Diffusion method for silicon wafer and photovoltaic silicon wafer

Through the step-by-step temperature-raising deposition and push-junction treatment method, the problems of high surface doping concentration and low internal doping are solved, which significantly improves the efficiency and life of the photovoltaic cell and reduces the attenuation rate.

CN114497283BActive Publication Date: 2024-11-08TONGWEI SOLAR ENERGY (CHENGDU) CO LID
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202210117046.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-07
Publication Date
2024-11-08
Estimated Expiration
2042-02-07

AI Technical Summary

Technical Problem

The existing silicon wafer diffusion method is difficult to effectively reduce the surface doping concentration and increase the internal doping concentration, resulting in low photoconversion efficiency and high attenuation rate of photovoltaic cells.

Method used

Using step-by-step temperature-raising deposition and junction-pushing treatment methods, through two deposition treatments and two push-junction treatments, the doping substances are deposited in the inactive state and penetrated deep into the silicon wafer, reducing the surface doping concentration and increasing the internal doping. Miscellaneousness.

Benefits of technology

It significantly reduces the surface recombination of silicon wafers, improves the photoelectric conversion efficiency, extends the life of minor numbers, improves the photoconversion efficiency, current density and open circuit voltage of solar cells, and reduces the series and parallel internal resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114497283B_ABST
    Figure CN114497283B_ABST
Patent Text Reader

Abstract

The embodiment of the present application provides a diffusion method for silicon wafers and photovoltaic silicon wafers, which relate to the field of photovoltaic cells. The diffusion method for silicon wafers includes the following steps: firstly subjecting the pretreated silicon wafer to a deposition treatment at a temperature of 700-780°C, and then subjecting the silicon wafer to a secondary deposition treatment at a temperature of 720-800°C, wherein the temperature of the secondary deposition treatment is higher than that of the primary deposition treatment; then subjecting the silicon wafer to a push-junction treatment at a temperature of 800-840°C; then subjecting the silicon wafer to a secondary push-junction treatment at a temperature of 840-880°C; the temperature of the first push-junction treatment is higher than the temperature of the secondary deposition and lower than the temperature of the secondary push-junction treatment. The photovoltaic silicon wafer obtained by the diffusion method has a low surface doping concentration of the silicon wafer, a high and uniform internal doping concentration, a small surface recombination effect of the silicon wafer, and a long minority carrier lifetime. When used in solar cells, a solar cell with high light conversion efficiency can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of photovoltaic cells, and more specifically, to a diffusion method for silicon wafers and photovoltaic silicon wafers. Background Art

[0002] In crystalline silicon solar cells, the silicon wafer needs to be diffused to reduce the surface doping concentration of the silicon wafer and increase the internal doping concentration of the silicon wafer, thereby improving the light conversion efficiency of the cell and reducing the cell attenuation rate.

[0003] The current diffusion method cannot effectively reduce the surface doping concentration of silicon wafers, and it is difficult to further increase the internal doping concentration of silicon wafers. The light conversion efficiency of the battery still needs to be improved, and the attenuation rate of the battery efficiency still needs to be reduced. Summary of the invention

[0004] The purpose of the embodiments of the present application is to provide a diffusion method for silicon wafers and photovoltaic silicon wafers. After the silicon wafers are treated with the diffusion method, the surface doping concentration of the silicon wafers can be reduced and the internal doping concentration of the silicon wafers can be increased, thereby greatly reducing the surface recombination of the silicon wafers and increasing the minority carrier lifetime in the silicon wafers. When the photovoltaic silicon wafers are used to prepare photovoltaic cells, the energy conversion efficiency of the cells can be improved.

[0005] In a first aspect, an embodiment of the present application provides a diffusion method for a silicon wafer, which includes the following steps: first subjecting the pretreated silicon wafer to a primary deposition treatment, and then subjecting it to a secondary deposition treatment, wherein the temperature of the secondary deposition treatment is higher than the temperature of the primary deposition treatment; then subjecting the silicon wafer to a primary push-junction treatment; and subsequently subjecting the silicon wafer to a secondary push-junction treatment; the temperature of the primary push-junction treatment is higher than the temperature of the secondary deposition, and lower than the temperature of the secondary push-junction treatment.

