Method for forming semiconductor structure

By forming a highly consistent sacrificial layer in the semiconductor structure and performing appropriate processing, the etching defect problem caused by the difference in through-hole arrangement density is solved, and the yield of the semiconductor structure is improved.

CN114496904BActive Publication Date: 2024-12-06CHANGXIN MEMORY TECH INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011165219.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-27
Publication Date
2024-12-06
Estimated Expiration
2040-10-27

AI Technical Summary

Technical Problem

The uneven arrangement density of the through-holes in the semiconductor structure leads to different filling heights, which in turn creates defects during the etching process, affecting the yield of the semiconductor structure.

Method used

By forming a sacrificial layer that fills the through holes and making it highly consistent in the direction perpendicular to the substrate surface, chemical mechanical grinding and hydrogen plasma are used to remove the sacrificial layer to ensure that the openings are connected to the through holes and avoiding the differences in pattern density Etching defects.

Benefits of technology

The consistency of through-hole filling height is achieved, the yield of semiconductor structure is improved, and the occurrence of etching defects is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114496904B_ABST
    Figure CN114496904B_ABST
Patent Text Reader

Abstract

An embodiment of the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate having a first region and a second region, wherein a plurality of discrete through holes are formed in the substrate, and the arrangement density of the through holes located in the first region is greater than the arrangement density of the through holes located in the second region; forming a sacrificial layer filling the through holes; etching the substrate to a thickness of a portion surrounding the sacrificial layer to form an opening, wherein the opening surrounds the sacrificial layer, and in a direction perpendicular to the surface of the substrate, the depth of the opening is less than the depth of the through hole; removing the sacrificial layer, and the opening is connected to the corresponding through hole to form a groove; the embodiment of the present invention is used to avoid etching defects caused by different pattern densities.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductors, and in particular to a method for forming a semiconductor structure. Background Art

[0002] As the characteristic size of semiconductor devices decreases, the spacing between through holes in the semiconductor structure decreases, and the arrangement density of through holes in the semiconductor structure is uneven, resulting in a large arrangement density of through holes in some areas and a small arrangement density of through holes in some areas.

[0003] In the process of filling the through holes, within the same filling time, the filling height of the through holes with a high arrangement density is lower, resulting in different filling heights of the through holes in the semiconductor structure. In the subsequent process of etching to form the Damascus structure, etching defects are easily generated due to the different filling heights of the through holes, thereby affecting the yield of the formed semiconductor structure. Summary of the invention

[0004] An embodiment of the present invention provides a method for forming a semiconductor structure, which avoids etching defects caused by different pattern densities.

[0005] To solve the above technical problems, an embodiment of the present invention provides a method for forming a semiconductor structure, including: providing a substrate having a first region and a second region, wherein a plurality of discrete through holes are formed in the substrate, and the arrangement density of the through holes located in the first region is greater than the arrangement density of the through holes located in the second region; forming a sacrificial layer filling the through holes; etching the substrate to a thickness of a portion surrounding the sacrificial layer to form an opening, wherein the opening surrounds the sacrificial layer, and in a direction perpendicular to the surface of the substrate, the depth of the opening is less than the depth of the through hole; removing the sacrificial layer, and the opening is connected to the corresponding through hole to form a groove.

[0006] Compared with the related art, a sacrificial layer is formed to fill the through hole, and the height of the sacrificial layer filling the through hole is consistent, thereby ensuring that in the subsequent process of etching the Damascus structure based on the sacrificial layer, etching defects caused by different pattern densities are eliminated, thereby improving the yield of the semiconductor structure.

[0007] In addition, in the direction perpendicular to the surface of the substrate, the height of the sacrificial layer located in the first area is flush with the height of the sacrificial layer located in the second area, forming a sacrificial layer filling the through hole, including the following steps: forming a sacrificial film filling the through hole and covering the substrate; flattening the sacrificial film, and the remaining sacrificial film serves as the sacrificial layer.

[0008] In addition, the sacrificial film is planarized until the top surface of the remaining sacrificial film is parallel to the top surface of the substrate. The structure of the formed sacrificial layer provided by the embodiment of the present invention makes the top surface of the sacrificial layer based on the filling through hole flush.

[0009] In addition, the sacrificial film is planarized until the top surface of the substrate is exposed. The structure of the formed sacrificial layer provided by the embodiment of the present invention makes the top surface of the sacrificial layer based on the filling through hole flush.

