A plasma cutting method for filter chip wafer

Through composite polymer film coating process and nitrogen reflow soldering and other technologies, the problems of electrode exposure and etching gas entering during filter chip wafer cutting are solved, achieving better cutting effect and electrical performance.

CN114496888BActive Publication Date: 2024-11-08RF360 TECH (WUXI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111634433.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-29
Publication Date
2024-11-08
Estimated Expiration
2041-12-29

AI Technical Summary

Technical Problem

During the plasma cutting process of the filter chip wafer, due to uneven thickness and poor fit of the protective film, electrode exposure and etching gases enter the gap, affecting the cutting effect.

Method used

The electrode is wrapped by a composite polymer film coating process, and the uniformity and adhesive sealing of the film are ensured through nitrogen reflow welding and hot pressing baking. The plasma cutting and laser groove technology are combined to ensure cutting accuracy and effect.

Benefits of technology

Effectively prevent electrode exposure and etching gas from entering, improve cutting effect, and ensure the quality and electrical performance of the filter chip.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114496888B_ABST
    Figure CN114496888B_ABST
Patent Text Reader

Abstract

The present invention provides a plasma cutting method for filter chip wafers, wherein the protective film on the electrode side of the wafer is evenly distributed, effectively protecting the electrode, and at the same time, the sealing performance of the wafer after pasting with the wafer is good, effectively preventing the etching gas or other foreign matter from entering, and ensuring the cutting effect. It includes S1, the filter chip wafer uses an electroplating method to electroplate the copper column of the electrode in the corresponding area on the front side, and electroplates the tin layer of the electrode on the surface of the copper column, and the tin layer is reflowed in a nitrogen reflow soldering furnace; S2, the front side of the filter chip wafer is pasted with a composite polymer film using a laminating process, and the laminating is performed in a vacuum matching chamber, wherein the composite polymer film includes a first substrate layer that wraps the front electrode of the filter chip wafer, a second substrate layer that matches and supports the first substrate layer is provided on the outside, and a ring-shaped adhesive layer that matches the edge of the filter chip wafer is provided on the inside of the first substrate layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of filter chips, and in particular to a plasma cutting method for a filter chip wafer. Background Art

[0002] The main cutting methods for semiconductor wafers include grinding wheel cutting, laser cutting, plasma cutting, etc. For filter chips, most of them are cut by grinding wheel cutting, but because the grinding wheel cutting process will cause a lot of edge collapse, so filter chips are usually designed with a part of the area reserved to avoid the impact of edge collapse on the functional area. The wafer utilization rate using this method is low, and the edge collapse and other abnormalities caused by cutting are still high.

[0003] At present, with the development of plasma cutting technology, some filter chip wafers have been cut using this method. Before plasma cutting, a protective film is usually pasted on the side of the wafer with the electrode. However, due to the uneven thickness of the protective film currently used and poor adhesion to the electrode, the electrode on the wafer will be partially or completely exposed, which will cause adverse effects such as corrosion of the electrode or adhesion of foreign matter in subsequent process processing, ultimately affecting the electrical performance of the filter chip; at the same time, the adhesion of the protective film to the wafer is also poor, and gaps are easily generated, which leads to the excess etching gas generated after the wafer is etched during the cutting process. The gap between the protective film and the wafer enters and continues to etch the wafer, resulting in many abnormalities such as incomplete cutting and over-etching during cutting, affecting the cutting effect. Summary of the invention

[0004] In view of the problem that during the cutting process of the filter chip wafer, the thickness of the protective film on the electrode side of the wafer is uneven, resulting in exposure of the electrode on the wafer, and at the same time, the adhesion between the protective film and the wafer is poor, resulting in excess etching gas entering the gap between the wafer and the protective film to etch the wafer, thus affecting the cutting effect. The present invention provides a plasma cutting method for filter chip wafers, in which the protective film on the electrode side of the wafer is evenly distributed, effectively protecting the electrode, and at the same time, the sealing performance of the protective film after bonding with the wafer is good, which effectively prevents the entry of etching gas or other foreign matter, thereby ensuring the cutting effect.

