Composite sheet and method for producing the same, and laminate and method for producing the same
By preparing a composite sheet of porous nitride sintered body and a thermosetting resin composition and connecting it with a metal substrate, the problem of heat dissipation deviation of the laminated body in the prior art is solved, and more uniform heat conduction performance and higher adhesiveness are achieved Connection strength.
Patent Information
- Application Number
- CN202080069954.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-23
- Filing Date
- 2020-10-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-10-21
AI Technical Summary
The heat dissipation properties of the existing composite sheets are deviated when laminated with metal substrates, resulting in uneven thermal conductivity and affecting efficient heat dissipation performance.
The composite sheet is prepared by cutting off the wire saw by a wire saw, and the main surface roughness Rz is controlled below 10 μm, and the main surface roughness Rz is controlled below 10 μm, and It is connected to the metal substrate by heating and pressurization to form an excellent laminated body.
The difference in heat dissipation properties on the laminated connection interface is effectively reduced, the consistency and adhesion properties of heat dissipation are improved, and the bonding strength and insulation between the composite sheet and the metal substrate are enhanced.
Smart Images

Figure CN114466899B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a composite sheet and a method for producing the same, and a laminate and a method for producing the same. Background Art
[0002] In electronic components such as LED lighting devices and automotive power modules, it is a problem to efficiently dissipate the heat generated during use. To address this problem, the following countermeasures have been taken: a method of increasing the thermal conductivity of the insulating layer of the printed wiring board on which the electronic components are mounted; a method of mounting the electronic components or printed wiring board on a heat sink via an electrically insulating thermal interface material (Thermal Interface Materials); etc. For such insulating layers and thermal interface materials, a composite (heat dissipation component) composed of a resin and ceramics such as boron nitride can be used.
[0003] As such a composite, a composite in which ceramic powder is dispersed in a resin has been conventionally used. In recent years, a composite in which a porous ceramic sintered body (for example, a boron nitride sintered body) is impregnated with a resin has also been studied (for example, Patent Document 1).
[0004] In addition, studies have been conducted to reduce the thermal resistance of the laminate by bringing the circuit substrate into direct contact with the primary particles constituting the boron nitride sintered body, thereby improving the heat dissipation. For example, Patent Document 2 describes a method for manufacturing a laminate by bonding a circuit substrate having an adjusted arithmetic mean roughness Ra and a composite body including a boron nitride sintered body by heating and pressing, and deforming the composite body by using the convex portion on the adhesive layer side surface of the circuit substrate to cause the composite body to penetrate.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2014 / 196496
[0008] Patent Document 2: Japanese Patent Application Publication No. 2016-103611 Summary of the invention
[0009] Problems to be solved by the invention
[0010] However, laminates produced using conventional composite sheets may have variations in heat dissipation, and there is room for improvement.
[0011] An object of the present invention is to provide a composite sheet having excellent heat dissipation when laminated with a metal substrate, and a method for producing the same. Another object of the present invention is to provide a laminate having excellent heat dissipation, and a method for producing the same.
[0012] Means for solving problems
[0013] One aspect of the present invention provides a composite sheet comprising: a nitride sintered body having a porous structure; and a semi-cured product of a thermosetting resin composition impregnated in the nitride sintered body, wherein the line roughness Rz (maximum height) of at least one main surface of the composite sheet as specified in JIS B 0601:2013 is 10 μm or less.
[0014] Since the composite sheet has a semi-cured product of a thermosetting composition, it can be bonded to an adherend. In addition, since the line roughness Rz of at least one main surface of the composite sheet is small, the thickness deviation of the resin layer portion with poor heat dissipation can be reduced at the interface when connected to the adherend. Therefore, a laminate with excellent heat dissipation can be manufactured.
[0015] When using conventional composite sheets to prepare a laminate with a metal substrate, there are sometimes deviations in thermal conductivity depending on the position. Such deviations in thermal conductivity corresponding to the position can become a problem in fields requiring high heat dissipation. With conventional composite sheets, since large depressions and projections can be formed on their surfaces, when using them to bond with metal substrates, resin layers of different thicknesses can be formed between the above-mentioned surface of the composite sheet and the metal substrate depending on the position. The inventors of the present application speculate that this is the reason why the laminate has deviations in thermal conductivity. On the other hand, in the composite sheet of the present invention, the main surface is smoother, and the deviation in the thickness of the resin layer as described above is small. Therefore, it is believed that the above-mentioned effect can be obtained.
[0016] The arithmetic mean roughness Ra of the main surface as specified in JIS B 0601: 2013 may be 2.0 μm or less. By setting the arithmetic mean roughness Ra of the main surface to a specified value or less, the variation in the in-plane heat dissipation at the interface with the adherend can be further reduced.
[0017] The content of the semi-cured material may be 20 to 70% by volume. When the content of the semi-cured material is within the above range, the adhesion between the adherend and the composite sheet can be further improved. In addition, when the content of the semi-cured material is within the above range, the insulation after bonding to the adherend is also excellent.
[0018] The thickness of the composite sheet may be 1.0 mm or less.
[0019] One aspect of the present invention provides a method for manufacturing a composite sheet, comprising: using a wire saw at a wire reciprocating speed of 155 to 1000 m / min and a worktable moving speed of 4 mm / min to cut a resin impregnation body having a porous structure and a semi-cured material of a thermosetting resin composition impregnated in the above-mentioned nitride sintered body to obtain a composite sheet, wherein the line roughness Rz (maximum height) of at least one main surface of the above-mentioned composite sheet as specified in JIS B 0601:2013 is less than 10 μm.
[0020] The above-mentioned method for producing a composite sheet can produce a composite sheet having a line roughness Rz of a main surface of a predetermined value or less by cutting the resin impregnation body with a wire saw operated under predetermined conditions.
[0021] The width of the resin impregnation body may be 5 to 150 mm. By setting the width of the resin impregnation body within the above range, the contact distance between the resin impregnation body and the wire can be reduced, and the Rz value of the main surface (processed surface) of the obtained composite sheet can be more easily adjusted.
[0022] One aspect of the present invention provides a laminate, which includes a first metal substrate, an intermediate layer arranged on the above-mentioned first metal substrate, and a second metal substrate arranged on the side of the above-mentioned intermediate layer opposite to the above-mentioned first metal substrate, the above-mentioned first metal substrate and the above-mentioned second metal substrate are connected by the above-mentioned intermediate layer, and the above-mentioned intermediate layer is a cured product of the above-mentioned composite sheet.
[0023] The laminate is formed by connecting the metal substrate with the cured product of the composite sheet, and thus has excellent heat dissipation. In addition, since the laminate is formed by connecting the metal substrate with the cured product of the composite sheet, the deviation of heat dissipation in the in-plane direction of the connection interface can be reduced.
[0024] The line roughness Rz (maximum height) of the main surface on the intermediate layer side of the first metal substrate and the second metal substrate as specified in JIS B 0601:2013 may be 10 μm or less.
[0025] At least one of the first metal substrate and the second metal substrate may include at least one selected from the group consisting of copper and aluminum.