[0010] In addition, chemical mechanical polishing is used for planarization.

[0011] In addition, the sacrificial layer is a hard mask formed by spin coating.

[0012] In addition, the material of the sacrificial layer includes polysilicon. The sacrificial layer formed by polysilicon has a larger etching selectivity, which prevents the sacrificial layer from being over-etched during the process of etching to form the opening.

[0013] In addition, in a direction parallel to the surface of the substrate, a width of the opening located in the second region is greater than a width of the opening located in the first region.

[0014] In addition, hydrogen plasma is used to remove the sacrificial layer. Hydrogen plasma daughter bodies are used to remove the sacrificial layer. The hydrogen plasma daughter bodies only have a chemical reaction effect, and there is no bombardment effect, so that the formed opening morphology is prevented from being destroyed in the process of removing the sacrificial layer.

[0015] In addition, etching a portion of the thickness of the substrate around the sacrificial layer to form an opening includes the following steps: forming a patterned mask layer on the top surface of the substrate, in a direction parallel to the substrate surface, the orthographic projection of the pattern exposed by the patterned mask layer on the substrate completely covers the orthographic projection of the sacrificial layer on the substrate; etching a portion of the height of the substrate based on the patterned mask layer to form an opening; and removing the patterned mask layer.

[0016] In addition, a patterned mask layer is formed on the top surface of the sacrificial layer, including the following steps: forming a mask layer on the top surface of the sacrificial layer; forming a patterned photoresist on the top surface of the mask layer, wherein the orthographic projection of the pattern exposed by the patterned photoresist on the substrate completely covers the orthographic projection of the sacrificial layer on the substrate; based on the patterned photoresist, etching a portion of the mask layer to form a patterned mask layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] One or more embodiments are exemplarily described by pictures in the corresponding drawings. Unless otherwise stated, the pictures in the drawings are not limited to scale.

[0018] Figures 1 to 8 A schematic diagram of the cross-sectional structures corresponding to each step in the method for forming a semiconductor structure provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0019] At present, in the process of filling through holes, within the same filling time, the filling height of through holes with high arrangement density is lower, resulting in different filling heights of various through holes in the semiconductor structure. In the subsequent process of etching to form a Damascus structure, etching defects are easily generated due to the different filling heights of the through holes, thereby affecting the yield of the formed semiconductor structure.

[0020] To solve the above problems, the first embodiment of the present invention provides a method for forming a semiconductor structure, including: providing a substrate having a first area and a second area, wherein a plurality of discrete through holes are formed in the substrate, and the arrangement density of the through holes located in the first area is greater than the arrangement density of the through holes located in the second area; forming a sacrificial layer filling the through holes; etching the substrate to form an opening with a thickness of a portion surrounding the sacrificial layer, wherein the opening surrounds the sacrificial layer, and in a direction perpendicular to the surface of the substrate, the depth of the opening is less than the depth of the through hole; removing the sacrificial layer, and the opening is connected with the corresponding through hole to form a groove; the embodiment of the present invention is used to avoid etching defects caused by different pattern densities.

[0021] To make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings. However, it will be appreciated by those skilled in the art that in the embodiments of the present invention, many technical details are proposed in order to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical scheme claimed in the present application can be implemented. The division of the following embodiments is for the convenience of description and should not constitute any limitation on the specific implementation of the present invention. The various embodiments can be combined with each other and quoted from each other without contradiction.

[0022] Figures 1 to 8 The cross-sectional structure schematic diagram corresponding to each step of the method for forming a semiconductor structure provided in an embodiment of the present invention is provided. The semiconductor structure of this embodiment is specifically described below.

[0023] refer to Figure 1 A substrate 100 having a first region 110 and a second region 120 is provided, and a plurality of discrete through holes 201 are formed in the substrate 100, and the arrangement density of the through holes 201 located in the first region 110 is greater than the arrangement density of the through holes 201 located in the second region 120.

