A wine lees-based fully degradable film, preparation method and application thereof
The preparation of distillers' grains-based fully degradable membranes through the synergistic reaction of distillers' grains and a variety of bio-based raw materials solves the problem of insufficient performance of distillers' grains composite materials in the existing technology, and realizes high-performance, degradable membrane products to meet a variety of application needs, and Achieve complete decomposition under appropriate conditions.
Patent Information
- Application Number
- CN202210259490.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-16
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2042-03-16
AI Technical Summary
In the existing technology, the mechanical properties, water repellency, flame retardancy and other indicators of composite materials converted from distiller's grains are lower than those of petroleum-based plastics, and they are expensive and difficult to meet customer needs, which limits the application and expansion of its downstream products.
The scientific compatibility of distiller's grains, various bio-based raw materials and fully degradable resins is used to prepare distiller's grains-based fully degradable films. By adjusting the proportion of raw materials, it can meet the application indicators of stretch film, food preservation film or shopping bags, and improve the mechanical properties through synergistic reactions. and decomposability.
It has achieved significant optimization in terms of appearance performance, physical and mechanical properties, sealing strength, automatic sterilization, oxygen transmission coefficient, water vapor transmission coefficient, etc. of the distiller's grain-based fully degradable film, and it can be completely decomposed into carbon dioxide and carbon dioxide within 180 days under appropriate conditions. water to improve soil microcirculation.
Smart Images

Figure BDA0003550232290000131 
Figure BDA0003550232290000132 
Figure BDA0003550232290000141
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fully degradable polymers, and in particular relates to a wine lees-based fully degradable film, a preparation method and application thereof. Background Art
[0002] Wine grains can be roughly divided into white wine grains and brewer grains. They are protein-rich products made from potatoes, beans, sorghum, corn, wheat, glutinous rice and other grains after wine is extracted. They have a certain alcohol content and are rich in growth factors, methionine, cystine, crude fiber, yeast, lactic acid bacteria, etc.
[0003] According to statistics, the output of distiller's grains in my country has exceeded 100 million tons. However, up to now, the utilization of distiller's grains is still in the low-value conversion of feed, fuel and fertilizer. How to transform distiller's grains, a recyclable and renewable resource derived from food, into high-value-added application materials is an important environmental protection strategy that is extremely in line with my country's green and sustainable development. According to the currently known technologies, most of the composite materials converted from distiller's grains have mechanical properties, water repellency, flame retardancy and other indicators that are lower than those of petroleum-based plastics, and their prices are extremely expensive, which makes it difficult to meet customer needs, and at the same time limits the application and expansion of downstream products.
[0004] Therefore, based on this, the technical solution of the present invention is proposed. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the present invention provides a wine lees-based fully degradable film, a preparation method and application thereof. The wine lees-based fully degradable film is prepared by scientifically matching a variety of bio-based raw materials with fully degradable resins, and by adjusting the different mixing ratios of the raw materials, it is possible to fully realize that the wine lees-based fully degradable film meets the actual application index requirements of stretch wrapping film, food cling film or shopping bag. After application and testing, the wine lees-based fully degradable film of the present invention is significantly better than the similar products on the market in terms of appearance performance, physical and mechanical / mechanical properties, sealing strength, automatic sterilization, oxygen permeability coefficient, water vapor permeability coefficient, gas permeability deviation (oxygen, carbon dioxide), moisture permeability deviation and other comprehensive indicators, reaching an excellent level. In addition, the inventors have also confirmed the actual application of the target product. In soil with suitable relative humidity and relative temperature, the wine lees-based fully degradable film can be completely decomposed into carbon dioxide and water within 180 days, as well as other organic matter that is conducive to improving soil microcirculation.
[0006] The scheme of the present invention is to provide a wine lees-based fully degradable film, comprising component A, component B and component C; wherein component A comprises the following raw materials: wine lees, plasticizer, polyvinyl alcohol and corn bran; component B comprises the following raw materials: acetate starch, sodium alginate, cellulose nanofibers and calcium chloride; component C comprises the following raw materials: epoxidized vegetable oil, lubricant and polyhydroxyalkanoate.
[0007] Preferably, the component A comprises the following raw materials in parts by mass: 30 to 50 parts of wine lees, 5 to 15 parts of plasticizer, 10 to 30 parts of polyvinyl alcohol and 5 to 15 parts of corn bran; the component B comprises the following raw materials in parts by mass: 3 to 5 parts of acetate starch, 3 to 5 parts of sodium alginate, 2 to 3 parts of cellulose nanofibers and 1 to 5 parts of calcium chloride; the component C comprises the following raw materials in parts by mass: 2 to 6 parts of epoxidized vegetable oil, 1 to 3 parts of lubricant and 50 to 70 parts of polyhydroxyalkanoate.