[0005] The technical solution is as follows: a plasma cutting method for a filter chip wafer, characterized in that it comprises the following steps: S1, electroplating the copper pillars of the electrodes in the corresponding area on the front side of the filter chip wafer by an electroplating method, and electroplating the tin layer of the electrodes on the surface of the copper pillars, and reflow soldering the tin layer in a nitrogen reflow soldering furnace;

[0006] S2. A composite polymer film is pasted on the front side of the filter chip wafer by a laminating process, and the film is aligned in a vacuum matching chamber, and the air pressure of the vacuum matching chamber is 0Pa~20Pa; wherein the composite polymer film includes a first substrate layer wrapping the front electrode of the filter chip wafer, a second substrate layer matching and supporting is provided on the outside of the first substrate layer, and a ring-shaped adhesive layer matching the edge of the filter chip wafer is provided on the inside of the first substrate layer;

[0007] S3, placing the filter chip wafer in a nitrogen high pressure oven for baking and hot pressing;

[0008] S4, placing the filter chip wafer in a grinder to grind and thin the back side thereof;

[0009] S5, coating the back side of the filter chip wafer with a layer of aqueous protective liquid by spin coating;

[0010] S6, laser grooving the back side of the filter chip wafer according to the cutting line position, the laser grooving width is 1µm~3µm, and the depth of the laser grooving into the back side of the filter chip wafer is 1 to 5um;

[0011] S7, plasma cutting the groove on the back side of the filter chip wafer using a plasma cutting device, and the cutting only cuts the filter chip wafer without penetrating the composite polymer film on the front side thereof;

[0012] S8, cleaning the back side of the filter chip wafer with a cleaning agent to remove the aqueous protective liquid thereon;

[0013] S9, affixing a UV film to the back of the filter chip wafer, and then peeling off the composite polymer film on the front side.

[0014] It is further characterized by:

[0015] In S1, the substrate of the filter chip wafer is made of silicon, and the diameter of the copper column electroplated thereon is 30µm~90µm, and the height is 20µm~80µm; the thickness of the tin layer on the surface of the copper column is 15µm~35µm, and the nitrogen reflow soldering furnace is a temperature-staged reflow soldering furnace, the maximum furnace temperature of the temperature-staged reflow soldering furnace is 250°C, and the length of the furnace temperature above 200°C accounts for 1 / 10~1 / 5 of the total furnace length, and the temperature difference between adjacent furnace temperatures of the temperature-staged reflow soldering furnace is not higher than 30°C; the filter chip wafer moves at a uniform speed in the temperature-staged reflow soldering furnace, and the total time in the temperature-staged reflow soldering furnace is 5min~10min.

[0016] In S2, the first substrate layer of the polymer film is a polyolefin or a polyurethane, and the thickness of the first substrate layer is 60µm~120µm; the second substrate layer is a polymethacrylate film or a polyethylene terephthalate film, and the thickness of the second substrate layer is 90µm~120µm; the annular adhesive layer is a polymethacrylate or a silicone, and the width of the annular adhesive layer is 5mm~15mm, and the thickness is 5µm~10µm.

[0017] In S3, the target pressure of the nitrogen high-pressure oven is 1.5atm~3.5atm, the baking temperature of the nitrogen high-pressure oven adopts programmed temperature rise, and the initial temperature is 20°C, the heating rate is 3~10°C / min, the maximum temperature is 130°C, and it is maintained for 1~3 minutes, and then dropped to room temperature; the initial pressure of the nitrogen high-pressure oven is normal pressure, and the pressure is evenly increased at the beginning of the temperature rise, and the target pressure value is reached at the same time when the maximum temperature is reached.

[0018] In S4, the thickness of the filter chip wafer after grinding is 120µm~150µm.

[0019] In S5, the aqueous protective liquid is a water-soluble polyether glue, and the aqueous protective liquid is applied to the back side of the filter chip wafer by a spin coating process with a thickness of 0.5µm to 3µm.

[0020] In S7, the working gas of the plasma cutting equipment is a mixed gas of O2, Ar, SF6, and C4F8, and the width of the cutting road etched by the plasma cutting equipment is 3µm~15µm.

[0021] In S8, the cleaning agent is any one of deionized water or deionized water in which carbon dioxide is dissolved.