[0024] In this embodiment, the substrate 100 includes a conductive layer 101, a first insulating layer 102, a dielectric layer 103, and a second insulating layer 104, which are stacked in sequence. It should be noted that this embodiment describes in detail the method for forming a semiconductor structure provided in this embodiment with a specific structure of the substrate 100, in order to help those skilled in the art understand the implementation of this solution, and does not constitute a limitation of the present invention. In a specific implementation, the method for forming a semiconductor structure provided in this embodiment can be applicable to semiconductors of different structures, and those skilled in the art can select a suitable position according to the structure of the substrate 100 to implement the method for forming a semiconductor structure provided in this embodiment.

[0025] Specifically, in this embodiment, the conductive layer 101 can be a conductive material or composed of multiple conductive materials, such as doped polysilicon, titanium, titanium nitride, tungsten and a tungsten composite; the materials of the first insulating layer 102, the dielectric layer 103 and the second insulating layer 104 include silicon nitride, silicon dioxide or silicon nitride oxide; in this embodiment, the material of the conductive layer 101 is copper, the material of the first insulating layer 102 and the second insulating layer 104 is silicon nitride, and the material of the dielectric layer 103 is silicon oxide.

[0026] Since there is a density difference in the arrangement of the through holes 201 in the first region 110 and the second region 120, when filling the through holes 201, the height of the through holes 201 in the first region 110 is often lower than the height of the through holes 201 in the second region 120. In the subsequent process of etching to form openings, since the through holes 201 are filled to different heights, in the process of forming openings in the first region 110 and the second region 120, the side walls of the through holes 201 in the first region 110 are easily over-etched, thereby affecting the morphology of the subsequently formed semiconductor structure, and further affecting the yield of the subsequently formed semiconductor structure.

[0027] This embodiment aims to form a sacrificial layer filling the through hole 201, so that the height of the sacrificial layer located in the first area 110 is flush with that of the sacrificial layer located in the second area 120. The method for forming the sacrificial layer in this embodiment is described in detail below with reference to the accompanying drawings.

[0028] refer to Figure 2 and Figure 3 , forming a sacrificial layer 202 filling the through hole 201. In a direction perpendicular to the surface of the substrate 100, the height of the sacrificial layer 202 located in the first area 110 is flush with the height of the sacrificial layer 202 located in the second area 120.

[0029] In one example, the material of the sacrificial layer 202 includes polysilicon, and the sacrificial layer 202 may be formed by chemical vapor deposition (CVD) or a furnace process.

[0030] Specifically, the sacrificial layer 202 is formed by chemical vapor deposition, and the formed sacrificial layer 202 has good compactness and can relatively completely fill the through hole 201. Since the furnace tube process deposits a large number of wafers at the same time, the sacrificial layer 202 is formed by the furnace tube process, which can improve the deposition efficiency of the sacrificial layer 202, thereby solving the time cost of semiconductor process manufacturing.

[0031] The sacrificial layer 202 is formed of polysilicon, and there is a large etching selectivity ratio between the sacrificial layer 202 and the dielectric layer 103, so that when the sacrificial layer 202 is subsequently etched, the etching material can avoid having a high etching rate on the dielectric layer 103, or when the dielectric layer 103 is subsequently etched, the etching material can avoid having a high etching rate on the sacrificial layer 202.

[0032] In another example, the sacrificial layer 202 is a hard mask formed by spin coating, and the formed hard mask has a certain etching selectivity ratio with the dielectric layer 103 , thereby achieving selective etching of the sacrificial layer 202 or the dielectric layer 103 .

[0033] Compared with a hard mask formed by spin coating, the sacrificial layer 202 formed by polycrystalline silicon has a larger etching selectivity than the hard mask. In the subsequent etching process to form an opening, the sacrificial layer 202 formed by polycrystalline silicon is etched less, thereby ensuring the integrity of the morphology of the subsequently formed semiconductor structure, thereby improving the yield of the subsequently formed semiconductor structure.

[0034] The sacrificial layer 202 filling the through hole 201 is formed, comprising the following steps:

[0035] A sacrificial film (not shown) is formed to fill the through hole 201 and cover the substrate 100 .

[0036] Specifically, since the arrangement density of the through holes 201 located in the first area 110 is greater than the arrangement density of the through holes 201 in the second area 120, in the process of forming the sacrificial film (not shown), due to the difference in arrangement density, less material is required to fill the through holes 201 in the second area 120, and more material is required to fill the through holes 201 in the first area 110; therefore, the formed sacrificial film (not shown) will first fill the through holes 201 located in the second area 120, resulting in the top surface of the sacrificial film (not shown) subsequently formed to cover the substrate 110 not being at the same height, and the height of the top surface of the sacrificial film (not shown) located in the second area 120 is higher than the height of the top surface of the sacrificial film (not shown) located in the first area 110.