[0008] Preferably, the component A comprises the following raw materials in parts by mass: 40 parts of wine lees, 10 parts of plasticizer, 20 parts of polyvinyl alcohol and 10 parts of corn bran; the component B comprises the following raw materials in parts by mass: 4 parts of acetate starch, 4 parts of sodium alginate, 2.5 parts of cellulose nanofibers and 3 parts of calcium chloride; the component C comprises the following raw materials in parts by mass: 4 parts of epoxidized vegetable oil, 2 parts of lubricant and 60 parts of polyhydroxyalkanoate.
[0009] In order to facilitate the understanding of the present invention, the raw materials used in the present invention are described.
[0010] Preferably, the lees are: fresh, mildew-free white wine lees or beer lees with a water content of 60% and a certain alcohol content (usually the alcohol content of white wine lees is about 35%), or a combination of the two in any mass ratio, which can be purchased commercially.
[0011] Preferably, the plasticizer is a combination of at least three of glycerol, propylene glycol, polyethylene glycol, triacetin, and sorbitol in any mass ratio, and can be commercially obtained.
[0012] Preferably, the polyvinyl alcohol is a unit product after instant dissolution and expansion, and under the temperature-controlled stirring state of 30-100°C, the present invention creatively combines it with water molecules in the lees and a small amount of residual ethanol and then rapidly alcoholizes it, and the alcoholysis rate can reach more than 96%, and effectively forms an interface bonding reaction with other materials, thereby achieving the purpose of one-step plasticization and toughening of the material. The polyvinyl alcohol grades described in the present invention are respectively: a combination of three arbitrary mass ratios of polyvinyl alcohol 100-27, polyvinyl alcohol 100-35 and polyvinyl alcohol 100-60, which can be purchased commercially.
[0013] Preferably, the corn bran is a major byproduct of corn starch processing, and the protein content is as high as 60% or more, of which nearly 50% is alcohol-soluble protein. The inventors have found that corn bran, ethanol remaining in vinasse and alcohol-based components in the plasticizer react and modify each other synergistically, and under the condition of temperature-controlled high-speed stirring, the protein in the corn bran can form alcohol-soluble protein. Alcohol-soluble protein not only has unique film-forming properties, but also has antibacterial, antioxidant and degradable properties. Because it contains a large amount of hydrophobic amino acids, it also has a water-repellent function and can be purchased commercially.
[0014] Preferably, the acetate starch is a corn modified starch with good film-forming properties, high viscosity and high clarity. When mixed with the other raw materials described in the present invention, it will form a synergistic effect, not only producing antioxidant properties, but also allowing the target product to be exposed to low temperatures for long-term storage. It is a low-cost stabilizer and can be purchased commercially.
[0015] Preferably, the sodium alginate is a byproduct of extracting iodine and mannitol from kelp or sargassum of brown algae, and is non-toxic and tasteless. The inventors have found that it can effectively synergize with the water molecules and other components including calcium ions in the material of the present invention, and quickly form a gel under extremely mild conditions, and has unique film-forming properties, which can improve the tensile strength, automatic sterilization function and thermal stability of the target product of the present invention, and can be commercially obtained.
[0016] Preferably, the cellulose nanofiber is a functional additive with good compatibility and high crystallinity. Under extremely mild conditions, it can fully and quickly penetrate into the molecular structure of the raw material of the present invention and form a network structure, effectively promoting the mutual synergistic reaction between materials, increasing the carboxyl content in the material, and improving the tensile elasticity of the target product of the present invention. The specific application indicators of the cellulose nanofiber are: diameter: 80-100nm, length: 5-20μm, purity: 99.9%, crystallinity: ≥85%, solid content: ≥5%, and it can be purchased commercially.
[0017] Preferably, the calcium chloride is a powder with strong water absorption. According to its characteristics, it can be used as a desiccant, a microbial inhibitor, or a curing agent. The inventors have found that after calcium chloride reacts with the sodium alginate described in the present invention, seaweed fiber with flame retardant properties is generated. After the seaweed fiber forms an interface with other raw materials involved in the present invention, it can effectively improve the tensile strength and flame retardant properties of the target product of the present invention, which can be purchased commercially.
[0018] Preferably, the epoxidized vegetable oil is a combination of epoxidized soybean oil, epoxidized cottonseed oil and epoxidized linseed oil in any mass ratio. The inventors have found that the combination of these three epoxidized vegetable oils, after synergistic reaction with the raw materials of the present invention, not only plasticizes the raw materials, but also effectively improves the weather resistance of the target product of the present invention, and can be commercially obtained.
[0019] Preferably, the lubricant is a combination of barium stearate and oleamide in a mass ratio of 1:1, which can be commercially obtained.
[0020] Preferably, the polyhydroxyalkanoate is a natural macromolecular biodegradable material synthesized by various microorganisms, and has extremely high film-forming properties. The inventors have found through research that the material has excellent compatibility with the various raw materials described in the present invention, can improve the gas barrier properties of the target product of the present invention, and has extremely high elasticity and adhesion. MireL (F1006) produced in the United States is preferred and can be purchased commercially.