[0006] In the above technical solution, the silicon wafer is subjected to deposition treatment, which can make the doping material deposited on the surface of the silicon wafer, facilitating the subsequent push-in treatment, and the temperature of the two deposition treatments is increased in a step-by-step manner, which can well ensure that during the deposition treatment, most of the doping materials on the surface of the silicon wafer are in an unactivated state.

[0007] First, the silicon wafer after deposition treatment is subjected to a push-junction treatment. At this time, the temperature of the push-junction treatment is higher than the temperature during the deposition treatment, which can activate the doping material and allow the doping material to enter the silicon wafer body; raising the temperature again for a second push-junction treatment can make the activated doping material further extend into the silicon wafer, which can effectively increase the doping degree inside the silicon wafer and reduce the doping concentration on the surface of the silicon wafer, which is beneficial to improving the photoelectric conversion efficiency of the silicon wafer.

[0008] In one possible implementation, the temperature of the first deposition process is 700-780°C; and / or, the temperature of the second deposition process is 720-800°C; and / or, the temperature of the first push-bonding process is 800-840°C; and / or, the temperature of the second push-bonding process is 840-880°C; and / or, the temperature of the second deposition process is 10-30°C higher than the temperature of the first deposition process; and / or, the temperature of the second push-bonding process is 20-40°C higher than the temperature of the first push-bonding process.

[0009] In the above technical scheme, the temperature of the two deposition treatments is within 800°C, which can make most of the doping substances on the surface of the silicon wafer in an activated state, and during the deposition treatment, the temperature difference between the first deposition treatment and the second deposition treatment cannot be too large or too small, and should be in the range of 10-30°C. If it is too large, the time is insufficient and the heating rate cannot reach the temperature. If it is too small, the total deposition time will be extended, and it is not conducive to improving the uniformity of the diffusion reaction; the temperature of the two push-junction treatments is above 800°C, which can activate the doping substances on the surface of the silicon wafer, and the temperature difference between the first push-junction and the second push-junction cannot be too large or too small, and should be in the range of 20-40°C. If it is too large, it is not conducive to controlling the junction depth. If the junction depth is too deep, the effective doping concentration is low and the uniformity is poor. If it is too small, the doping substances may not penetrate particularly deeply into the interior of the silicon wafer, and the doping uniformity inside the silicon wafer may also be poor.

[0010] In a possible implementation, the time for the first push-knot process is 360 to 700 seconds, and the time for the second push-knot process is 200 to 500 seconds, and the time for the first push-knot process is longer than that for the second push-knot process.

[0011] In the above technical solution, the time of the first push-junction treatment is longer than that of the second push-junction treatment, which is beneficial for the doping substances deposited on the surface of the silicon wafer to be activated and penetrate into the interior of the silicon wafer.

[0012] In a possible implementation, the step of deposition processing includes: a first deposition processing time is 200 to 500 seconds; and / or a second deposition processing time is 200 to 500 seconds.

[0013] In the above technical solution, since the deposition is performed twice according to the temperature, the deposition time each time can be maintained within a shorter range, which facilitates shortening the processing time of the silicon wafer.

[0014] In a possible implementation, the small nitrogen flow rate of the first deposition process is 500-1000 sccm; and / or the small nitrogen flow rate of the second deposition process is 500-1000 sccm.

[0015] In the above technical solution, since the deposition process is carried out in two steps, even if the flow rate of small nitrogen is increased, it can ensure that the doping degree on the silicon wafer surface will not be too high, so the flow rate of small nitrogen can be controlled at 500-1000sccm to improve the uniformity inside the silicon wafer.

[0016] In a possible implementation, the diffusion method also includes the following steps: oxidizing the silicon wafer after a deposition process, the oxidation time is 100 to 240 seconds; the oxidation temperature is greater than the temperature during the first deposition process and less than the temperature during the second deposition process; optionally, the oxidation temperature is 720 to 800°C.

[0017] In the above technical solution, the silicon wafer is oxidized between the first deposition process and the second deposition process to further reduce the diffusion surface concentration.