[0037] The sacrificial film (not shown) is planarized, and the remaining sacrificial film (not shown) serves as the sacrificial layer 202 .

[0038] In this embodiment, a planarization process is performed by chemical mechanical polishing (CMP) to form a sacrificial layer 202 with the same height between the first region 110 and the second region 120. In other embodiments, an etching process may be used to planarize the top surface of the sacrificial film (not shown). The top of the sacrificial film (not shown) is polished by chemical mechanical polishing to form the sacrificial layer 202. Compared with the etching process, chemical mechanical polishing has a higher removal rate, which is conducive to shortening the process cycle.

[0039] Specifically, this embodiment provides two morphologies of the sacrificial layer 202 formed by planarization treatment.

[0040] The first one: reference Figure 2 , the sacrificial film (not shown) is planarized until the top surface of the remaining sacrificial film (not shown) is parallel to the top surface of the substrate 100. The formed sacrificial layer 202 not only fills the through hole 201, but also the height of the sacrificial layer 202 located in the first area 110 and the height of the sacrificial layer 202 located in the second area 120 are flush. That is, the sacrificial layer 202 covering the substrate 100 is at the same height, for example, the top surface of the sacrificial layer 202 is parallel to the top surface of the base 100.

[0041] The second type: reference Figure 3 The sacrificial film (not shown) is planarized until the top surface of the substrate 100 is exposed. The formed sacrificial layer 202 is only used to fill the through holes 201 located in the first area 110 and the second area 120. That is, the height of the sacrificial layer 202 filling the through holes 201 is flush with the height of the base 100.

[0042] It should be noted that the structure of the sacrificial layer 202 formed in the first manner in this embodiment provides a detailed introduction to the method for forming a semiconductor structure provided, and the method for forming a semiconductor structure applicable to the structure of the sacrificial layer 202 formed in the first manner is also applicable to the structure of the sacrificial layer 202 formed in the second manner.

[0043] refer to Figures 4 to 7 The substrate 100 is etched to a thickness of a portion around the sacrificial layer 202 to form an opening 301 . The opening 301 surrounds the sacrificial layer 202 . In a direction perpendicular to the surface of the substrate 100 , the depth of the opening 301 is less than the depth of the through hole 201 .

[0044] Specifically, refer to Figure 4-5A patterned mask layer 203 is formed on the top surface of the substrate 100. In a direction parallel to the surface of the substrate 100, the orthographic projection of the pattern exposed by the patterned mask layer 203 on the substrate 100 completely covers the orthographic projection of the sacrificial layer 202 on the substrate 100. The orthographic projection of the pattern exposed by the patterned mask layer 203 on the substrate 100 completely covers the orthographic projection of the sacrificial layer 202 on the substrate 100, ensuring that the formed opening 301 surrounds the sacrificial layer 202.

[0045] Forming the patterned mask layer 203 includes the following steps:

[0046] refer to Figure 4 A mask layer 213 is formed on the top surface of the sacrificial layer 202 , and a patterned photoresist 204 is formed on the top surface of the mask layer 213 . The orthographic projection of the pattern exposed by the patterned photoresist 204 on the substrate 100 completely covers the orthographic projection of the sacrificial layer 202 on the substrate 100 .

[0047] refer to Figure 5 , based on the patterned photoresist, a portion of the mask layer 213 is etched to form a patterned mask layer 203 .

[0048] refer to Figure 6 Based on the patterned mask layer 203, the sacrificial layer 202 located on the top surface of the substrate 100 is patterned. Since the present application takes the sacrificial layer 202 formed in the first way as an example to describe the method for forming a semiconductor structure, at this time, the sacrificial layer 202 is still located on the top surface of the substrate 100. If the sacrificial layer 202 is formed in the second way, this step can be omitted.

[0049] refer to Figure 7 Based on the patterned mask layer 203 , a portion of the height of the substrate 100 is etched to form an opening 301 .