[0021] Based on the same technical concept, another embodiment of the present invention is to provide a method for preparing a wine lees-based fully degradable film, the preparation method comprising the following steps:
[0022] (1) mixing distiller's grains, a plasticizer, polyvinyl alcohol and corn bran, and heating and stirring to obtain a mixture a;
[0023] (2) adding acetate starch, sodium alginate, cellulose nanofibers and calcium chloride to the mixture a, mixing, heating and stirring to obtain a mixture b;
[0024] (3) the mixture b is subjected to filamenting to achieve shearing, friction, dispersion, reaction, compression, melting, exhaust, and plasticization, and after completion, it is dried and ultrafinely pulverized to obtain a multi-element mixture powder;
[0025] (4) mixing epoxy vegetable oil, lubricant and polyhydroxyalkanoate to obtain a mixture C; mixing the mixture C with the multi-protocol mixture powder, heating and stirring, and then extruding and granulating to obtain a masterbatch;
[0026] (5) forming a film from the masterbatch by a casting or blowing process, and obtaining a wine lees-based fully degradable film after completion.
[0027] Preferably, in step (3), the straw brooming machine is used for the silk separation and brooming; the screw diameter of the three-screw straw brooming machine is 270 mm, the aspect ratio is 10:1, the screw speed is 400 r / min, the zone temperatures are: zone 1: 75°C, zone 2: 85°C, zone 3: 95°C, zone 4: 105°C, zone 5: 115°C, zone 6: 90°C, and the vacuum degree of each zone is 0.04-0.08 MPa.
[0028] Preferably, in step (4), the extrusion granulation adopts a three-screw extrusion granulator; the screw diameter of the three-screw extrusion granulator is 80 mm, the aspect ratio is 30:1, the screw speed is 400 r / min, the zone temperature is: zone 1: 100°C, zone 2: 110°C, zone 3: 115°C, zone 4: 120°C, zone 5: 125°C, zone 6: 130°C, zone 7: 120°C, zone 8: 110°C, and die: 100°C, and the vacuum degree of each section is 0.03 MPa.
[0029] Preferably, in step (5), the equipment used in the film-forming process of the casting is a casting machine; the screw speed of the casting machine is 60-110 r / min, the zone temperature is: zone 1: 80°C, zone 2: 100°C, zone 3: 120°C, zone 4: 140°C, zone 5: 120°C, and the line speed is 4-8 m / min.
[0030] Preferably, in step (5), the equipment used in the film-forming process of the blown film is a film blowing machine; the screw speed of the film blowing machine is 40 to 80 r / min, the zone temperature is: zone 1: 90°C, zone 2: 110°C, zone 3: 130°C, zone 4: 150°C, and the line speed is 4 to 8 m / min.
[0031] Based on the same technical concept, another scheme of the present invention is to provide an application of the wine lees-based fully degradable film in the preparation of stretch wrapping film, food cling film or shopping bags.
[0032] The beneficial effects of the present invention are:
[0033] The preparation method of the distiller's grains-based fully degradable film of the present invention is prepared by scientifically combining and synergistically reacting a variety of bio-based raw materials including distiller's grains, creatively utilizing the ethanol component in the distiller's grains and the protein in the corn bran, synergistically reacting to form alcohol-soluble proteins with antibacterial effects, and the alcohol-soluble proteins are fully compatible with other raw materials to form an interface bond, and the reaction generates an alcohol-soluble protein film with antibacterial effects; in addition, sodium alginate reacts with calcium chloride in the material to generate seaweed fibers with antibacterial and flame-retardant effects, and the derivative substances generated during the synergistic reaction of these raw materials greatly improve the mechanical properties of the target film product. And by adjusting the different mixing ratios of various raw materials, the wine lees-based fully degradable film will produce various targeted indicators required by different types of film products, so it can fully meet the practical application of stretch wrap film, food cling film or shopping bags. After testing, the wine lees-based fully degradable film of the present invention is significantly better than similar products on the market in terms of appearance performance, physical and mechanical / mechanical properties, sealing strength, automatic sterilization, oxygen permeability coefficient, water vapor permeability coefficient, gas permeability deviation (oxygen, carbon dioxide), moisture permeability deviation, etc., and has reached an excellent level. In addition, the inventor has determined in the actual application process of the target film product that in soil with suitable relative humidity and relative temperature, the wine lees-based fully degradable film can be completely decomposed into carbon dioxide and water within 180 days, as well as other organic matter that is conducive to improving soil microcirculation. DETAILED DESCRIPTION
[0034] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0035] Example 1
[0036] This embodiment provides a method for preparing a wine lees-based fully degradable film, the preparation method comprising the following steps:
[0037] (1) 30 kg of brewer's grains, 5 kg of plasticizer (a combination of glycerol, propylene glycol and polyethylene glycol in any mass ratio), 10 kg of polyvinyl alcohol (a combination of polyvinyl alcohol 100-27, polyvinyl alcohol 100-35 and polyvinyl alcohol 100-60 in any mass ratio) and 5 kg of corn bran are mixed and put into a temperature-controlled mixer (preferably: SRL-W800 horizontal high-speed mixer produced by Zhangjiagang Ouchuang Machinery Technology Co., Ltd.), and all the raw materials of component A are fully mixed at a stirring and mixing speed of 200 r / min under a temperature-controlled state of 80° C. until a film layer is formed on the surface of the brewer's grain particles and the mixture has dispersibility, thereby obtaining a mixture a;
[0038] (2) 3kg of acetate starch, 3kg of sodium alginate, 2kg of cellulose nanofibers (preferably: diameter: 80nm, length: 5μm, purity: 99.9%, crystallinity: 85%, solid content: 5%) and 1kg of calcium chloride are mixed and added to the mixture a to completely fuse component A and component B. To ensure that the two groups of raw materials can fully react with each other, the surface temperature is strictly controlled at 100°C, the stirring speed is 200r / min, and the mixture is stirred until there is no steam on the surface of the material. When the surface of the mixed material has obvious glossiness and carries more flaky elastomers, it means that the mixed material has good compatibility, the interfaces of various materials have formed a firm bond, and great activity has been generated. It can be confirmed that the material graft copolymerization process step has been completed, the material is cooled and standby, and the mixture b is obtained;
[0039] (3) The mixture b is conveyed to a 270-type parallel three-screw straw brooming machine, the screw diameter of which is 270 mm, the aspect ratio is 10:1, and the three screws are arranged in parallel and rotate in the same direction; the screw speed is 400 r / min, and the zone temperatures are: zone 1: 75°C, zone 2: 85°C, zone 3: 95°C, zone 4: 105°C, zone 5: 115°C, zone 6: 90°C, and the vacuum degree of each zone is 0.04 MPa. The mixture b is sheared, rubbed, dispersed, reacted, compressed, melted, exhausted, and plasticized in the body cavity of the 270-type parallel three-screw straw brooming machine along with the three screws rotating in the same direction, and then discharged from the discharge port of the brooming machine. At this time, the surface of the material has high strength and toughness, as well as a fish-scale structure with plasticity, and it can be determined that the material melting and plasticization modification process step is completed;
[0040] (4) The melt-plasticized and modified material is then subjected to primary crushing and vacuum drying. In view of the characteristics of the melt-plasticized and modified material, the vacuum dryer selected is the SZG double-cone vacuum dryer produced by Changzhou Jinxiang Drying Equipment Co., Ltd. During the drying process, the material is completely exposed to a vacuum state in the drying chamber. In a very short time, the moisture in the internal and surface structures of the material is fully dried to less than 4%, and the drying step is considered to be completed;
[0041] Continue to put the dried material into the airflow superfine pulverizer. The airflow superfine pulverizer is purchased from: QLM20 explosion-proof airflow superfine pulverizer produced by Shandong Jingxin Powder Equipment Co., Ltd. The airflow superfine pulverizer has the advantages of indicators, which can improve and strengthen the uniformity and physical stability of the particle size of the material after micronization, so that the material can easily reach the average particle size requirement of 400 mesh, and the raw material micronized powder is obtained after completion;
[0042] (5) 2 kg of epoxidized vegetable oil (a combination of epoxidized soybean oil, epoxidized cottonseed oil and epoxidized linseed oil in any mass ratio), 1 kg of lubricant (a combination of barium stearate and oleic acid amide in a mass ratio of 1:1) and 50 kg of polyhydroxyalkanoate are mixed to obtain a mixture c; the raw material powder and the mixture c are mixed in a mass ratio of 3:7, and stirred and mixed at 100° C. and 200 r / min until the surface of the polyhydroxyalkanoate is evenly coated into a powder; then the mixture is conveyed to an inverted T-shaped three-screw extruder granulator, and the material is melted, sheared, dispersed, reacted, compressed, exhausted and molded in the machine. The extruder is extruded into strips, stretched with the conveying steel chain, cooled at multiple wind points, and then pelletized to obtain a masterbatch; wherein the inverted T-shaped three-screw extruder granulator unit is an 80-type inverted T-shaped three-screw extruder granulator unit produced by Beijing Zhongxing Xinchuang Plastic Machinery Manufacturing Co., Ltd., with a screw diameter of 80 mm, an aspect ratio of 30:1, a screw speed of 400 r / min, and interval temperatures of: zone 1: 100°C, zone 2: 110°C, zone 3: 115°C, zone 4: 120°C, zone 5: 125°C, zone 6: 130°C, zone 7: 120°C, zone 8: 110°C, and die head: 100°C, and the vacuum degree of each section is 0.03MPa;
[0043] (6) The masterbatch is cast into film by a casting machine, the screw speed of the casting machine is 60r / min, the zone temperature is: zone 1: 80°C, zone 2: 100°C, zone 3: 120°C, zone 4: 140°C, zone 5: 120°C, the line speed is 4m / min, and after completion, a wine lees-based fully degradable film is obtained.