[0026] One aspect of the present invention provides a method for manufacturing a laminate, which includes the following steps: arranging and stacking a first metal substrate and a second metal substrate in a manner opposite to a pair of main surfaces of the above-mentioned composite sheet, respectively, heating the above-mentioned first metal substrate and the above-mentioned second metal substrate while being pressurized in the stacking direction, and connecting the above-mentioned composite sheet to the above-mentioned first metal substrate and the above-mentioned second metal substrate by curing the above-mentioned thermosetting resin composition.
[0027] The method for producing a laminated body uses the composite sheet, and thus can produce a laminated body having excellent heat dissipation properties.
[0028] Effects of the Invention
[0029] According to the present invention, a composite sheet having excellent heat dissipation when laminated with a metal substrate and a method for producing the same can be provided. According to the present invention, a laminate having excellent heat dissipation and a method for producing the same can also be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] [ Figure 1 ] Figure 1 This is a perspective view showing an example of a composite sheet.
[0031] [ Figure 2 ] Figure 2 This is a partial end view of the composite sheet.
[0032] [ Figure 3 ] Figure 3 This is a schematic diagram showing an example of a method for producing a composite sheet.
[0033] [ Figure 4 ] Figure 4 It is a schematic cross-sectional view showing an example of a laminated body.
[0034] [ Figure 5 ] Figure 5 This is a partial cross-sectional view of a laminate obtained using a conventional composite sheet. DETAILED DESCRIPTION
[0035] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings as appropriate. The following embodiments are illustrative for describing the present invention and are not intended to limit the present invention to the following contents. When describing, the same reference numerals are used for elements having the same element or the same function, and repeated descriptions are omitted as appropriate. In addition, unless otherwise specified, positional relationships such as up, down, left, and right are set based on the positional relationships shown in the accompanying drawings. In addition, the size ratios of the elements are not limited to the ratios shown in the drawings.
[0036] Unless otherwise specified, the materials exemplified in this specification may be used alone or in combination of two or more. In the case where there are multiple substances equivalent to each component in the composition, unless otherwise specified, the content of each component in the composition refers to the total amount of the multiple substances present in the composition.
[0037] One embodiment of the composite sheet comprises a nitride sintered body having a porous structure, and a semi-cured product of a thermosetting resin composition impregnated in the nitride sintered body. The composite sheet of the present invention is useful as an adhesive component (e.g., an adhesive sheet, etc.) that requires thermal conductivity and insulation. Specifically, the composite sheet of the present invention can be used as an adhesive component for bonding a metal circuit substrate to other layers in a power module structure and an LED light-emitting device.
[0038] Figure 1 It is a perspective view showing an example of a composite sheet. The composite sheet 10 has a pair of main surfaces 10a and 10b. Figure 2 This is a partial end view of the composite sheet. Figure 2 The case where the line roughness Rz (maximum height) of one main surface 10 a of the composite sheet 10 is small is shown.
[0039] In this specification, "sheet" means the area relative to the main surface (for example, in mm 2 The ratio of the thickness (e.g., value in mm) to the thickness (e.g., value in mm) of the composite sheet 10 is less than 0.01. The main surface (at least one of the main surface 10a or the main surface 10b) of the composite sheet 10 is a newly formed processed surface (a surface cut out from the resin impregnation body) in the manufacturing process. It should be noted that the resin impregnation body is sometimes also referred to as a casting (ingot).
[0040] The line roughness Rz (maximum height) specified by JIS B0601:2013 of at least one main surface (at least one of the main surface 10a or the main surface 10b) of the above-mentioned composite sheet 10 is 10μm or less. The upper limit value of the above-mentioned line roughness Rz can be, for example, 7μm or less, 5μm or less, or 4.5μm or less. By making the upper limit value of the above-mentioned line roughness Rz within the above-mentioned range, the proportion of the resin layer portion when connected to the metal substrate can be reduced, and the heat dissipation can be further improved. The lower limit value of the above-mentioned line roughness Rz can be, for example, 0.5μm or more, 1μm or more, or 2μm or more. The line roughness Rz of the above-mentioned composite sheet can also be controlled by, for example, adjusting the reciprocating line speed of the steel wire when cutting out from the resin impregnation body described later.
[0041] The upper limit of the arithmetic mean roughness Ra of the above-mentioned main surface (at least one of the main surface 10a or the main surface 10b, and the main surface with the above-mentioned Rz being less than 10μm) specified by JIS B 0601:2013 can be, for example, less than 2.0μm, less than 1.8μm, less than 1.5μm, less than 1.2μm, less than 1.0μm, or less than 0.9μm. When the above-mentioned arithmetic mean roughness Ra is within the above-mentioned range, the deviation of the in-plane heat dissipation at the interface with the adherend can be further reduced. The lower limit of the above-mentioned arithmetic mean roughness Ra can be, for example, more than 0.05μm, more than 0.1μm, or more than 0.5μm. The arithmetic mean roughness Ra of the above-mentioned composite sheet can also be controlled by, for example, adjusting the reciprocating linear speed of the steel wire when cutting out from the resin impregnation body described later.
[0042] The upper limit of the thickness of the composite sheet 10 may be, for example, 1.0 mm or less, 0.9 mm or less, 0.8 mm or less, or 0.7 mm or less. When the upper limit of the thickness of the composite sheet 10 is within the above range, the thermal resistance of the composite sheet 10 itself can be further reduced. The lower limit of the thickness of the composite sheet 10 may be, for example, 0.15 mm or more, or 0.20 mm or more. When the lower limit of the thickness of the composite sheet 10 is within the above range, the laminate obtained by using the composite sheet 10 can exert more sufficient insulation even when used at a high voltage.
[0043] A nitride sintered body having a porous structure and a semi-cured body of a thermosetting resin composition impregnated in the nitride sintered body. The nitride sintered body having a porous structure may be a sintered body formed by sintering primary particles of the nitride. The nitride sintered body having a porous structure may be, for example, a sintered body formed by sintering primary particles of boron nitride (a sintered body of boron nitride).
[0044] In this specification, the so-called "porous structure" refers to a structure having a plurality of micropores (hereinafter, also referred to as pores), including a structure in which at least a portion of the above-mentioned pores are connected to form a continuous hole. The average pore diameter of the above-mentioned pores can be, for example, less than 7 μm, less than 6 μm or less than 5 μm. If the average pore diameter is within the above range, the thermal conductivity of the composite can be improved. The average pore diameter of the above-mentioned pores can be, for example, more than 0.3 μm, more than 0.5 μm or more than 0.7 μm. If the average pore diameter is within the above range, it is easy to fill the pores with a thermosetting composition, which can further improve the adhesion between the composite and the adherend. In this specification, "average pore diameter" refers to the value measured by mercury penetration.
[0045] In this specification, the so-called "semi-cured" (also called B stage) state refers to a state that can be further cured by a subsequent curing treatment. The semi-cured state can be used to temporarily press-bond adherends such as metal substrates, and then bonded to the adherends by heating. The above-mentioned semi-cured material is in a semi-cured state, and by further curing treatment, it can become a "fully cured" (also called C stage) state. Whether the semi-cured material in the composite is in a semi-cured state that can be further cured can be confirmed, for example, by a differential scanning calorimeter.
[0046] As for the semi-cured product of the thermosetting composition (hereinafter, sometimes referred to as "semi-cured product"), as described later, it means that the curing reaction of the thermosetting composition has been carried out to a certain extent or more. Therefore, the semi-cured product of the thermosetting composition may include a thermosetting resin obtained by reacting the raw material components (compounds contained in the thermosetting composition, etc.) in the thermosetting composition. The above-mentioned semi-cured product may include compounds of unreacted components in the above-mentioned raw material components in addition to the above-mentioned thermosetting resin.