[0050] In the direction parallel to the substrate 100, the width of the opening 301 is based on the width of the pattern exposed by the patterned mask layer 203. Since the arrangement density of the through holes 201 located in the first area 110 is greater than the arrangement density of the through holes 201 located in the second area 120, accordingly, the width of the opening 301 formed in the first area 110 is smaller than the width of the opening 301 located in the second area 120, that is, in the direction parallel to the surface of the substrate 100, the width of the opening 301 located in the second area 120 is greater than the width of the opening 301 located in the first area 110. In this embodiment, even if located in the same area, the smaller the arrangement density of the through holes 201, the larger the width of the formed opening 301.

[0051] It should be noted that the depth of the opening 301 is controlled by the time of etching the substrate 100 . The longer the etching time is, the deeper the depth of the formed opening 301 is.

[0052] The arrangement density of the through holes 201 located in the first region 110 is large, and there are more through holes 201 in the substrate 100 of the same size, and the spacing between the through holes 201 is small, so the etching load effect in the first region 110 is large; the arrangement density of the through holes 202 located in the second region 120 is small, and there are fewer through holes 201 in the substrate 100 of the same size, and the spacing between the through holes 201 is large, so the etching load effect in the second region 120 is small. That is, due to different etching load effects, in the same etching time, the depths of the openings 301 etched in the first region 110 and the second region 120 are different, and the smaller the arrangement density of the through holes 201, the smaller the etching load effect, and the deeper the depth of the openings 301 formed around the through holes 201. After the openings 301 are formed, the patterned photoresist 204 and the patterned mask layer 203 are removed in sequence. In this embodiment, the remaining sacrificial layer 202 located on the top surface of the substrate 100 also needs to be removed.

[0053] In this embodiment, an etching process is used to sequentially remove the patterned photoresist 204, the patterned mask layer 203, and the remaining sacrificial layer 202 until the top surface of the substrate 100 is exposed. The etching process is used to ensure that the formed semiconductor structure is not subjected to excessive impact, thereby causing collapse and affecting the yield of the semiconductor structure. In other embodiments, the patterned photoresist, the patterned mask layer, and the remaining sacrificial layer can be removed by chemical mechanical polishing. The chemical mechanical polishing has a higher removal rate than the etching process, which is conducive to shortening the process cycle.

[0054] refer to Figure 8 , the sacrificial layer 202 is removed, and the opening 301 is connected with the corresponding through hole 201 to form a groove 302. The formed groove 302 includes a through hole 201 with a depth greater than the opening 301 and an opening 301 with a width greater than the through hole 201. It can be seen that the formed groove 302 is a Damascus structure.

[0055] In this embodiment, the formed Damascus structure exposes the conductive layer 101 in the substrate 100 , so that the conductive structure formed by subsequently filling the Damascus structure is electrically connected to the conductive layer 101 .

[0056] In this embodiment, hydrogen plasma is used to remove the sacrificial layer 202 .

[0057] In this embodiment, the hydrogen plasma used to remove the sacrificial layer 202 has only a chemical reaction effect, but no ion effect. Specifically, radio frequency ionization of hydrogen is used in the furnace tube device to form high-energy molecules and high-energy ions, and the directional high-energy ions are filtered out by a grid set in the furnace tube device, and the remaining hydrogen plasma is used to remove the sacrificial layer 202. Removing the sacrificial layer 202 by high-energy molecules can further improve the removal efficiency of the sacrificial layer 202.

[0058] Since the material of the sacrificial layer 202 formed in this embodiment includes polysilicon, the etching rate of hydrogen plasma on polysilicon is relatively high, and the etching rate on other semiconductor structures is extremely low, so in the process of removing the sacrificial layer 202 by etching with hydrogen plasma, there is a very large etching selectivity, and the etching selectivity is generally greater than 1000: 1. It can be considered that the hydrogen plasma only reacts with the sacrificial layer 202, and does not react with other structures in the substrate 100.

[0059] In addition, since the hydrogen plasma ion bombardment effect used to remove the sacrificial layer 202 is weak, the opening 301 will not continue to be etched, so that in the process of removing the sacrificial layer 202, the depth of the opening 301 will not change significantly. By preventing the formation of the formed semiconductor structure from changing, that is, the formed Damascus structure will not be destroyed, the yield of the formed semiconductor structure is improved.