[0044] The wine lees-based fully degradable film obtained in this example can be used to prepare a stretch wrap film.
[0045] Example 2
[0046] This embodiment provides a method for preparing a wine lees-based fully degradable film, the preparation method comprising the following steps:
[0047] (1) 50 kg of lees (a combination of beer lees and white lees in any mass ratio), 15 kg of plasticizer (a combination of polyethylene glycol, triacetin, and sorbitol in any mass ratio), 30 kg of polyvinyl alcohol (a combination of polyvinyl alcohol 100-27, polyvinyl alcohol 100-35, and polyvinyl alcohol 100-60 in any mass ratio) and 15 kg of corn bran are mixed and put into a temperature-controlled mixer (preferably: SRL-W800 horizontal high-speed mixer produced by Zhangjiagang Ouchuang Machinery Technology Co., Ltd.), and all the raw materials of component A are fully mixed at a stirring and mixing speed of 200 r / min under a temperature-controlled state of 80° C. until a film layer appears on the surface of the lees particles and they are dispersible, thereby obtaining a mixture a;
[0048] (2) 5kg of acetate starch, 5kg of sodium alginate, 3kg of cellulose nanofibers (preferably: diameter: 100nm, length: 20μm, purity: 99.9%, crystallinity: 87%, solid content: 6%) and 5kg of calcium chloride are mixed and added to the mixture a to completely fuse component A and component B. To ensure that the two groups of raw materials can fully react with each other, the surface temperature is strictly controlled at 100°C, the stirring speed is 200r / min, and the mixture is stirred until there is no steam on the surface of the material. When the surface of the mixed material has obvious glossiness and carries more flaky elastomers, it means that the mixed material has good compatibility, the interfaces of various materials have formed a firm bond, and great activity has been generated. It can be confirmed that the material graft copolymerization process step has been completed, the material is cooled and used, and the mixture b is obtained;
[0049] (3) The mixture b is conveyed to a 270-type parallel three-screw straw filament broom machine, the screw diameter of the 270-type parallel three-screw straw filament broom machine is 270 mm, the aspect ratio is 10:1, and the three screws are arranged in parallel and rotate in the same direction; the screw speed is 400 r / min, and the zone temperature is: zone 1: 75°C, zone 2: 85°C, zone 3: 95°C, zone 4: 105°C, zone 5: 115°C, zone 6: 90°C, and the vacuum degree of each zone is 0.08 MPa. The mixture b is sheared, rubbed, dispersed, reacted, compressed, melted, exhausted, and plasticized in the body cavity of the 270-type parallel three-screw straw filament broom machine along with the three screws rotating in the same direction, and then discharged from the discharge port of the filament broom machine. At this time, the surface of the material has high strength and toughness, as well as plastic fish-scale structure characteristics. At this time, it can be determined that the material melting and plasticization modification process steps are completed;
[0050] (4) The melt-plasticized and modified material is then subjected to primary crushing and vacuum drying. In view of the characteristics of the melt-plasticized and modified material, the vacuum dryer selected is the SZG double-cone vacuum dryer produced by Changzhou Jinxiang Drying Equipment Co., Ltd. During the drying process, the material is completely exposed to a vacuum state in the drying chamber. In a very short time, the moisture in the internal and surface structures of the material is fully dried to less than 4%, and the drying is considered complete.