[0022] In S9, when the composite polymer film is peeled off, a vacuum suction cup with a heating function is used in conjunction with the operation. The temperature of the vacuum suction cup is set to 30°C~70°C. The back side of the filter chip wafer is attached and fixed to the vacuum suction cup, and then the polymer film is slowly torn off.

[0023] After adopting the above structure, since the front side of the filter chip wafer is pasted with a composite polymer film by a lamination process, and since the composite polymer film includes a three-layer structure, the first substrate layer of the composite polymer film can wrap the electrode on the back side of the filter chip wafer, which can effectively prevent the electrode from being exposed and ensure the quality of the filter chip thereon. At the same time, the second substrate layer outside the first substrate layer plays a supporting role, and its smooth surface is also convenient for subsequent processing. The annular adhesive layer at the bottom of the first substrate layer can seal the edge of the wafer, thereby preventing excess etching gas generated by the plasma cutting equipment from entering the wafer and corroding the wafer, thereby ensuring the cutting effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A flow chart showing the overall structure of the present invention;

[0025] Figure 2 This is the effect diagram of the copper pillar and tin layer reflow soldering on the current filter chip wafer;

[0026] Figure 3 This is a diagram showing the effect of reflow soldering of the copper pillars and tin layer on the filter chip wafer of the present invention. DETAILED DESCRIPTION

[0027] like Figure 1 As shown, a plasma cutting method for a filter chip wafer comprises the following steps:

[0028] S1. The filter chip wafer 1 is a silicon material substrate. The copper pillar 2 of the electrode is first electroplated in the corresponding area on the substrate of the filter chip wafer 1 by electroplating. The diameter of the copper pillar 2 is 30µm~90µm, and the height is 20µm~80µm. Then, the tin layer 3 of the electrode is electroplated on the surface of the copper pillar 2. The thickness of the tin layer is 15µm~35µm. The tin layer 3 is reflowed in a nitrogen reflow soldering furnace. Specifically, the nitrogen reflow soldering furnace is a temperature segmented reflow soldering furnace, and the maximum furnace temperature of the temperature segmented reflow soldering furnace is 250°C, and the length of the furnace temperature above 200°C accounts for 1 / 10~1 / 5 of the total furnace length. The temperature difference between adjacent furnace temperatures in the temperature segmented reflow soldering furnace is not higher than 30°C. The filter chip wafer 1 moves at a uniform speed in the temperature segmented reflow soldering furnace, and the total time in the temperature segmented reflow soldering furnace is 5min~10min. Figure 2 and Figure 3 As shown, it can be seen that the reflow soldering method of the present invention can ensure that the tin layer 3 on the copper column 2 will not climb up to its surface through the temperature-staged reflow soldering furnace, and no excess impurities will adhere to the copper column 2. At the same time, the tin layer 3 thereon is a smooth sphere, and there are no pits, bubbles and other abnormalities on the tin layer 3, and the reflow soldering effect is good.

[0029] S2. The composite polymer film 4 is pasted on the front side of the filter chip wafer by using a laminating process, and an alignment laminating process is performed in a vacuum alignment chamber, wherein the air pressure of the vacuum alignment chamber is 0Pa~20Pa.

[0030] Specifically, the composite polymer film 4 includes a first substrate layer 42 that wraps the back electrode of the filter chip wafer 1. The first substrate layer is a polyolefin or a carbamate, and the thickness of the first substrate layer 42 is 60µm~120µm. Since the thickness of the first substrate layer 42 is greater than the height of the electrode, the back electrode can be wrapped by the first substrate layer 42. At the same time, since the first substrate layer 42 has a certain degree of softness, the adhesion between the electrode is high and there are no bubbles. A matching second substrate layer 43 that plays a supporting role is provided on the outside of the first substrate layer 42. The second substrate layer is a polymethacrylate film or a polyethylene terephthalate film, and the thickness of the second substrate layer is 90µm~120µm. The second base layer 43 has a high hardness and can play a supporting and protective role. At the same time, the outer surface of the second base layer 43 is smooth, which is convenient for the subsequent processing of the filter chip wafer. An annular adhesive layer 41 matching the edge of the filter chip wafer 1 is provided inside the first substrate layer 42. The annular adhesive layer 41 is a polymethyl methacrylate or silicone type. The width of the annular adhesive layer 41 is 5mm~15mm, and the thickness is 5µm~10µm. The composite polymer film 4 is firmly adhered to the front of the filter chip wafer 1 through the annular adhesive layer 41. The edge has good sealing, which can effectively prevent excess etching gas generated in the subsequent cutting process from entering the front of the filter chip wafer 1 to continue etching the wafer, thereby ensuring the cutting effect and the quality of the wafer.