[0018] In a possible implementation, the pretreatment step of the silicon wafer includes: performing a pre-oxidation treatment on the silicon wafer at a temperature of 700 to 780° C. for a time of 200 to 400 seconds.

[0019] In the above technical solution, the silicon wafer is oxidized before a deposition process, which can reduce the surface concentration of the silicon wafer and improve the diffusion uniformity.

[0020] In a possible implementation, it also includes the following steps: performing three deposition processes on the silicon wafer after the second push-on treatment, at a temperature of 760-780° C. and a small nitrogen flow rate of 1200-2500 sccm.

[0021] In the above technical solution, after the secondary push-up treatment is completed, the silicon wafer is further subjected to a third deposition treatment, which can be coordinated with subsequent SE and other processes to further process the silicon wafer.

[0022] In a possible implementation, it also includes the following steps: after three deposition processes, post-oxidation treatment is performed on the silicon wafer, the time is 480 to 640 seconds, and the temperature is 760 to 780°C.

[0023] In a second aspect, an embodiment of the present application provides a photovoltaic silicon wafer, which is obtained after the silicon wafer is processed by the above-mentioned diffusion method.

[0024] In the above technical solution, the photovoltaic silicon wafer treated by the above method has a low surface doping concentration and a high and uniform internal doping concentration, which can reduce the surface recombination of the silicon wafer and increase the life of minority carriers. When used to prepare solar cells, the light conversion efficiency, current density, and open circuit voltage of the solar cell are significantly improved, and the series internal resistance and parallel internal resistance can also be effectively reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 This is a partial process flow chart of the diffusion method in the embodiment of the present application;

[0027] Figure 2 This is a comparison chart of the ECV curves of the photovoltaic silicon wafers in Example 1 and Comparative Example 7 of the present application. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0029] The photovoltaic silicon wafer and the processing method thereof according to the embodiment of the present application are described in detail below.

[0030] The embodiment of the present application provides a photovoltaic silicon wafer, which is obtained by treating the silicon wafer with a diffusion method. Since the diffusion method requires a series of specific operations such as heating, nitrogen, oxygen, and phosphorus, the silicon wafer is generally placed in a quartz boat and placed in a diffusion furnace for preparation. The diffusion method of the present application is as follows:

[0031] S110, first check whether the diffusion furnace is leaking;

[0032] S120, sending the textured silicon wafer into a diffusion furnace, and then heating it to 700-780°C;

[0033] S130, pre-oxidation: oxygen and nitrogen (i.e. pure nitrogen) are introduced into a diffusion furnace at 700-780°C. The oxygen flow rate is controlled at 500-1500sccm and the pressure is controlled at 50-150mbar. The purpose of introducing oxygen is to oxidize the silicon wafer, which can reduce the surface concentration of the silicon wafer and improve the diffusion uniformity. The time is generally controlled at 1-5min.

[0034] Figure 1 A partial process flow chart of the diffusion method in the embodiment of the present application is shown, mainly S140, deposition process and S141, push-in process, the two process steps are respectively:

[0035] S140, deposition process: the temperature is raised in stages, and the silicon wafer is subjected to two layer deposition processes, and the silicon wafer is also oxidized during the two deposition processes. The details are as follows:

[0036] S141. One deposition treatment: maintain the large nitrogen flow unchanged, control the oxygen flow at 500-1000sccm, increase the temperature and introduce small nitrogen, the small nitrogen flow is 500-1000sccm, and perform one deposition treatment on the silicon wafer after the pre-oxidation treatment for 200-500s; the temperature is controlled in the range of 700-780℃, and the temperature of the one deposition treatment is higher than the temperature of the pre-oxidation treatment, specifically, it can be 760-780℃.

[0037] S142, temperature increase and oxidation: maintain the large nitrogen flow unchanged, control the oxygen flow at 500-1500 sccm, increase the temperature and stop introducing small nitrogen, oxidize the silicon wafer after one deposition treatment for 100-240s, the temperature is generally controlled at 750-800°C, specifically, it can be 780-800°C.

[0038] S143, secondary deposition treatment: continue to increase the temperature and continue to introduce a small amount of nitrogen, the temperature is generally controlled at 720-800°C, specifically, it can be 780-800°C; the flow rate of the small amount of nitrogen is 500-1000sccm, and the treatment time is generally 200-500s.