[0047] For the semi-cured product of thermosetting composition, for example, at least one structural unit selected from the group consisting of structural units from cyanate group, structural units from bismaleimide group, and structural units from epoxy group can be included, at least two structural units selected from the group consisting of structural units from cyanate group, structural units from bismaleimide group, and structural units from epoxy group can be included, and structural units from cyanate group, structural units from bismaleimide group, and structural units from epoxy group can be included. The semi-cured product of thermosetting composition has structural units from cyanate group, structural units from bismaleimide group, and structural units from epoxy group, so that the manufacture of composite becomes easy, and the adhesion of composite and adherend can be further improved.
[0048] The semi-cured material may have, for example, a structural unit derived from a cyanate group, may have at least one structural unit selected from the group consisting of a structural unit derived from a cyanate group, a structural unit derived from a bismaleimide group, and a structural unit derived from an epoxy group, or may have all of a structural unit derived from a cyanate group, a structural unit derived from a bismaleimide group, and a structural unit derived from an epoxy group.
[0049] As the structural unit having a cyanate group, for example, a triazine ring can be mentioned. As the structural unit derived from a bismaleimide group, for example, a structure represented by the following formula (1) can be mentioned. As the structural unit derived from an epoxy group, for example, a structure represented by the following general formula (2) can be mentioned. These structural units can be obtained by using 1 H-NMR and 13C-NMR can be used for detection. Alternatively, GPC (gel permeation chromatography) can be used for detection. The above structural units can be detected by either NMR or GPC.
[0050] [Chemical formula 1]
[0051]
[0052] [Chemical formula 2]
[0053]
[0054] In the above general formula (2), R 1 represents a hydrogen atom or other functional groups. Examples of other functional groups include alkyl groups.
[0055] The semi-cured material may have other structural units besides the structural units derived from the cyanate group, the structural units derived from the bismaleimide group, and the structural units derived from the epoxy group.
[0056] The semi-cured material may contain a thermosetting resin, or may contain at least one selected from the group consisting of a cyanate resin, a bismaleimide resin, and an epoxy resin. In addition to the thermosetting resin, the semi-cured material may contain, for example, a phenolic resin, a melamine resin, a urea-formaldehyde resin, and an alkyd resin.
[0057] The semi-cured material may also contain at least one curing agent selected from the group consisting of a phosphine curing agent and an imidazole curing agent. The phosphine curing agent can promote the triazine formation reaction based on the trimerization of the compound having a cyanate group. As the phosphine curing agent, for example, tetraphenylphosphine tetra-p-tolyl boronate can be mentioned. The imidazole curing agent generates oxazoline and promotes the curing reaction of the compound having an epoxy group. As the imidazole curing agent, for example, 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole can be mentioned. The semi-cured material may be a cured material formed by curing the polymerizable compound (for example, a compound having a cyanate group, a compound having an epoxy group, etc.) contained in the thermosetting composition by these curing agents.
[0058] The degree of curing of the semi-cured material can be, for example, the curing rate of the thermosetting composition with the curing rate of 100% when the curing rate is in a completely cured state as an index. The curing rate of the semi-cured material can be, for example, less than 70%, less than 65% or less than 60%. If the curing rate of the semi-cured material is within the above range, the adhesion between the composite and the adherend can be improved. In addition, since the semi-cured material moves in the resin composite, the pores in the resin composite can be filled and the dielectric breakdown voltage can be improved. In addition, the curing rate of the resin semi-cured material can be, for example, more than 5%, more than 15%, more than 30% or more than 40%. If the curing rate of the semi-cured material is within the above range, the semi-cured material can be suppressed from flowing out of the resin composite, and the semi-cured material can be fully kept in the pores of the nitride sintered body.
[0059] The above-mentioned cure rate can be determined by using a differential scanning calorimeter. First, the heat Q generated when 1g of the thermosetting composition in an uncured state is completely cured is measured. Next, 1g of a semi-cured material is collected from the composite to be measured, and the heat R generated when the collected semi-cured material is completely cured is measured. In the measurement, a differential scanning calorimeter is used. Afterwards, the cure rate of the semi-cured material can be calculated according to the following formula (A). It should be noted that whether the semi-cured material is completely cured can be confirmed by the end of the heat release in the heat release curve obtained by differential scanning calorimetry.
[0060] Curing rate of semi-cured product [%] = [(QR) / R] × 100···(A)
[0061] The above-mentioned curing rate can also be calculated as follows. That is, the curing rate of the semi-cured material impregnated in the nitride sintered body can be calculated by the following method. First, the calorific value Q2 generated when the uncured thermosetting composition is heated to make it completely cured is calculated. Then, the calorific value R2 generated when the sample collected from the semi-cured material possessed by the composite is heated in the same manner and completely cured is calculated. At this time, the mass of the sample used for the measurement by the differential scanning calorimeter is set to be the same as that of the thermosetting composition used in the measurement of the calorific value Q2. If it is assumed that the semi-cured material contains c (mass %) of a thermosetting component, the curing rate of the thermosetting composition impregnated in the composite is calculated by the following formula (B).
[0062] Curing rate of impregnated semi-cured product (%) = {1-[(R2 / c)×100] / Q2}×100···(B)
[0063] For the content of the above-mentioned semi-cured material, the composite is used as a reference, for example, it can be 20% by volume or more, 25% by volume or more, 30% by volume or more, 35% by volume or more, or 40% by volume or more. When the content of the thermosetting composition is within the above range, the adhesion when bonding to the adherend by heating and pressurizing can be further improved. Taking the composite as a reference, the content of the above-mentioned thermosetting composition can be, for example, 70% by volume or less, 65% by volume or less, 60% by volume or less, or 55% by volume or less. When the content of the thermosetting composition is within the above range, it is possible to have both adhesion and insulation of the composite at a higher level. The content of the thermosetting composition can be adjusted within the above range, for example, it can be 20 to 70% by volume. The semi-cured material is volatilized by heating the resin composite at about 600°C, and the weight difference before and after is measured, thereby obtaining the content of the semi-cured material.
[0064] The content of the thermosetting composition in the composite can be regarded as the porosity of the nitride sintered body and can be calculated by the following formula (C). The true density of the nitride sintered body is 2.28 g / cm2 in the case of boron nitride, for example. 3 .
[0065] Content of thermosetting composition [volume %] = porosity of nitride sintered body = [1-(D / true density of nitride sintered body]...(C)
[0066] In the above formula (C), D means the bulk density of the nitride sintered body represented by the following formula (D).
[0067] Bulk density of nitride sintered body [g / cm 3 ] = mass of nitride sintered body / volume of nitride sintered body (D)
[0068] In the above formula (C), the true density of the nitride sintered body refers to the value calculated by multiplying the true density of each nitride by the respective mixing ratio (mass ratio) when the nitride sintered body is a substance obtained from a plurality of nitrides. For example, when nitride A and nitride B are mixed at a mass ratio of a:b, the true density of the nitride sintered body is obtained by the following formula (D).