[0051] Continue to put the dried material into the airflow superfine pulverizer. The airflow superfine pulverizer is purchased from: QLM20 explosion-proof airflow superfine pulverizer produced by Shandong Jingxin Powder Equipment Co., Ltd. The airflow superfine pulverizer has the advantages of indicators, which can improve and strengthen the uniformity and physical stability of the particle size of the material after micronization, so that the material can easily reach the requirement of an average particle size of 400 meshes, and the raw material micronized powder is obtained after completion;
[0052] (5) 6 kg of epoxidized vegetable oil (a combination of epoxidized soybean oil, epoxidized cottonseed oil and epoxidized linseed oil in any mass ratio), 3 kg of lubricant (a combination of barium stearate and oleic acid amide in a mass ratio of 1:1) and 70 kg of polyhydroxyalkanoate are mixed to obtain a mixture c; the raw material powder and the mixture c are mixed in a mass ratio of 4:6, and stirred and mixed at 100° C. and 200 r / min until the surface of the polyhydroxyalkanoate is evenly coated into a powder; then the mixture is conveyed to an inverted tri-screw extruder granulator, and the material is melted, sheared, dispersed, reacted, compressed, exhausted and molded in the machine. The extruder is extruded into strips, stretched with the conveying steel chain, cooled at multiple wind points, and then pelletized to obtain a masterbatch; wherein the inverted T-shaped three-screw extruder granulator unit is an 80-type inverted T-shaped three-screw extruder granulator unit produced by Beijing Zhongxing Xinchuang Plastic Machinery Manufacturing Co., Ltd., with a screw diameter of 80mm, an aspect ratio of 30:1, a screw speed of 400r / min, and interval temperatures of: zone 1: 100°C, zone 2: 110°C, zone 3: 115°C, zone 4: 120°C, zone 5: 125°C, zone 6: 130°C, zone 7: 120°C, zone 8: 110°C, and die head: 100°C, and the vacuum degree of each section is 0.03MPa;
[0053] (6) The masterbatch is cast into film by a casting machine, the screw speed of the casting machine is 110 r / min, the zone temperature is: zone 1: 80°C, zone 2: 100°C, zone 3: 120°C, zone 4: 140°C, zone 5: 120°C, the line speed is 8 m / min, and after completion, a wine lees-based fully degradable film is obtained.
[0054] The wine lees-based fully degradable film obtained in this example can be used to prepare food preservative film.
[0055] Example 3
[0056] This embodiment provides a method for preparing a wine lees-based fully degradable film, the preparation method comprising the following steps:
[0057] (1) 40 kg of white wine lees, 10 kg of plasticizer (a combination of glycerol, propylene glycol, polyethylene glycol, and triacetin in any mass ratio), 20 kg of polyvinyl alcohol (a combination of polyvinyl alcohol 100-27, polyvinyl alcohol 100-35, and polyvinyl alcohol 100-60 in any mass ratio) and 10 kg of corn bran are mixed and put into a temperature-controlled mixer (preferably: SRL-W800 horizontal high-speed mixer produced by Zhangjiagang Ouchuang Machinery Technology Co., Ltd.), and all the raw materials of component A are fully mixed at a stirring and mixing speed of 200 r / min under a temperature-controlled state of 80° C. until a film layer is formed on the surface of the wine lees particles and the particles are dispersible, thereby obtaining a mixture a;
[0058] (2) 4kg of acetate starch, 4kg of sodium alginate, 2.5kg of cellulose nanofibers (diameter: 90nm, length: 12μm, purity: 99.9%, crystallinity: 88%, solid content: 7%) and 3kg of calcium chloride are mixed and added to the mixture a to completely fuse component A and component B. To ensure that the two groups of raw materials can fully react with each other, the surface temperature is strictly controlled at 100°C, the stirring speed is 200r / min, and the mixture is stirred until there is no steam on the surface of the material. When the surface of the mixed material has obvious glossiness and carries more flaky elastomers, it means that the mixed material has good compatibility, the interfaces of various materials have formed a firm bond, and great activity has been generated. It can be confirmed that the material graft copolymerization process step has been completed, the material is cooled and used, and the mixture b is obtained;
[0059] (3) The mixture b is conveyed to a 270-type parallel three-screw straw brooming machine. The screw diameter of the 270-type parallel three-screw straw brooming machine is 270 mm, the aspect ratio is 10:1, and the three screws are arranged in parallel and rotate in the same direction. The screw speed is 400 r / min, and the zone temperature is: Zone 1: 75°C, Zone 2: 85°C, Zone 3: 95°C, Zone 4: 105°C, Zone 5: 115°C, Zone 6: 90°C. The vacuum degree of each zone is 0.06 MPa. The mixture b is sheared, rubbed, dispersed, reacted, compressed, melted, exhausted, and plasticized in the body cavity of the 270-type parallel three-screw straw brooming machine along with the three screws rotating in the same direction, and then discharged from the discharge port of the brooming machine. At this time, the surface of the material has high strength and toughness, as well as a fish-scale structure with plasticity. At this time, it can be determined that the material melting and plasticization modification process steps are completed;
[0060] (4) The melt-plasticized and modified material is then subjected to primary crushing and vacuum drying. In view of the characteristics of the melt-plasticized and modified material, the vacuum dryer selected is the SZG double-cone vacuum dryer produced by Changzhou Jinxiang Drying Equipment Co., Ltd. During the drying process, the material is completely exposed to a vacuum state in the drying chamber. In a very short time, the moisture in the internal and surface structures of the material is fully dried to less than 4%, and the drying is considered complete.
