Apple-derived activated carbon material and preparation method thereof

By using apple-derived activated carbon materials, the problem of precious metal catalyst resource shortage and high cost has been solved, and low-cost electrocatalytic electrode materials suitable for mass production have been achieved, demonstrating excellent electrochemical energy storage performance and environmentally friendly characteristics. .

CN114477176BInactive Publication Date: 2024-10-29NANJING ZHIHUI ENVIRONMENTAL METEOROLOGICAL IND RES INST CO LTD +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210085039.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-25
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing technology, precious metal catalysts such as platinum electrodes are resource scarce and expensive when used in acidic systems, making them unsuitable for large-scale production, making it difficult to develop efficient and low-cost electrocatalytic electrode materials.

Method used

An apple-derived activated carbon material and its preparation method are used. By soaking, carbonizing and processing apple slices in a zinc chloride solution, an activated carbon material with a hierarchical porous structure is prepared as an alternative electrocatalytic electrode material. .

Benefits of technology

A low-cost, simple and easy preparation method is achieved, with low production cost and suitable for large-scale industrialization. The activated carbon material exhibits excellent electrochemical energy storage performance and environmentally friendly green catalyst characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114477176B_ABST
    Figure CN114477176B_ABST
Patent Text Reader

Abstract

The invention relates to an activated carbon material derived from apples and a preparation method thereof, and belongs to the technical field of environmentally friendly materials. The preparation method is as follows: slice apples as raw materials, add zinc chloride into ethanol and stir until dissolved, soak the apples in ethanol for a period of time and then dry. The dried material is placed in a corundum tube, heated and kept at a constant temperature for a period of time, cooled to room temperature at the same rate, then rinsed with ethanol and distilled water, and then dried. The material is obtained by the preparation method. The preparation method has low cost, high yield, simplicity, convenience in post-reaction treatment, sufficient source of raw materials, and is suitable for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an apple-derived activated carbon material and a preparation method thereof, and belongs to the technical field of environmentally friendly materials. Background Art

[0002] Nowadays, with the continuous development of global science and technology, people's requirements for quality of life and environment are increasing day by day, energy shortage and environmental degradation are becoming increasingly prominent, and the search for renewable clean energy has become the focus of people's attention. However, most renewable resources, such as wind energy, tidal energy, hydropower and thermal energy, are limited to varying degrees by geographical or environmental conditions, and unstable energy output makes them unable to completely replace fossil resources. A green, stable and widely applicable renewable energy has become a major problem.

[0003] Biomass energy is renewable, low-polluting and widely distributed. It is the fourth largest energy source in the world, second only to coal, oil and natural gas. According to estimates by biologists, the earth's land produces 100-125 billion tons of biomass each year; the ocean produces 50 billion tons of biomass each year. The annual production of biomass energy far exceeds the total energy demand of the world, equivalent to 10 times the current total energy consumption of the world. With the development of agriculture and forestry, especially the promotion of charcoal and firewood forests, biomass resources will continue to increase.

[0004] Apple is a genus of plant with high economic value in the Rosaceae family. It is widely distributed in the northern temperate zone and is more common in Northeast my country, North China and Northwest China. China is the main apple supplier in Asia. With its high quality and low price, it is widely exported to Southeast Asia and South Asia, and also exported to America and Europe.

[0005] There are few electrocatalytic electrodes that can be used in acidic systems. The main ones used are precious metal catalysts such as platinum (Pt) electrodes. Due to the shortage and high price of precious metal resources such as platinum, they cannot be used in large-scale production. Therefore, it is urgent to develop electrocatalytic electrode materials with high catalytic performance, mass production and low price. Summary of the invention

[0006] Purpose of the invention: In view of the above existing problems and shortcomings, the purpose of the present invention is to provide an apple-derived activated carbon material and a preparation method thereof. Apple, as a common fruit, makes the preparation method low-cost, simple and easy, with sufficient raw material sources, suitable for large-scale industrial production. Post-reaction treatment is convenient, and it can be washed with ethanol and water.

[0007] Technical solution: To achieve the above-mentioned invention object, the present invention adopts the following technical solution:

[0008] A method for preparing an apple-derived activated carbon material comprises the following steps:

[0009] Step 1: Add 100% anhydrous ethanol to zinc chloride, stir evenly and dissolve to obtain solution a;

[0010] Step 2: Select apples without mildew or black spots, pests, rot, or mechanical damage, slice the apples, and soak them in solution a obtained in step 1, ensuring that the apple slices do not fit each other, soak for 2 to 6 hours, then take them out and dry them at 40 to 80°C;

[0011] Step 3: Place the apple slices dried in step 2 in a corundum tube, pre-flow nitrogen for 25-50 min to exhaust the air inside the tube, perform carbonization reaction on the apple slices, raise the temperature to 720-730°C, and keep the temperature constant for 2-4 hours;

[0012] Step 4: Cool down to room temperature at the same rate as in step 3, rinse with ethanol and distilled water, and then soak in distilled water to test its pH value. When the pH is neutral, take it out, rinse with ethanol and distilled water, and dry it at 40-80℃ to a moisture content of less than 15%.

[0013] Furthermore, in the step 1, 100% anhydrous ethanol is added to the zinc chloride at a material-liquid ratio of 1:14-2:7 g / ml.

[0014] Furthermore, in step 3, the corundum tube is tubular and the heating rate is set to 5°C / min.

[0015] Furthermore, after selecting apples in step 2, the apple core and the apple pulp are separated and then sliced, and in steps 3 and 4, the core slices and the pulp slices are processed separately.

[0016] Furthermore, in step 2, the apple slices are added to solution a at a material-liquid ratio of 3:1 to 2.5:1.