[0069] True density of nitride sintered body [g / cm 3 ]=(A×a+B×b)÷(a+b)···(D)
[0070] The composite sheet 10 can be manufactured, for example, by the manufacturing method described below. One embodiment of the manufacturing method of the composite sheet includes the following steps: using a wire saw, under the conditions of a wire reciprocating speed of 155 to 1000 m / min and a table moving speed of 4 mm / min or less, a resin impregnation body having a nitride sintered body with a porous structure and a semi-cured product of a thermosetting resin composition impregnated in the nitride sintered body is cut to obtain a composite sheet. According to the manufacturing method of the composite sheet, the line roughness Rz (maximum height) of at least one main surface of the composite sheet as specified in JIS B 0601:2013 can be set to 10 μm or less.
[0071] Regarding the resin impregnation body having a nitride sintered body with a porous structure and a semi-cured body of a thermosetting resin composition impregnated in the above-mentioned nitride sintered body, a pre-prepared one can be used, and another one can be prepared separately and used. The method for preparing the resin impregnation body includes, for example, a step of impregnating the nitride sintered body with a porous structure with a thermosetting composition (hereinafter, also referred to as an impregnation step), and a step of heating the above-mentioned thermosetting composition to a heating temperature of 80 to 130°C to semi-cure it (hereinafter, also referred to as a semi-curing step). The above-mentioned impregnation step is a step of setting the temperature of the thermosetting composition to a temperature higher than the above-mentioned heating temperature in the above-mentioned semi-curing step and to a temperature lower than the above-mentioned heating temperature + 20°C, so as to impregnate the thermosetting composition.
[0072] The nitride sintered body having a porous structure may be a material obtained by sintering primary particles of nitride to each other. The nitride sintered body having a porous structure may use a commercially available nitride sintered body or a material prepared by sintering a powder containing nitride. That is, the method for preparing a resin impregnated body may further include a step of sintering a powder containing nitride (hereinafter, also referred to as nitride powder) to obtain a nitride sintered body having a porous structure. For the nitride sintered body, a slurry containing nitride powder may be spheroidized using a spray dryer or the like, and then sintered after further molding to prepare a nitride sintered body having a porous structure. During molding, a mold may be used, or a cold isostatic pressing (CIP) method may be employed.
[0073] The nitride may contain, for example, at least one nitride selected from the group consisting of boron nitride, aluminum nitride, and silicon nitride, preferably boron nitride. Boron nitride may be any of amorphous boron nitride and hexagonal boron nitride. The thermal conductivity of the nitride may be, for example, 40 W / (m·K) or more, 50 W / (m·K) or more, or 60 W / (m·K) or more. By using a nitride having excellent thermal conductivity as described above as a nitride, the thermal resistance of the obtained resin impregnation and the composite sheet cut from the resin impregnation can be further reduced.
[0074] During the sintering of the nitride powder, a sintering aid may also be used. The sintering aid may be, for example, oxides of rare earth elements such as yttrium oxide, aluminum oxide and magnesium oxide, carbonates of alkali metals such as lithium carbonate and sodium carbonate, and boric acid. In the case of a sintering aid, the amount of the sintering aid added may be, for example, more than 0.01 parts by mass or more than 0.1 parts by mass relative to a total of 100 parts by mass of the nitride and the sintering aid. The amount of the sintering aid added may be, for example, less than 20 parts by mass, less than 15 parts by mass or less than 10 parts by mass relative to a total of 100 parts by mass of the nitride and the sintering aid. By setting the amount of the sintering aid added to the above range, it becomes easy to adjust the average pore diameter of the nitride sintered body to the above range.
[0075] The sintering temperature of the nitride may be, for example, 1600° C. or 1700° C. or more. The sintering temperature of the nitride may be, for example, 2200° C. or less or 2000° C. or less. The sintering time of the nitride may be, for example, 1 hour or more, or 30 hours or less. The atmosphere during sintering may be, for example, an inert gas atmosphere such as nitrogen, helium, or argon.
[0076] For sintering, for example, a batch furnace and a continuous furnace can be used. Examples of the batch furnace include a muffle furnace, a tubular furnace, and an atmosphere furnace. Examples of the continuous furnace include a rotary furnace, a screw conveyor furnace, a tunnel furnace, a belt furnace, a pusher furnace, and a machinist continuous furnace.
[0077] In the impregnation step, a solution containing a thermosetting composition is prepared in an impregnation device, and the nitride sintered body is immersed in the solution, so that the thermosetting composition is impregnated into the pores of the nitride sintered body. The solution containing the thermosetting composition may contain a solvent in addition to the thermosetting composition, or may be only the thermosetting composition. Examples of the solvent include aliphatic alcohols, ether alcohols, glycol ethers, ketones, and hydrocarbons.
[0078] The thermosetting composition contains at least one compound selected from the group consisting of compounds having a cyanate group, compounds having a bismaleimide group and compounds having an epoxy group, and at least one curing agent selected from the group consisting of phosphine-based curing agents and imidazole-based curing agents.
[0079] Examples of the compound having a cyanate group include dimethylmethylenebis(1,4-phenylene)dicyanate and bis(4-cyanatephenyl)methane. Dimethylmethylenebis(1,4-phenylene)dicyanate is commercially available as TACN (trade name, manufactured by Mitsubishi Gas Chemical Company, Inc.).
[0080] Examples of compounds having a bismaleimide group include N,N'-[(1-methylethylene)bis[(p-phenylene)oxy(p-phenylene)]]bismaleimide and 4,4'-diphenylmethanebismaleimide. N,N'-[(1-methylethylene)bis[(p-phenylene)oxy(p-phenylene)]]bismaleimide is commercially available as, for example, BMI-80 (trade name, manufactured by KI Chemicals Co., Ltd.).
[0081] Examples of compounds having an epoxy group include 1,6-bis(2,3-epoxypropane-1-yloxy)naphthalene and compounds represented by the following general formula (3). In the general formula (3), the value of n is not particularly limited and may be an integer greater than 0 or 1, and is usually 1 to 10, preferably 2 to 5. 1,6-bis(2,3-epoxypropane-1-yloxy)naphthalene is commercially available, for example, as HP-4032D (manufactured by DIC Corporation, trade name).
[0082] [Chemical formula 3]
[0083]
[0084] In the thermosetting composition, the total amount of the compound having a cyanate group, the compound having a bismaleimide group and the compound having an epoxy group can be 50% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more, based on the total amount of the thermosetting composition.
[0085] The content of the compound having a cyanate group in the thermosetting composition may be, for example, 50 parts by mass or more, 60 parts by mass or more, or 70 parts by mass or more relative to 100 parts by mass of the total amount of the compound having a cyanate group and the compound having a bismaleimide group. When the content of the compound having a cyanate group in the thermosetting composition is within the above range, the curing reaction when the composite sheet cut out from the obtained resin impregnation body is bonded to an adherend including a metal substrate proceeds rapidly, and the insulation after bonding to the adherend can be further improved.
[0086] The content of the compound having a bismaleimide group in the thermosetting composition may be, for example, 15 parts by mass or more, 20 parts by mass or more, or 25 parts by mass or more relative to 100 parts by mass of the total amount of the compound having a cyanate group and the compound having a bismaleimide group. If the content of the compound having a bismaleimide group in the thermosetting composition is within the above range, the water absorption of the semi-cured product is reduced, and the reliability of the product can be improved.