[0061] Continue to put the dried material into the airflow superfine pulverizer. The airflow superfine pulverizer is purchased from: QLM20 explosion-proof airflow superfine pulverizer produced by Shandong Jingxin Powder Equipment Co., Ltd. The airflow superfine pulverizer has the advantages of indicators, which can improve and strengthen the uniformity and physical stability of the particle size of the material after micronization, so that the material can easily reach the requirement of an average particle size of 400 meshes, and the raw material micronized powder is obtained after completion;
[0062] (5) 4 kg of epoxidized vegetable oil (a combination of epoxidized soybean oil, epoxidized cottonseed oil and epoxidized linseed oil in any mass ratio), 2 kg of lubricant (a combination of barium stearate and oleic acid amide in a mass ratio of 1:1) and 60 kg of polyhydroxyalkanoate are mixed to obtain a mixture c; the raw material powder and the mixture c are mixed in a mass ratio of 5:5, and stirred and mixed at 100° C. and 200 r / min until the surface of the polyhydroxyalkanoate is evenly coated into a powder; then the mixture is conveyed to an inverted T-shaped three-screw extruder granulator, and the material is melted, sheared, dispersed, reacted, compressed, exhausted and molded in the machine. The extruder is extruded into strips, stretched with the conveying steel chain, cooled at multiple wind points, and then pelletized to obtain a masterbatch; wherein the inverted T-shaped three-screw extruder granulator unit is an 80-type inverted T-shaped three-screw extruder granulator unit produced by Beijing Zhongxing Xinchuang Plastic Machinery Manufacturing Co., Ltd., with a screw diameter of 80mm, an aspect ratio of 30:1, a screw speed of 400r / min, and interval temperatures of: zone 1: 100°C, zone 2: 110°C, zone 3: 115°C, zone 4: 120°C, zone 5: 125°C, zone 6: 130°C, zone 7: 120°C, zone 8: 110°C, and die head: 100°C, and the vacuum degree of each section is 0.03MPa;
[0063] (6) The masterbatch is blown into film by a film blowing machine, the screw speed of the film blowing machine is 40 r / min, the zone temperature is: zone 1: 90° C., zone 2: 110° C., zone 3: 130° C., zone 4: 150° C., and the line speed is 4 m / min. After completion, a wine lees-based fully degradable film is obtained.
[0064] The wine lees-based fully degradable film obtained in this example can be used to prepare shopping bags.
[0065] The wine lees-based fully degradable film obtained in Example 1 of the present invention can be used to prepare a stretch wrap film. In order to verify the effect, it is compared with similar products on the market. The results are shown in Table 1.
[0066] Table 1 Physical and mechanical properties
[0067]
[0068] In addition, to demonstrate the bactericidal effect, 50 μL of E. coli suspension was applied to the surface of the sample membrane to be tested. After 10 min, 20 min, and 30 min, the bactericidal rate was measured. The results are shown in Table 2. (The same below)
[0069] Table 2 Bactericidal effect
[0070]
[0071]
[0072] It can be seen from Table 1 and Table 2 that the physical properties and sterilization effect of the wine lees-based fully degradable film obtained in Example 1 of the present invention are significantly better than similar products on the market, reaching an excellent level; in addition, after on-site testing by the inventor, the viscosity of the stretch wrap film obtained in Example 1 is better than similar products on the market, and it can wrap the goods more tightly and more securely; finally, especially the oxygen permeability coefficient and the water vapor permeability coefficient, Example 1 is less than and better than similar products on the market, indicating that in the process of wrapping goods with stretch wrap film, external gases such as water vapor and oxygen are more difficult to penetrate, and the tightness of the wrapping effect will be better than similar products on the market.
[0073] The wine lees-based fully degradable film obtained in Example 2 of the present invention can be used to prepare food preservative film. In order to verify the effect, it is compared with similar products on the market. The results are shown in Tables 3, 4 and 5.
[0074] Table 3 Appearance test results
[0075]
[0076]
[0077] Table 4 Physical and mechanical properties requirements
[0078]
[0079] Table 5 Bactericidal effect
[0080]
[0081]
[0082] As shown in Tables 3, 4 and 5, the appearance performance, physical and mechanical properties and sterilization effect of the wine lees-based fully degradable film obtained in Example 2 of the present invention are significantly better than similar products on the market. In particular, the oxygen and carbon dioxide gas permeation deviations in Example 2 are significantly smaller than similar products on the market, indicating that the product has higher stability.
[0083] The wine lees-based fully degradable film obtained in Example 3 of the present invention can be used to prepare shopping bags. In order to verify the effect, it is compared with similar products on the market. The results are shown in Tables 6, 7 and 8.
[0084] Table 6 Physical and mechanical properties
[0085]
[0086] Table 7 Sealing strength
[0087]
[0088] Table 8 Sterilization effect
[0089] Group Sterilization rate / 10min Sterilization rate / 20min Sterilization rate / 30min Example 3 40.1% 81.2% 93.3% Similar products on the market 0 0 0
[0090] It can be seen from Tables 6, 7 and 8 that the lees-based fully degradable film obtained in Example 3 of the present invention has significantly better physical and mechanical properties, sealing strength and sterilization effect than similar products on the market; especially the oxygen and carbon dioxide gas permeability deviation, Example 3 is significantly smaller than similar products on the market, indicating that its product stability is higher.
