using the following formula. Generally, the index is below 100, and the closer the index is to 100, the better (the smaller the change in hardness over time). An index above 90 is considered acceptable.
[0154] (Mass change index) = (Mass after immersion in acetone) / (Mass before immersion in acetone) × 100
[0155] The mass change index can be used to determine the mass after immersion in acetone. For example, a mass change index of 80 means that the mass after immersion in acetone is 80% of the mass before immersion.
[0156] (Hardness change)
[0157] The hardness (JIS-A hardness) of each vulcanized rubber composition sample at room temperature (25° C.) was measured using a type A durometer in accordance with “Rubber, vulcanized or thermoplastic rubber—Determination of hardness—Part 3: Durometer method” in JIS K6253-3 (2012).
[0158] Furthermore, the sample to be measured was immersed in acetone for 24 hours, dried, and the hardness at room temperature was measured as described above.
[0159] Then, the change in hardness after immersion in acetone is expressed as an index using the following formula. Generally, the index is below 100, and the closer the index is to 100, the better (the smaller the change in hardness over time). An index above 95 is considered acceptable.
[0160] (Hardness change index) = (Hardness before immersion in acetone) / (Hardness after immersion in acetone) × 100
[0161] The hardness change index can be used to determine the hardness change (%) after immersion in acetone. For example, a hardness change index of 80 means that the hardness change after immersion in acetone is 20% relative to the hardness before immersion.
[0162] (Fuel Economy)
[0163] The tan δ of the vulcanized rubber composition was measured using a viscoelasticity spectrometer (RSA from TA Instruments) at a temperature of 30° C., an initial strain of 10%, a dynamic strain of 2.5%, and a frequency of 10 Hz. The results were expressed as an index (fuel economy index) relative to the reciprocal of the tan δ value of Comparative Example 1, where Comparative Example 1 was taken as 100. A higher index indicates better fuel economy.
[0164] (Wet grip performance)
[0165] The tan δ of the vulcanized rubber composition was measured using a viscoelasticity spectrometer (RSA from TA Instruments) at 0°C, 10% initial strain, 0.5% dynamic strain and 10 Hz frequency. The results were expressed as an index (wet grip performance index) relative to the tan δ value of Comparative Example 1, where Comparative Example 1 was taken as 100. A higher index indicates better wet grip performance.
[0166] [Table 1]
[0167]
[0168] As shown in Table 1, the examples, which comprise a hydrogenated conjugated diene polymer (A) having a weight average molecular weight of 100,000 or more and a degree of hydrogenation of 75 mol% or more, a hydrogenated conjugated diene polymer (B) having a weight average molecular weight of less than 100,000, and a resin having a softening point of 20° C. or more, exhibited less variation in hardness and mass and excellent durability performance. These examples also had good fuel economy and wet grip performance.
Claims
1. Rubber composition, in, The rubber composition comprises: at least one hydrogenated conjugated diene polymer (A), the hydrogenated conjugated diene polymer (A) having a weight average molecular weight of 100,000 or more and a degree of hydrogenation of 75 mol % or more; at least one hydrogenated conjugated diene polymer (B), the hydrogenated conjugated diene polymer (B) having a weight average molecular weight of 4,500 or less; and At least one resin, the softening point of the resin is above 20°C; Wherein, the hydrogenated conjugated diene polymer (A) is a copolymer of a conjugated diene compound and an aromatic vinyl compound; The hydrogenated conjugated diene polymer (A) contains 33% by mass or less of a structural unit derived from at least one aromatic vinyl compound.
2. The rubber composition according to claim 1, in, The absolute value of the difference in hydrogenation degree between the hydrogenated conjugated diene polymer (A) and the hydrogenated conjugated diene polymer (B) is 90 mol % or less.
3. The rubber composition according to claim 1 or 2, in, The hydrogenation degree of the hydrogenated conjugated diene polymer (B) is 25 mol % or more.
4. The rubber composition according to claim 1 or 2, in, The hydrogenated conjugated diene polymer (B) is present in an amount of 5 parts by mass or more relative to 100 parts by mass of the rubber component in the rubber composition.
5. The rubber composition according to claim 1 or 2, in, The total amount of the hydrogenated conjugated diene polymer (B) and the resin is 40 parts by mass or less relative to 100 parts by mass of the rubber component in the rubber composition.
6. The rubber composition according to claim 1 or 2, in, The rubber composition has a hardness that changes by 20% or less after being immersed in acetone for 24 hours relative to the hardness before being immersed.
7. The rubber composition according to claim 1 or 2, in, The mass of the rubber composition after being immersed in acetone for 24 hours is more than 80% of the mass before the immersion.
8. The rubber composition according to claim 1 or 2, in, The rubber composition comprises at least one filler selected from carbon black and silica.
9. The rubber composition according to claim 1 or 2, in, The resin is at least one selected from coumarone-indene resin, styrene resin and terpene resin.
10. The rubber composition according to claim 1 or 2, in, The hydrogenated conjugated diene polymer (A) has a weight average molecular weight of 200,000 to 1,000,000 and a degree of hydrogenation of 90 mol % to 98 mol %; and The hydrogenated conjugated diene polymer (B) has a weight average molecular weight of 1,000 to 6,000 and a degree of hydrogenation of 40 mol % to 98 mol %.
11. The rubber composition according to claim 1 or 2, in, The hydrogenated conjugated diene polymer (A) and the hydrogenated conjugated diene polymer (B) are each a copolymer of a conjugated diene compound and an aromatic vinyl compound; The hydrogenated conjugated diene polymer (A) contains 10% to 50% by mass of a structural unit derived from at least one aromatic vinyl compound; and The hydrogenated conjugated diene polymer (B) contains 10% to 50% by mass of a structural unit derived from at least one aromatic vinyl compound.
12. The rubber composition according to claim 1 or 2, in, The hydrogenated conjugated diene polymer (A) is present in an amount of 80% by mass or more based on 100% by mass of the rubber component in the rubber composition.
13. The rubber composition according to claim 1 or 2, in, The softening point of the resin is 30°C to 130°C.
14. The rubber composition according to claim 1 or 2, in, The rubber composition includes 1 to 25 parts by mass of a resin, 1 to 30 parts by mass of carbon black, and 20 to 100 parts by mass of silica, relative to 100 parts by mass of a rubber component in the rubber composition. 15 . A tire comprising a tire component comprising the rubber composition according to claim 1 .