[0087] The content of the compound having an epoxy group in the thermosetting composition may be, for example, 10 parts by mass or more, 20 parts by mass or more, or 30 parts by mass or more relative to 100 parts by mass of the total amount of the compound having a cyanate group and the compound having a bismaleimide group. The content of the compound having an epoxy group in the thermosetting composition may be, for example, 70 parts by mass or less, or 60 parts by mass or less relative to 100 parts by mass of the total amount of the compound having a cyanate group and the compound having a bismaleimide group. If the content of the compound having an epoxy group in the thermosetting composition is within the above range, the decrease in the thermal curing starting temperature of the thermosetting composition can be suppressed, making it easier to impregnate the thermosetting composition into the nitride sintered body.
[0088] The curing agent may further contain a phosphine-based curing agent and an imidazole-based curing agent.
[0089] The phosphine curing agent promotes the triazine formation reaction based on the trimerization of the compound having a cyanate group or the cyanate resin. As the phosphine curing agent, for example, tetraphenylphosphine tetra-p-tolyl boronate and tetraphenylphosphine tetraphenyl boronate can be cited. Tetraphenylphosphine tetra-p-tolyl boronate can be commercially obtained as TPP-MK (manufactured by Hokko Chemical Industry Co., Ltd., trade name).
[0090] Imidazole curing agents generate oxazoline, which promotes the curing reaction of compounds or epoxy resins having epoxy groups. As imidazole curing agents, for example, 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole and 2-ethyl-4-methylimidazole can be cited. 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole can be commercially obtained as 2E4MZ-CN (manufactured by Shikoku Chemical Industry Co., Ltd., trade name).
[0091] The content of the phosphine curing agent may be, for example, 5 parts by mass or less, 4 parts by mass or less, or 3 parts by mass or less, relative to 100 parts by mass of the total amount of the compound having a cyanate group, the compound having a bismaleimide group, and the compound having an epoxy group. The content of the phosphine curing agent may be, for example, 0.1 parts by mass or more, or 0.5 parts by mass or more, relative to 100 parts by mass of the total amount of the compound having a cyanate group, the compound having a bismaleimide group, and the compound having an epoxy group. When the content of the phosphine curing agent is within the above range, the preparation of the resin impregnation is easy, and the time required for the composite sheet cut out from the resin impregnation to be bonded to the adherend can be further shortened.
[0092] For example, the content of the imidazole curing agent can be less than 0.1 mass part, less than 0.05 mass part, or less than 0.03 mass part relative to the total amount of 100 mass parts of the compound having a cyanate group, the compound having a bismaleimide group, and the compound having an epoxy group. For example, the content of the imidazole curing agent can be more than 0.001 mass part or more than 0.005 mass part relative to the total amount of 100 mass parts of the compound having a cyanate group, the compound having a bismaleimide group, and the compound having an epoxy group. When the content of the imidazole curing agent is within the above range, the preparation of the resin impregnation body is easy, and the time required for bonding to the adherend when using a composite sheet cut out from the resin impregnation body can be further shortened.
[0093] The thermosetting composition may include a compound having a cyanate group, a compound having a bismaleimide group, a compound having an epoxy group, a curing agent, and other components. As other components, for example, other resins such as phenolic resin, melamine resin, urea-formaldehyde resin, and alkyd resin, silane coupling agent, leveling agent, defoamer, surface conditioner, and wetting dispersant may also be included. The content of these other components is based on the total amount of the thermosetting composition, for example, 20% by mass or less, 10% by mass or less, or 5% by mass or less.
[0094] The viscosity of the solution containing the above-mentioned thermosetting composition at 100°C can be, for example, 50 mPa·seconds or less, 30 mPa·seconds or less, 20 mPa·seconds or less, 10 mPa·seconds or less, or 5 mPa·seconds. If the viscosity of the solution at 150°C is within the above-mentioned range, the preparation of the resin impregnation body becomes easier. The viscosity of the above-mentioned solution at 100°C can be 3 mPa·seconds or more. With regard to the viscosity of the above-mentioned solution at 100°C, it is preferred to maintain it at 50 mPa·seconds or less for more than 5 hours while maintaining the temperature of the solution at 100°C. The viscosity of the above-mentioned solution at 100°C refers to a value measured using a rotational viscometer at a shear rate of 10 (1 / second).
[0095] The impregnation process may be carried out under any conditions of reduced pressure or pressurized conditions, or the impregnation under reduced pressure and the impregnation under pressurized conditions may be carried out in combination. The pressure in the impregnation device when the impregnation process is carried out under reduced pressure may be, for example, 1000 Pa or less, 500 Pa or less, 100 Pa or less, 50 Pa or less, or 20 Pa or less. The pressure in the impregnation device when the impregnation process is carried out under pressurized conditions may be, for example, 1 MPa or more, 3 MPa or more, 10 MPa or more, or 30 MPa or more.
[0096] In the impregnation process, the solution containing the thermosetting composition is heated. By heating the above solution in the following temperature range, the viscosity of the solution can be adjusted and the impregnation of the resin can be promoted, thereby obtaining an excellent resin impregnation body. The temperature of heating the above solution is higher than the heating temperature for semi-curing. The upper limit of the temperature of heating the above solution is a temperature below the heating temperature for semi-curing + 20°C.
[0097] In the impregnation step, the nitride sintered body is kept immersed in the solution containing the thermosetting composition for a predetermined time, which may be, for example, 5 hours or more, 10 hours or more, 100 hours or more, or 150 hours or more.
[0098] The semi-curing step is a step of heating the thermosetting composition impregnated in the nitride sintered body to semi-cure it. The semi-curing step can adjust the semi-cured state of the thermosetting composition in the resin impregnation body. The heating temperature at this time is 80 to 130°C.
[0099] The semi-cured material obtained by the semi-curing process can contain at least one thermosetting resin and a curing agent selected from the group consisting of cyanate resin, bismaleimide resin and epoxy resin. The semi-cured material, in addition to the above-mentioned thermosetting resin and curing agent, can also contain other resins such as phenolic resin, melamine resin, urea-formaldehyde resin and alkyd resin and components from silane coupling agent, leveling agent, defoamer, surface conditioner and wetting dispersant. The total content of these other resins and this component can be, for example, less than 20% by mass, less than 10% by mass, or less than 5% by mass based on the semi-cured material total amount.
[0100] The composite sheet can be prepared by cutting the resin-impregnated body with a wire saw (for example, a multi-cut wire saw). Figure 3 This is a schematic diagram showing an example of a method for producing a composite sheet. Figure 3The present invention is a schematic diagram of the device structure when the resin impregnation body 100 is cut by a multi-cut wire saw 500 to prepare a composite sheet. The multi-cut wire saw 500 may include a first roller 22, a second roller 24, and a third roller 26, a steel wire 30 supported by the three rollers, and a supply nozzle 42 for supplying a slurry-like polishing liquid to the steel wire 30. The steel wire 30 is supported by the first roller 22, the second roller 24, and the third roller 26, and moves at a predetermined reciprocating speed, wrapping the polishing liquid supplied from the supply nozzle 42 to gradually cut the resin impregnation body 100. The resin impregnation body 100 is placed on a movable worktable (not shown) and is lifted by the worktable that gradually rises as the steel wire 30 is cut, and as a result, the resin impregnation body 100 is cut to prepare a plurality of composite sheets.