[0017] An apple-derived activated carbon material obtained by the above method.

[0018] Beneficial effects: Compared with the prior art, this is a new type of apple-derived activated carbon material and its preparation method. The present invention has the following advantages: In the present invention, the activated carbon material has the advantages of being stable, environmentally friendly, and free of secondary pollution, and is an ideal green catalyst. The prepared activated carbon material has a multi-level pore structure with a large number of micropores and mesopores evenly distributed, showing excellent electrochemical energy storage performance, and is a good electrode material with broad application prospects. The preparation method is low in cost, high in yield, simple and easy, convenient for post-reaction treatment, and sufficient source of raw materials, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a flow chart of the preparation method of an embodiment of the present invention;

[0020] Figure 2 is an absorbance graph of an embodiment of the present invention;

[0021] Figure 3 is a graph of hydrogen peroxide concentration produced at different times according to an embodiment of the present invention;

[0022] Figure 4 It is a diagram showing the degradation effect of 30 ppm of SMX according to an embodiment of the present invention. DETAILED DESCRIPTION

[0023] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.

[0024] like Figure 1 As shown, an apple-derived activated carbon material and a preparation method thereof, the preparation steps of the embodiment are as follows:

[0025] (1) Add 10 g zinc chloride into 70 mL ethanol and stir until dissolved;

[0026] (2) Soak the apple slices in the solution obtained in (1) for 4 h, and then dry them at 60°C;

[0027] (3) Place the dried material in a corundum tube and heat it to 725°C at a heating rate of 5°C / min in a tube furnace and keep it at this temperature for 2 hours;

[0028] (4) Continue to cool to room temperature at the same rate, rinse with ethanol and distilled water, and bake at 60°C until dry. The activated carbon material of the present invention is obtained.

[0029] The material prepared by the present invention is used as a cathode, and the following experimental method is used to verify its stability and high efficiency.

[0030] 1. Hydrogen peroxide production experiment:

[0031] 100mL ultrapure water was placed in an electrolytic cell and 0.05mol / L sodium sulfate was added as electrolyte. The prepared electrode plate was used as cathode, platinum electrode as anode, and saturated silver chloride electrode as reference electrode. The electrolysis experiment was carried out under the conditions of -0.6v voltage and pH=3. Then, a sample was taken every 15min, and the sampling volume was 4mL for color development. The color development steps were as follows: 0.2, 0.4, 0.6, 0.8, 1.0, and 1.2mL of the prepared hydrogen peroxide standard solution (100mg / L) was calibrated by potassium permanganate method, and 0.5ml of 3.0mol / L sulfuric acid solution and 0.05mol / L potassium titanium oxalate solution were added respectively, and then an appropriate amount of pure water was added to 5ml. Let it stand for 10min.

[0032] Then, at a wavelength of 410 nm, with the reagent blank as a reference, the absorbance data of the experimental samples and the absorbance data of the experimental samples as shown in Table 1 were obtained. Figure 2 The curve diagram shown:

[0033] Table 1

[0034]

[0035] Then through calculation, we get Figure 3 Hydrogen peroxide concentrations of the samples shown.

[0036] 2. Degradation experiment:

[0037] 100 mL of 30 mg / L sulfamethoxazole solution was placed in an electrolytic cell and 0.05 mol / L sodium sulfate was added as an electrolyte. The prepared material was used as the cathode, the platinum electrode was used as the anode, and the saturated silver chloride electrode was used as the reference electrode. Sulfamethoxazole was degraded under an external voltage of -0.6 V. Samples were taken every 15 minutes. After reacting for 1 hour, the concentration of SMX was detected by high performance liquid chromatography (HPLC). Figure 4 The degradation effect diagram of 30ppm SMX was shown on the apple slice carbon material.

[0038] It can be seen that the activated carbon material obtained in the present invention can be used as a cathode for electrocatalysis to obtain hydrogen peroxide, and has an excellent degradation effect on SMX, and is a good electrode material.

Claims

1. A method for preparing an activated carbon material derived from apples, characterized in that: The steps include: Step 1: Add 100% anhydrous ethanol to zinc chloride, stir evenly and dissolve to obtain solution a; Step 2: Select apples without mildew or black spots, pests, rot, or mechanical damage, slice the apples, and soak them in solution a obtained in step 1, ensuring that the apple slices do not fit each other, soak for 2 to 6 hours, then take them out and dry them at 40 to 80°C; Step 3: Place the apple slices dried in step 2 in a corundum tube, pre-flow nitrogen for 25 to 50 minutes to exhaust the air inside, perform carbonization reaction on the apple slices, raise the temperature to 720 to 730°C, and then keep the temperature constant for 2 to 4 hours; Step 4: Cool down to room temperature at the same rate as in step 3, rinse with ethanol and distilled water, and then soak in distilled water to test its pH value. When the pH is neutral, take it out, rinse with ethanol and distilled water, and dry it at 40 ~ 80℃ until the water content is less than 15%; In the step 1, 100% anhydrous ethanol is added to zinc chloride at a material-liquid ratio of 1:14 to 2:7 g / ml; In step 3, the corundum tube is a tubular tube, and the heating rate is set to 5°C / min; After selecting the apples in step 2, the apple core and the apple pulp are separated and then sliced, and in steps 3 and 4, the core slices and the pulp slices are processed separately; In step 2, the apple slices are added to solution a at a material-liquid ratio of 3:1 to 2.5:

1.

2. An apple-derived activated carbon material, characterized in that: It is obtained by the method described in claim 1.

Citation Information

Patent Citations

  • High-specific area activated carbon electrode material and preparation method thereof

    CN109305678A