[0039] During the deposition process, the temperature difference between the first deposition process and the second deposition process should be in the range of 10 to 30° C., so that the junction depth and the overall doping concentration can be controlled.

[0040] Large nitrogen is pure nitrogen; small nitrogen is nitrogen carrying phosphorus oxychloride, which is generally obtained by passing nitrogen through phosphorus oxychloride liquid; oxygen is pure oxygen; during deposition processing, small nitrogen is introduced to provide raw material phosphorus so that phosphorus can be deposited on the surface of the silicon wafer. Moreover, the flow rate of small nitrogen cannot be too large, otherwise it is easy to increase the doping concentration on the surface of the silicon wafer and increase the surface recombination of the silicon wafer, resulting in a decrease in conversion efficiency during the subsequent preparation of the battery; but the flow rate of small nitrogen cannot be too low, otherwise the phosphorus content is low, and it is not mixed enough in the gas, resulting in insufficient reaction, which leads to poor uniformity of the subsequent silicon wafer, and also affects the conversion efficiency of the battery; and too small a flow rate will also increase the processing time and increase the deposition temperature.

[0041] from Figure 1It can be seen that during the deposition process of the present application, the temperature is increased in a step-by-step manner, and different stages correspond to different temperatures. From the first deposition to oxidation and then to the second deposition, the temperature is gradually increased, so that during the deposition process, the flow rate of small nitrogen can be increased to 500-1000sccm, which will not increase the doping degree on the surface of the silicon wafer, and can also make the uniformity inside the silicon wafer better. Specifically, the small nitrogen flow rate can be 500sccm, 600sccm, 700sccm, 800sccm, 900sccm or 1000sccm. Moreover, the step-by-step temperature increase can also ensure that the silicon wafer can complete the deposition step within 800°C, so that most of the phosphorus source on the surface of the silicon wafer is in an unactivated state, ensuring that the phosphorus source will not be pushed into the inside of the silicon wafer during the deposition process.

[0042] S150, push-junction treatment: the temperature is raised in stages, and the silicon wafer is subjected to two layer push-junction treatments, as follows:

[0043] S151, one-time push-junction treatment: stop introducing small amounts of nitrogen and oxygen, adjust the large nitrogen flow rate to 1000-3000sccm, raise the temperature to 800-840°C and treat the silicon wafer for 360-700s.

[0044] S152, secondary push-junction treatment: heat the silicon wafer to 840-880°C for 200-500s. The time for the secondary push-junction treatment must be shorter than that for the primary push-junction treatment.

[0045] During the push-junction treatment, the temperature difference between the first push-junction treatment and the second push-junction treatment should be in the range of 20 to 40°C, so that the heating rate and the junction depth of the silicon wafer can be better controlled.

[0046] from Figure 1 It can be seen that the temperature of this application is also increased in a step-by-step manner during the push-junction treatment, and different stages correspond to different temperatures. During the first push-junction treatment, the temperature is 800℃~840℃, which can not only activate the phosphorus source and make the phosphorus source on the surface diffuse into the silicon wafer, but also ensure that the activity of the phosphorus source is low and will not penetrate deeply into the silicon wafer; this is conducive to improving the uniformity of the silicon wafer, and the time of the first push-junction treatment is relatively long, which is also conducive to improving the uniformity of the silicon wafer; during the second push-junction treatment, the temperature is 840~880℃, which can fully activate the phosphorus source, so that the doping elements can penetrate deeper into the silicon wafer, further improving the effective doping concentration inside the silicon wafer, which is conducive to improving the battery efficiency.

[0047] During the deposition process, the temperature is changed, and two step-by-step deposition processes are performed. At the end of the two deposition processes, two more push-up processes are performed (see the process flow chart). Figure 1), the synergistic effect of two deposition processes and two push-junction processes can greatly reduce the surface recombination phenomenon of photovoltaic silicon wafers, increase the life of minority carriers, and thus improve the light conversion efficiency of solar cells. Surface recombination is the phenomenon that minority carriers of semiconductors disappear on the surface, which will have a negative impact on the light conversion efficiency of solar cells.