[0091] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A wine lees-based fully degradable film, characterized in that: The invention comprises component A, component B and component C; wherein component A comprises the following raw materials in parts by weight: 30 to 50 parts of distiller's grains, 5 to 15 parts of plasticizer, 10 to 30 parts of polyvinyl alcohol and 5 to 15 parts of corn bran; component B comprises the following raw materials in parts by weight: 3 to 5 parts of acetate starch, 3 to 5 parts of sodium alginate, 2 to 3 parts of cellulose nanofibers and 1 to 5 parts of calcium chloride; component C comprises the following raw materials in parts by weight: 2 to 6 parts of epoxidized vegetable oil, 1 to 3 parts of lubricant and 50 to 70 parts of polyhydroxyalkanoate; The wine lees is one or a combination of two of white wine lees or beer lees; the plasticizer is a combination of at least three of glycerol, propylene glycol, polyethylene glycol, triacetin, and sorbitol; the epoxidized vegetable oil is a combination of epoxidized soybean oil, epoxidized cottonseed oil, and epoxidized linseed oil; the lubricant is a combination of barium stearate and oleamide; the weight ratio of the barium stearate to oleamide is 1:1; the model of the polyhydroxyalkanoate is MireL (F1006).
2. The wine lees-based fully degradable film according to claim 1, characterized in that: The component A comprises the following raw materials in parts by mass: 40 parts of wine lees, 10 parts of plasticizer, 20 parts of polyvinyl alcohol and 10 parts of corn bran; the component B comprises the following raw materials in parts by mass: 4 parts of acetate starch, 4 parts of sodium alginate, 2.5 parts of cellulose nanofibers and 3 parts of calcium chloride; the component C comprises the following raw materials in parts by mass: 4 parts of epoxidized vegetable oil, 2 parts of lubricant and 60 parts of polyhydroxyalkanoate.
3. The method for preparing the wine lees-based fully degradable film according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: (1) mixing distiller's grains, a plasticizer, polyvinyl alcohol and corn bran, and heating and stirring to obtain a mixture a; (2) adding acetate starch, sodium alginate, cellulose nanofibers and calcium chloride to the mixture a, mixing, heating and stirring to obtain a mixture b; (3) the mixture b is subjected to filamenting to achieve shearing, friction, dispersion, reaction, compression, melting, exhaust, and plasticization, and after completion, it is dried and ultrafinely pulverized to obtain a multi-element mixture powder; (4) mixing epoxy vegetable oil, lubricant and polyhydroxyalkanoate to obtain a mixture C; mixing the mixture C with the multi-protocol mixture powder, heating and stirring, and then extruding and granulating to obtain a masterbatch; (5) forming a film from the masterbatch by a casting or blowing process, and obtaining a wine lees-based fully degradable film after completion.
4. The method for preparing the wine lees-based fully degradable film according to claim 3, characterized in that: In step (3), the three-screw straw brooming machine is used for the brooming; the screw diameter of the three-screw straw brooming machine is 270 mm, the aspect ratio is 10:1, the screw speed is 400 r / min, the zone temperatures are: zone 1: 75°C, zone 2: 85°C, zone 3: 95°C, zone 4: 105°C, zone 5: 115°C, zone 6: 90°C, and the vacuum degree of each zone is 0.04-0.08 MPa.
5. The method for preparing the wine lees-based fully degradable film according to claim 3, characterized in that: In step (4), the extrusion granulation adopts a three-screw extrusion granulator; the screw diameter of the three-screw extrusion granulator is 80 mm, the aspect ratio is 30:1, the screw speed is 400 r / min, the zone temperature is: zone 1: 100°C, zone 2: 110°C, zone 3: 115°C, zone 4: 120°C, zone 5: 125°C, zone 6: 130°C, zone 7: 120°C, zone 8: 110°C, and the die head is 100°C, and the vacuum degree of each section is 0.03 MPa.
6. The method for preparing the wine lees-based fully degradable film according to claim 3, characterized in that: In step (5), the equipment used in the film-forming process of the casting is a casting machine; the screw speed of the casting machine is 60-110 r / min, the zone temperature is: zone 1: 80°C, zone 2: 100°C, zone 3: 120°C, zone 4: 140°C, zone 5: 120°C, and the line speed is 4-8 m / min.
7. The method for preparing the wine lees-based fully degradable film according to claim 3, characterized in that: In step (5), the equipment used in the film-forming process of the film blowing is a film blowing machine; the screw speed of the film blowing machine is 40-80 r / min, the zone temperature is: zone 1: 90°C, zone 2: 110°C, zone 3: 130°C, zone 4: 150°C, and the line speed is 4-8 m / min.
8. Use of the wine lees-based fully degradable film according to claim 1 or 2 in the preparation of stretch wrapping film, food cling film or shopping bag.