[0031] S3. Place the filter chip wafer 1 that has been coated in a nitrogen high-pressure oven for baking and hot pressing. The target pressure of the nitrogen high-pressure oven is 1.5atm~3.5atm; the baking temperature of the nitrogen high-pressure oven is programmed, with an initial temperature of 20°C, a heating rate of 3~10°C / min, a maximum temperature of 130°C, and is maintained for 1~3 minutes, then dropped to room temperature; the initial pressure of the nitrogen high-pressure oven is normal pressure, and the pressure is evenly increased at the beginning of the temperature rise, and the target pressure value is reached at the same time when the maximum temperature is reached.

[0032] S4. The filter chip wafer 1 that has been subjected to the baking and hot pressing treatment is placed in a grinder to grind and thin the back side thereof. The wafer thickness of the filter chip wafer 1 after grinding is 120µm~150µm (excluding the height of the electrode).

[0033] S5. A layer of aqueous protective liquid 5 is applied to the back of the filter chip wafer 1 after the grinding and thinning process by spin coating. The aqueous protective liquid 5 is a water-soluble polyether glue. The aqueous protective liquid is applied to the back of the filter chip wafer 1 by spin coating, and its thickness is 0.5µm~3µm.

[0034] S6. Laser groove 6 is performed on the back side of the filter chip wafer 1 according to the cutting line position. The groove width of the laser groove 6 is 1µm~3µm, and the depth of the laser groove 6 penetrating into the back side of the filter chip wafer 1 is 1 to 5um.

[0035] S7. A plasma cutting device is used to perform plasma cutting on the groove 6 on the back side of the filter chip wafer 1. At the same time, the cutting only cuts the substrate of the filter chip wafer without penetrating the composite polymer film 4 on the front side thereof. The working gas of the plasma cutting device is a mixed gas of O2, Ar, SF6, and C4F8. The width of the cutting path etched by the plasma cutting device is 3µm~15µm.

[0036] S8. Clean the back side of the filter chip wafer with a cleaning agent to remove the aqueous protective liquid 5 thereon, wherein the cleaning agent 5 is any one of deionized water or deionized water containing dissolved carbon dioxide.

[0037] S9. A UV film 7 is pasted on the back of the filter chip wafer 1. The UV film 7 consists of a substrate and an adhesive layer. The substrate is made of either a polyurethane resin or a polyvinyl chloride film. The adhesive layer is a polymethyl methacrylate adhesive layer containing a UV photosensitive polymerizer component. The composite polymer film 4 on the front is then peeled off. Specifically, the peeling method is that when peeling off the composite polymer film 4, a vacuum suction cup with a heating function is used in conjunction with the operation. The temperature of the vacuum suction cup is set to 30°C~70°C. The back of the filter chip wafer 1 is attached and fixed to the vacuum suction cup, and then the polymer film is slowly peeled off by manual or external film peeling equipment.