[0048] S160, cooling: introducing oxygen with the oxygen flow rate controlled at 300-1000 sccm, and cooling the temperature in the diffusion furnace to below 800°C within 800-1500 seconds.

[0049] S170, three deposition treatments: further cool the temperature in the furnace to 760-780°C, adjust the large nitrogen flow rate to 500-1500sccm, and introduce small nitrogen, the oxygen flow rate is 500-1000sccm, the small nitrogen flow rate is 1200-2500sccm, and the silicon wafer is subjected to three deposition treatments for 480-640s.

[0050] During the third deposition process, the flow rate of small nitrogen is greater than that of the previous two deposition processes, that is, high-source low-temperature deposition. This can increase the concentration of unactivated reaction sources on the surface of the silicon wafer, which is beneficial to the SE process after the diffusion process. The subsequent SE process, through laser experiments, heavily doped the screen-printed area and lightly doped the non-printed area, can improve the battery efficiency, which will not be repeated here.

[0051] S180, post-oxidation treatment: maintain the temperature and large nitrogen flow unchanged, adjust the oxygen flow to 1000-3000sccm, stop introducing small nitrogen, oxidize the silicon wafer after three deposition treatments for 480-640s, and protect the silicon wafer after three deposition treatments.

[0052] S190, pressure adjustment and boat discharge: adjust the pressure in the furnace to atmospheric pressure, open the furnace door, and send the silicon wafer out of the diffusion furnace. Specifically, the pressure adjustment time is 60-180s, the temperature is 760-780°C, the oxygen flow rate is 1000-3000sccm, and the maximum nitrogen flow rate is 500-1500sccm; the boat discharge time is 400-600s, the temperature is 760-780°C, and the maximum nitrogen flow rate is 2000-4000sccm.

[0053] The silicon wafers processed by the above diffusion method can be used as photovoltaic silicon wafers in the field of solar cells to improve the light conversion efficiency of the cells.

[0054] The features and performance of the present application are further described in detail below in conjunction with the embodiments.

[0055] Example 1

[0056] This embodiment provides a photovoltaic silicon wafer, which is obtained by placing the silicon wafer in a quartz boat and treating it in a diffusion furnace by a diffusion method. The specific steps of the diffusion method are as follows in order:

[0057] 1. First check whether the diffusion furnace is leaking;

[0058] 2. Send the textured silicon wafer into the diffusion furnace and then heat it to 740℃;

[0059] 3. Pre-oxidation: Maintain the pressure in the furnace at 100 mbar, introduce oxygen and nitrogen for 3 minutes; the oxygen flow rate is 1000 sccm, and the nitrogen flow rate is 1000 sccm.

[0060] 4. Deposition treatment: a. Primary deposition treatment: raise the temperature to 760°C, introduce small nitrogen for 350 seconds, the small nitrogen flow rate is 750 sccm, and the treatment time is 350 seconds.

[0061] b. Temperature-raising oxidation: Stop introducing nitrogen and raise the temperature to 780°C for 170 seconds.

[0062] c. Secondary deposition treatment: Raise the temperature to 790°C, continue to introduce nitrogen, maintain the nitrogen flow rate at 750 sccm, and the treatment time is 350 s.

[0063] 5. Push-knot treatment: a. Push-knot treatment: stop introducing small nitrogen and oxygen, maintain the large nitrogen flow rate at 1000sccm, and heat to 820℃ for 530s.

[0064] b. Secondary push-knot treatment: heat to 860℃ and treat for 350s.

[0065] 6. Cooling: Introduce oxygen with an oxygen flow rate of 1000 sccm, and cool the temperature in the diffusion furnace to 780°C within 1000 seconds.

[0066] 7. Three deposition treatments: The temperature in the furnace is further cooled to 760°C, and a small amount of nitrogen is introduced with a flow rate of 1900 sccm. The silicon wafer is subjected to three deposition treatments for 560 seconds.

[0067] 8. Post-oxidation treatment: Stop introducing nitrogen and oxidize the silicon wafer for 560 seconds.