[0101] The lower limit of the reciprocating speed of the wire of the wire saw is 155 m / min or more, for example, it can be 200 m / min or more, 300 m / min or more, 400 m / min or more, or 500 m / min or more. By setting the lower limit of the reciprocating speed of the wire to the above range, the occurrence of wire breakage and wire relaxation can be suppressed, and the resin impregnation body can be cut more stably. The upper limit of the reciprocating speed of the wire of the wire saw is 1000 m / min or less, for example, it can be 950 m / min or less, 900 m / min or less, 800 m / min or less, 700 m / min or less, or 600 m / min or less. By setting the upper limit of the reciprocating speed of the wire to the above range, the line roughness Rz and the arithmetic mean roughness Ra of the main surface of the obtained composite sheet can be further reduced. The reciprocating speed of the wire can be adjusted within the above range, for example, it can be 155 to 1000 m / min, or 400 to 900 m / min.
[0102] The table moving speed of the wire saw is related to the penetration speed of the wire saw into the resin impregnation body that is the cutting object of the wire saw. The upper limit of the table moving speed of the wire saw is 4 mm / min or less, for example, it can be 3 mm / min or less, 2 mm / min or less, or 1.5 mm / min or less. By setting the table moving speed within the above range, the line roughness Rz and the arithmetic mean roughness Ra of the main surface of the obtained composite sheet can be made smaller. The lower limit of the table moving speed of the wire saw can be, for example, 0.1 mm / min or more, 0.3 mm / min or more, or 0.5 mm / min or more. By setting the lower limit of the table moving speed of the wire saw within the above range, the line roughness Rz and the arithmetic mean roughness Ra of the main surface of the obtained composite sheet can be made smaller, and productivity can be maintained at a high level. The table moving speed can also be adjusted within the above range according to the relationship with the reciprocating wire speed of the wire, for example, it can be 0.5 to 4 mm / min, or 0.5 to 2 mm / min.
[0103] The size of the resin impregnation body may also be adjusted before being cut by the wire saw. The lower limit of the width of the resin impregnation body may be, for example, 5 mm or more, 10 mm or more, or 50 mm or more. By setting the lower limit of the width to the above range, vibration of the resin impregnation body during cutting can be suppressed, and the line roughness Rz and the arithmetic mean roughness Ra can be made smaller. The upper limit of the width of the resin impregnation body may be, for example, 150 mm or less, 120 mm or less, or 110 mm or less. By setting the upper limit of the width to the above range, the contact distance between the resin impregnation body and the steel wire can be reduced, and the line roughness Rz and the arithmetic mean roughness Ra of the main surface of the obtained composite sheet can be made smaller. The width of the resin impregnation body may be adjusted within the above range, for example, 5 to 150 mm.
[0104] The composite sheet can be used, for example, for the manufacture of a laminate such as a thermally conductive adhesive sheet. One embodiment of the laminate comprises: a first metal substrate, an intermediate layer provided on the first metal substrate, and a second metal substrate provided on the side of the intermediate layer opposite to the first metal substrate. Here, the first metal substrate and the second metal substrate are connected via the intermediate layer, and the intermediate layer is a cured product of the composite sheet.
[0105] Figure 4 The laminate 300 includes the composite sheet 10 , a first metal substrate 52 provided on one main surface of the composite sheet 10 , and a second metal substrate 53 provided on the other main surface of the composite sheet 10 .
[0106] The thickness of the first metal substrate 52 and the second metal substrate 53 may be, for example, independently 0.035 mm or more, or 10 mm or less. The first metal substrate 52 and the second metal substrate 53 may form a circuit, for example.
[0107] The first metal substrate 52 and the second metal substrate 53 may be the same metal substrate or different metal substrates. The first metal substrate 52 and the second metal substrate 53 may include at least one selected from the group consisting of copper and aluminum, and may be copper or aluminum. The first metal substrate 52 and the second metal substrate 53 may also include metals other than copper and aluminum.
[0108] In the case of conventional composite sheets, the Rz of the main surface of the composite sheet is large, so the heat dissipation of the laminate may vary. It is speculated that this is because the thickness of the resin layer, which is a cured product of the thermosetting resin composition from the composite sheet, varies in the in-plane direction of the interface between the metal substrate and the main surface of the composite sheet when laminated with the metal substrate. Figure 5 This is a partial cross-sectional view of a laminate obtained using a conventional composite sheet. Figure 5 As shown, since the Rz etc. of the main surface of the conventional composite sheet 110 is large, the resin layer 130 having different thicknesses at different positions exists at the interface between the conventional composite sheet 110 and the metal substrate 150. Therefore, the inventors of the present application presume that there is a deviation in thermal diffusion.
[0109] The laminate of the present invention includes the composite sheet 10, and thus can suppress the deviation of heat dissipation in the in-plane direction of the interface between the composite sheet 10 and at least one of the first metal substrate 52 and the second metal substrate 53. This is because the thickness difference of the resin layer from the composite sheet 10 is reduced.
[0110] The laminated body can be manufactured, for example, by the following method. One embodiment of the method for manufacturing the laminated body includes the following steps: arranging and stacking a first metal substrate and a second metal substrate respectively in a manner facing a pair of main surfaces of the composite sheet, heating the first metal substrate and the second metal substrate while being pressurized in a stacking direction to cure the thermosetting resin composition, thereby connecting the composite sheet to the first metal substrate and the second metal substrate.
[0111] In the method for producing the laminate, the composite body is used, so that the first metal substrate and the second metal substrate can be bonded to each other in a short time. The bonding time can be set to 2 hours or less, 1 hour or less, or 0.5 hours or less.
[0112] Although some embodiments have been described above, the descriptions of the common configurations can be applied to each other. In addition, the present invention is not limited to the above-described embodiments at all.
[0113] Example
[0114] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples. The present invention is not limited to the following Examples.
[0115] (Example 1)
[0116] [Production of Boron Nitride Sintered Body]
[0117] 40.0% by mass of amorphous boron nitride powder (produced by Denka Corporation, oxygen content: 1.5%, boron nitride purity: 97.6%, average particle size: 6.0 μm) and 60.0% by mass of hexagonal boron nitride powder (produced by Denka Corporation, oxygen content: 0.3%, boron nitride purity: 99.0%, average particle size: 30.0 μm) were weighed into a container respectively, and after adding sintering aids (boric acid, calcium carbonate), an organic binder and water were added for mixing, and then dried and granulated to adjust the mixed powder of nitride.
[0118] The mixed powder is filled in a cold isostatic pressing (CIP) device (manufactured by Kobe Steel, Ltd., trade name: ADW800), and a pressure of 20 to 100 MPa is applied to the mixed powder to compress it, thereby obtaining a molded body. A batch-type high-frequency furnace (manufactured by Fuji Electric Industry Co., Ltd., trade name: FTH-300-1H) is used to sinter the obtained molded body at 2000°C for 10 hours, thereby preparing a nitride sintered body. It should be noted that while nitrogen is allowed to flow in the furnace at a flow rate of 10 L / min in a standard state, the furnace is adjusted to a nitrogen atmosphere for sintering. The average pore size of the obtained boron nitride sintered body is 5 μm, and the porosity is 50% by volume.