[0038] The above are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by anyone familiar with the technology within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A plasma cutting method for filter chip wafers, characterized in that: It includes the following steps: S1. The filter chip wafer is electroplated in the corresponding area on the front side of the copper column of the electrode by electroplating, and the tin layer of the electrode is electroplated on the surface of the copper column, and the tin layer is reflowed in a nitrogen reflow soldering furnace; S2. A composite polymer film is pasted on the front side of the filter chip wafer by a laminating process, and the film is aligned in a vacuum matching chamber, and the air pressure of the vacuum matching chamber is 0Pa~20Pa; wherein the composite polymer film includes a first substrate layer wrapping the front electrode of the filter chip wafer, a second substrate layer matching and supporting is provided on the outside of the first substrate layer, and a ring-shaped adhesive layer matching the edge of the filter chip wafer is provided on the inside of the first substrate layer; S3, placing the filter chip wafer in a nitrogen high pressure oven for baking and hot pressing; S4, placing the filter chip wafer in a grinder to grind and thin the back side thereof; S5, coating the back side of the filter chip wafer with a layer of aqueous protective liquid by spin coating; S6, laser grooving the back side of the filter chip wafer according to the cutting path position, the laser grooving width is 1µm~3µm, and the depth of the laser grooving into the back side of the filter chip wafer is 1 to 5um; S7, plasma cutting the groove on the back side of the filter chip wafer using a plasma cutting device, and at the same time, the cutting step only cuts the filter chip wafer without penetrating the composite polymer film on the front side thereof; S8, cleaning the back side of the filter chip wafer with a cleaning agent to remove the aqueous protective liquid thereon; S9, affixing a UV film to the back of the filter chip wafer, and then peeling off the composite polymer film on the front side; In S2, the first substrate layer of the polymer film is a polyolefin or a polyurethane, and the thickness of the first substrate layer is 60µm~120µm; the second substrate layer is a polymethacrylate film or a polyethylene terephthalate film, and the thickness of the second substrate layer is 90µm~120µm; the annular adhesive layer is a polymethacrylate or a silicone, and the width of the annular adhesive layer is 5mm~15mm, and the thickness is 5µm~10µm.

2. The plasma cutting method for filter chip wafer according to claim 1, characterized in that: In S1, the substrate of the filter chip wafer is made of silicon, and the diameter of the copper column electroplated thereon is 30µm~90µm, and the height is 20µm~80µm; the thickness of the tin layer on the surface of the copper column is 15µm~35µm, and the nitrogen reflow soldering furnace is a temperature-staged reflow soldering furnace, the maximum furnace temperature of the temperature-staged reflow soldering furnace is 250°C, and the length of the furnace temperature above 200°C accounts for 1 / 10~1 / 5 of the total furnace length, and the temperature difference between adjacent furnace temperatures of the temperature-staged reflow soldering furnace is not higher than 30°C; the filter chip wafer moves at a uniform speed in the temperature-staged reflow soldering furnace, and the total time in the temperature-staged reflow soldering furnace is 5min~10min.

3. The plasma cutting method for filter chip wafer according to claim 1, characterized in that: In S3, the target pressure of the nitrogen high-pressure oven is 1.5atm~3.5atm, the baking temperature of the nitrogen high-pressure oven adopts programmed temperature rise, and the initial temperature is 20°C, the heating rate is 3~10°C / min, the maximum temperature is 130°C, and it is maintained for 1~3 minutes, and then dropped to room temperature; the initial pressure of the nitrogen high-pressure oven is normal pressure, and the pressure is evenly increased at the beginning of the temperature rise, and the target pressure value is reached at the same time when the maximum temperature is reached.

4. The plasma cutting method for filter chip wafer according to claim 1, characterized in that: In S4, the thickness of the filter chip wafer after grinding is 120µm~150µm.

5. The plasma cutting method for filter chip wafer according to claim 1, characterized in that: In S5, the aqueous protective liquid is a water-soluble polyether glue, and the aqueous protective liquid is applied to the back side of the filter chip wafer by a spin coating process with a thickness of 0.5µm to 3µm.

6. The plasma cutting method for filter chip wafer according to claim 1, characterized in that: In S7, the working gas of the plasma cutting equipment is a mixed gas of O2, Ar, SF6, and C4F8, and the width of the cutting road etched by the plasma cutting equipment is 3µm~15µm.

7. The plasma cutting method for filter chip wafer according to claim 1, characterized in that: In S8, the cleaning agent is deionized water or deionized water in which carbon dioxide is dissolved.

8. The plasma cutting method for filter chip wafer according to claim 1, characterized in that: In S9, when the composite polymer film is peeled off, a vacuum suction cup with a heating function is used in conjunction with the operation. The temperature of the vacuum suction cup is set to 30°C~70°C. The back side of the filter chip wafer is attached and fixed to the vacuum suction cup, and then the polymer film is slowly torn off.