[0060] It should be noted that, in other embodiments, if the material of the sacrificial layer is other semiconductor materials besides polysilicon, those skilled in the art have reason to select a plasma with a high selectivity ratio corresponding to the sacrificial layer material for etching. For example, an etching material with a relatively large etching selectivity between the sacrificial layer and the dielectric layer can be used to etch the sacrificial layer. Due to the large etching selectivity, during the etching process of the sacrificial layer, the depth of the opening will decrease, but the impact on the formed semiconductor structure is small.

[0061] Compared with the related art, by forming a sacrificial layer to fill the through hole, the height of the sacrificial layer filling the through hole is consistent, thereby ensuring that in the subsequent process of etching the Damascus structure based on the sacrificial layer, etching defects caused by different pattern densities are eliminated, thereby improving the yield of the semiconductor structure.

[0062] The above-mentioned various steps are divided only for the purpose of clear description. When implemented, they can be combined into one step or some steps can be split and decomposed into multiple steps. As long as they include the same logical relationship, they are all within the protection scope of this patent. Adding insignificant modifications to the process or introducing insignificant designs that do not change the core design of the process are all within the protection scope of this patent.

[0063] Those skilled in the art will appreciate that the above embodiments are specific embodiments for implementing the present invention, and that in actual applications, various changes may be made in form and detail without departing from the spirit and scope of the present invention.

Claims

1. A method for forming a semiconductor structure, characterized in that: include: Providing a substrate having a first region and a second region, wherein a plurality of discrete through holes are formed in the substrate, and an arrangement density of the through holes in the first region is greater than an arrangement density of the through holes in the second region; forming a sacrificial layer filling the through hole; Etching the substrate of a portion of the thickness around the sacrificial layer to form an opening, the opening surrounds the sacrificial layer, and in a direction perpendicular to the surface of the substrate, the depth of the opening is less than the depth of the through hole; and the smaller the arrangement density of the through holes, the deeper the depth of the opening formed around the through holes; The sacrificial layer is removed, and the opening is connected with the corresponding through hole to form a groove.

2. The method for forming a semiconductor structure according to claim 1, wherein: In a direction perpendicular to the surface of the substrate, the height of the sacrificial layer located in the first area is flush with the height of the sacrificial layer located in the second area, so as to form a sacrificial layer filling the through hole, comprising the following steps: forming a sacrificial film filling the through hole and covering the substrate; The sacrificial film is planarized, and the remaining sacrificial film serves as the sacrificial layer.

3. The method for forming a semiconductor structure according to claim 2, wherein: The sacrificial film is planarized until the top surface of the remaining sacrificial film is parallel to the top surface of the substrate.

4. The method for forming a semiconductor structure according to claim 2, wherein: The sacrificial film is planarized until the top surface of the substrate is exposed.

5. The method for forming a semiconductor structure according to claim 3 or 4, characterized in that: The planarization process is performed by chemical mechanical polishing.

6. The method for forming a semiconductor structure according to claim 1, wherein: The sacrificial layer is a hard mask formed by spin coating.

7. The method for forming a semiconductor structure according to claim 1, wherein: The material of the sacrificial layer includes polysilicon.

8. The method for forming a semiconductor structure according to claim 1, wherein: In a direction parallel to the surface of the substrate, a width of the opening located in the second region is greater than a width of the opening located in the first region.

9. The method for forming a semiconductor structure according to claim 6, wherein: The sacrificial layer is removed by using hydrogen plasma.

10. The method for forming a semiconductor structure according to claim 1, wherein: Etching the substrate to form an opening by a thickness of a portion around the sacrificial layer comprises the following steps: Forming a patterned mask layer on the top surface of the substrate, wherein in a direction parallel to the surface of the substrate, the orthographic projection of the pattern exposed by the patterned mask layer on the substrate completely covers the orthographic projection of the sacrificial layer on the substrate; Based on the patterned mask layer, etching a portion of the substrate at a height to form the opening; The patterned mask layer is removed.

11. The method for forming a semiconductor structure according to claim 10, characterized in that: Forming a patterned mask layer on the top surface of the sacrificial layer comprises the following steps: forming a mask layer on a top surface of the sacrificial layer; forming a patterned photoresist on the top surface of the mask layer, wherein the orthographic projection of the pattern exposed by the patterned photoresist on the substrate completely covers the orthographic projection of the sacrificial layer on the substrate; Based on the patterned photoresist, a portion of the mask layer is etched to form the patterned mask layer.