[0119] <Measurement of average pore diameter>
[0120] The obtained boron nitride sintered body was subjected to a mercury porosimeter (manufactured by Shimadzu Corporation) while increasing the pressure from 0.03 atmospheres to 4000 atmospheres, and the pore size distribution (horizontal axis: pore size, vertical axis: cumulative pore volume) during pressurization was measured. The average pore size was calculated from the pore size distribution as the pore size at which the cumulative pore volume reached 50% of the total pore volume.
[0121] <Measurement of porosity>
[0122] The volume and mass of the obtained boron nitride sintered body were measured, and the bulk density (D; g / cm 3 ). The bulk density and the theoretical density of boron nitride (2.28 g / cm 3 ), and the porosity is calculated according to the following formula:
[0123] Porosity (volume %) = [1-(D / 2.28)]×100.
[0124] [Impregnation of resin composition]
[0125] 80 parts by mass of a compound having a cyanate group, 20 parts by mass of a compound having a bismaleimide group, and 50 parts by mass of a compound having an epoxy group were weighed in a container, and 1 part by mass of a phosphine curing agent and 0.01 part by mass of an imidazole curing agent were added to and mixed with respect to the total amount of 100 parts by mass of the above three compounds, thereby preparing a thermosetting composition. It should be noted that since the epoxy resin is in a solid state at room temperature, the mixing is performed in a state heated to about 80°C. The viscosity of the obtained thermosetting composition at 100°C is 10 mPa·second.
[0126] The following compounds were used in the preparation of the thermosetting composition.
[0127] <Compounds with specific functional groups>
[0128] Compound having a cyanate group: dimethylmethylenebis(1,4-phenylene)dicyanate (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name: TA-CN)
[0129] Compound having a bismaleimide group: N,N'-[(1-methylethylene)bis[(p-phenylene)oxy(p-phenylene)]]bismaleimide (manufactured by KI Chemicals Co., Ltd., trade name: BMI-80)
[0130] Compound having an epoxy group: 1,6-bis(2,3-epoxypropane-1-yloxy)naphthalene (manufactured by DIC Corporation, trade name: HP-4032D)
[0131] Compound having a benzoxazine group: Bisphenol F type benzoxazine (manufactured by Shikoku Chemical Industry Co., Ltd., trade name: Fa type benzoxazine)
[0132] <Curing agent>
[0133] Phosphine-based curing agent: tetraphenylphosphine tetra-p-tolyl boronate (manufactured by Chemical Industry Co., Ltd., trade name: TPP-MK)
[0134] Imidazole curing agent: 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole (manufactured by Shikoku Chemicals Co., Ltd., trade name: 2E4MZ-CN)
[0135] Metal catalyst: Zinc(II) bis(2,4-pentanedionate) (Tokyo Chemical Industry Co., Ltd.)
[0136] The thermosetting composition prepared as described above is impregnated into the nitride sintered body prepared as described above by the following method. First, the nitride sintered body and the thermosetting composition in a container are placed in a vacuum heating impregnation device (manufactured by Kyosin Engineering Corporation, trade name: G-555AT-R). Next, the inside of the device is degassed for 10 minutes under the conditions of temperature: 100°C and pressure: 15 Pa. After degassing, the nitride sintered body is immersed in the thermosetting composition for 40 minutes while maintaining the conditions, so that the thermosetting composition is impregnated into the nitride sintered body.
[0137] After that, the container containing the above-mentioned nitride sintered body and thermosetting composition was taken out and placed in a pressurized heating impregnation device (manufactured by Kyosin Engineering Corporation, trade name: HP-4030AA-H45), and kept at a temperature of 130°C and a pressure of 3.5 MPa for 120 minutes, thereby impregnating the nitride sintered body with the thermosetting composition. After that, the nitride sintered body was taken out from the device, and heated at a temperature of 120°C and atmospheric pressure for 8 hours to semi-cure the thermosetting composition, thereby preparing a boron nitride sintered body (resin impregnation body) filled with resin. The content of the semi-cured material in the obtained resin impregnation body was 50% by volume. The dimensions of the obtained composite resin impregnation body were vertical (length): 50 mm, horizontal (width): 50 mm, and height (thickness): 50 mm.
[0138] <Determination of content of resin (semi-cured product)>
[0139] The content of the resin in the obtained composite was measured by the following procedure. The content (volume %) of the resin in the resin impregnation was determined by measuring the bulk density of the boron nitride sintered body and the bulk density of the composite shown below.
[0140] Resin content in resin impregnation (%) = ((bulk density of resin impregnation - bulk density of boron nitride sintered body) / (theoretical density of composite - bulk density of boron nitride sintered body)) × 100
[0141] In addition, the theoretical density of the complex is a value calculated by the following formula.
[0142] Theoretical density of composite body = true density of boron nitride + true density of resin × (1-bucking density of boron nitride sintered body / true density of boron nitride)
[0143] The bulk density of the boron nitride sintered body and the resin impregnated body is determined based on the volume calculated from the length of each side of the boron nitride sintered body or composite body in the shape of a regular hexahedron (measured by a vernier caliper) according to the "Determination method of density and specific gravity based on geometric measurement" of JIS Z 8807:2012, and the mass of the boron nitride sintered body or composite body measured by an electronic balance (see Article 9 of JIS Z 8807:2012). The true density of the boron nitride sintered body and the resin is calculated from the volume and mass of the boron nitride sintered body and the resin measured using a dry automatic density meter according to the "Determination method of density and specific gravity based on gas replacement method" of JIS Z 8807:2012 (see Formulas (14) to (17) of Article 11 of JIS Z 8807:2012).
[0144] [Preparation of composite sheet: Cutting out composite sheet from resin impregnation body]
[0145] The resin impregnation body prepared as described above is set on the workbench of a multi-cut wire saw, and a plurality of composite sheets are prepared by using the multi-cut wire saw under the conditions described in Table 1. The conditions of the multi-cut wire saw are adjusted as described in Table 1. In Table 1, the wire reciprocating linear speed (unit: m / min) refers to the working speed of the wire, the workbench moving speed (unit: mm / min) refers to the rising speed of the workbench, and the sample width (unit: mm) refers to the width of the resin impregnation body to be cut. The thickness of the obtained composite sheet is 0.40 mm.
[0146] (Comparative Example 1)
[0147] A composite sheet was prepared in the same manner as in Example 1 except that the wire reciprocating speed of the multi-cut wire saw was changed to 150 m / min. The thickness of the obtained composite sheet was 0.41 mm.
[0148] <Evaluation 1 of composite sheet: Line roughness Rz (maximum height) and arithmetic mean roughness Ra>
[0149] The composite sheets obtained in Example 1 and Comparative Example 1 were measured for the line roughness Rz and the arithmetic mean roughness Ra of the processed surface (based on the cut section of the multi-cut wire). The line roughness Rz and the arithmetic mean roughness Ra were measured in accordance with JIS B 0601:2013 "Geometric properties of products (GPS) - Surface properties: Profile curve method - Terms, definitions and surface property parameters". The results are shown in Table 1.
[0150] <Evaluation of composite sheet 2: Thermal resistance and heat dissipation>
[0151] Regarding the composite sheet obtained in Example 1 and Comparative Example 1, the above-mentioned composite is arranged between two copper plates, heated and pressurized at 200°C and 10MPa for 5 minutes, and then heated at 200°C and atmospheric pressure for 2 hours to prepare a laminated body, which is used as a measurement object. The thermal resistance is measured in accordance with ASTM-D5470. The thermal resistance (unit: K / W) of the laminated body prepared using the composite sheet obtained in Comparative Example 1 is used as a benchmark to evaluate the thermal resistance of the laminated body prepared using the composite sheet obtained in Example 1. In addition, the heat dissipation of the above-mentioned laminated body is evaluated using the following benchmarks. The results are shown in Table 1.
[0152] A: When the value of Comparative Example 1 is set to 1, the thermal resistance is less than 0.8.
[0153] B: When the value of Comparative Example 1 is set to 1, the thermal resistance is 0.8 or more and less than 1.
[0154] C: When the value of Comparative Example 1 is set to 1, the thermal resistance is 1 or more.
[0155] [Table 1]
[0156] In Table 1, in the item of whether or not it can be cut, "A" indicates that the composite can be cut from the resin impregnation body in a sheet shape (a composite sheet can be prepared), and "B" indicates that the composite cannot be cut from the resin impregnation body in a sheet shape (a composite sheet cannot be prepared). The same is true in Tables 2 and 3.
[0157] (Example 2)
[0158] The composite sheet was prepared in the same manner as in Example 1 except that the wire reciprocating speed of the multi-cut wire saw was changed to 900 m / min. The thickness of the obtained composite sheet was 0.41 mm. The line roughness Rz (maximum height) and the arithmetic mean roughness Ra were measured for the obtained composite sheet, and the thermal resistance and heat dissipation were evaluated. The results are shown in Table 2.
[0159] (Example 3)
[0160] The composite sheet was prepared in the same manner as in Example 1 except that the wire reciprocating speed of the multi-cut wire saw was changed to 500 m / min and the table moving speed was changed to 0.1 mm / min. The thickness of the obtained composite sheet was 0.39 mm. The line roughness Rz (maximum height) and the arithmetic mean roughness Ra were measured for the obtained composite sheet, and the thermal resistance and heat dissipation were evaluated. The results are shown in Table 2.
[0161] (Example 3)
[0162] The composite sheet was prepared in the same manner as in Example 1 except that the wire reciprocating speed of the multi-cut wire saw was changed to 500 m / min and the table moving speed was changed to 2 mm / min. The thickness of the obtained composite sheet was 0.40 mm. The line roughness Rz (maximum height) and the arithmetic mean roughness Ra were measured for the obtained composite sheet, and the thermal resistance and heat dissipation were evaluated. The results are shown in Table 2.
[0163] (Example 4)
[0164] The composite sheet was prepared in the same manner as in Example 1 except that the wire reciprocating speed of the multi-cut wire saw was changed to 500 m / min and the sample width was changed to 10 mm. The thickness of the obtained composite sheet was 0.41 mm. The line roughness Rz (maximum height) and the arithmetic mean roughness Ra were measured for the obtained composite sheet, and the thermal resistance and heat dissipation were evaluated. The results are shown in Table 2.
[0165] (Example 2)
[0166] The composite sheet was prepared in the same manner as in Example 1 except that the wire reciprocating speed of the multi-cut wire saw was changed to 500 m / min and the sample width was changed to 120 mm. The thickness of the obtained composite sheet was 0.40 mm. The line roughness Rz (maximum height) and the arithmetic mean roughness Ra were measured for the obtained composite sheet, and the thermal resistance and heat dissipation were evaluated. The results are shown in Table 2.
[0167] [Table 2]
[0168]
[0169] (Comparative Example 2)
[0170] The composite sheet was prepared in the same manner as in Example 1 except that the wire reciprocating speed of the multi-cut wire saw was changed to 1200 m / min. The thickness of the obtained composite sheet was 0.40 mm. The line roughness Rz (maximum height) and arithmetic mean roughness Ra were measured for the obtained composite sheet, and the thermal resistance and heat dissipation were evaluated. The results are shown in Table 3.
[0171] (Comparative Example 3)
[0172] The preparation of the composite sheet was attempted in the same manner as in Example 1 except that the wire reciprocating speed of the multi-cut wire saw was changed to 500 m / min and the table moving speed was changed to 5 mm / min, but the composite could not be cut from the resin impregnated body in a sheet form. The results are shown in Table 3. It should be noted that in Table 3, "-" means that the measurement was not performed.
[0173] [Table 3]
[0174]
[0175] Industrial Applicability
[0176] According to the present invention, a composite sheet having excellent heat dissipation when laminated with a metal substrate and a method for producing the same can be provided. According to the present invention, a laminate having excellent heat dissipation and a method for producing the same can also be provided.
[0177] Description of Reference Numerals
[0178] 10, 110...composite sheet, 10a, 10b...main surface, 30...steel wire, 52...first metal substrate, 53...second metal substrate, 100...resin impregnation body, 130...resin layer, 150...metal substrate, 300...laminated body, 500...multi-cut wire saw.
Claims
1. A composite sheet comprising: a nitride sintered body having a porous structure; and a semi-cured body of a thermosetting resin composition impregnated in the nitride sintered body. The linear roughness Rz of at least one main surface of the composite sheet as defined in JIS B 0601:2013 is 10 μm or less.
2. The composite sheet according to claim 1, in, The arithmetic mean roughness Ra of the main surface specified in JIS B0601:2013 is 2.0 μm or less.
3. The composite sheet according to claim 1 or 2, in, The content of the semi-cured material is 20 to 70 volume %.
4. The composite sheet according to claim 1 or 2, which has a thickness of 1.0 mm or less. The composite sheet according to claim 3 , which has a thickness of 1.0 mm or less.
6. A method for producing a composite sheet, wherein include: A process of cutting a resin impregnation body comprising a nitride sintered body having a porous structure and a semi-cured body of a thermosetting resin composition impregnated in the nitride sintered body using a wire saw at a wire reciprocating speed of 155 to 1000 m / min and a table moving speed of 4 mm / min or less to obtain a composite sheet, The linear roughness Rz of at least one main surface of the composite sheet as defined in JIS B 0601:2013 is 10 μm or less.
7. The manufacturing method according to claim 6, in, The width of the resin impregnation body is 5 to 150 mm.
8. A laminate comprising a first metal substrate, an intermediate layer provided on the first metal substrate, and a second metal substrate provided on the side of the intermediate layer opposite to the first metal substrate side, in, The first metal substrate and the second metal substrate are connected through the intermediate layer. The intermediate layer is a cured product of the composite sheet according to any one of claims 1 to 5.
9. The laminate according to claim 8, in, The line roughness Rz of the main surface on the intermediate layer side of the first metal substrate and the second metal substrate as specified in JIS B 0601:2013 is 10 μm or less.
10. The laminate according to claim 8 or 9, in, At least one of the first metal substrate and the second metal substrate includes at least one selected from the group consisting of copper and aluminum.
11. A method for producing a laminate, comprising the following steps: A first metal substrate and a second metal substrate are respectively arranged and stacked in a manner opposite to a pair of main surfaces of the composite sheet described in any one of claims 1 to 5, and the first metal substrate and the second metal substrate are heated while being pressurized in the stacking direction to cure the thermosetting resin composition, thereby connecting the composite sheet to the first metal substrate and the second metal substrate.