[0068] 9. Adjust the pressure to remove the boat: Use 120s to adjust the pressure in the furnace to atmospheric pressure and control the temperature at 760℃; then control the maximum nitrogen flow rate to 2000sccm and maintain the temperature at 760℃ for 400s, and finally take the silicon wafer out of the diffusion furnace.

[0069] Example 2

[0070] This embodiment provides a photovoltaic silicon wafer, which is obtained by treating the silicon wafer with a diffusion method. The specific steps of the diffusion method are different from those of Embodiment 1 mainly in that:

[0071] During the deposition process, the temperature of the first deposition process is 760°C, and the temperature of the second deposition process is 775°C, and the temperature difference between the two is 15°C.

[0072] Example 3

[0073] This embodiment provides a photovoltaic silicon wafer, which is obtained by treating the silicon wafer with a diffusion method. The specific steps of the diffusion method are different from those of Embodiment 1 mainly in that:

[0074] During the push-knot treatment, the temperature of the first push-knot treatment is 830°C, and the temperature of the second push-knot treatment is 840°C, and the temperature difference between the two is 10°C.

[0075] Comparative Example 1

[0076] This comparative example provides a photovoltaic silicon wafer, which is obtained by treating the silicon wafer with a diffusion method. The specific steps of the diffusion method are different from those of Example 1 mainly in that:

[0077] During the deposition process, the temperature of the secondary deposition process is 810°C.

[0078] Comparative Example 2

[0079] This comparative example provides a photovoltaic silicon wafer, which is obtained by treating the silicon wafer with a diffusion method. The specific steps of the diffusion method are different from those of Example 1 mainly in that:

[0080] Deposition treatment: Under the condition of a small nitrogen flow rate of 750 sccm, the temperature in the furnace was gradually increased from 760°C to 790°C within 870s.

[0081] Comparative Example 3

[0082] This comparative example provides a photovoltaic silicon wafer, which is obtained by treating the silicon wafer with a diffusion method. The specific steps of the diffusion method are different from those of Example 1 mainly in that:

[0083] Deposition treatment: a. Deposition: Heat to 760°C, introduce nitrogen for 350 seconds, nitrogen flow rate is 750 sccm, treatment time is 350 seconds. b. Temperature rise oxidation: Stop introducing nitrogen, heat to 780°C and treat for 170 seconds.

[0084] Comparative Example 4

[0085] This comparative example provides a photovoltaic silicon wafer, which is obtained by treating the silicon wafer with a diffusion method. The specific steps of the diffusion method are different from those of Example 1 mainly in that:

[0086] Deposition treatment: a. Temperature rise oxidation: heat to 780°C for 170s. b. Deposition: heat to 790°C, introduce nitrogen for 350s, with a nitrogen flow rate of 750sccm.

[0087] Comparative Example 5

[0088] This comparative example provides a photovoltaic silicon wafer, which is obtained by treating the silicon wafer with a diffusion method. The specific steps of the diffusion method are different from those of Example 1 mainly in that:

[0089] Push-junction treatment: stop introducing small amounts of nitrogen and oxygen, maintain a large nitrogen flow of 1000 sccm, and heat the diffusion furnace from 790°C to 860°C for 880 seconds.

[0090] Comparative Example 6

[0091] This comparative example provides a photovoltaic silicon wafer, which is obtained by treating the silicon wafer with a diffusion method. The specific steps of the diffusion method are different from those of Example 1 mainly in that:

[0092] Push-junction treatment: stop introducing small amounts of nitrogen and oxygen, maintain a large nitrogen flow of 1000 sccm, and keep the temperature of the diffusion furnace at 820°C for 530 seconds.

[0093] Comparative Example 7

[0094] This comparative example provides a photovoltaic silicon wafer, which is obtained by treating the silicon wafer with a diffusion method. The specific steps of the diffusion method are different from those of Example 1 mainly in that:

[0095] Push-knot treatment: a. First push-knot treatment: stop introducing nitrogen and oxygen, maintain nitrogen flow rate at 1000 sccm, temperature at 790℃ for 530s. b. Second push-knot treatment: heat to 860℃ for 350s.

[0096] In summary, the preparation conditions of the deposition process and the push-in process of Examples 1 to 3 and Comparative Examples 1 to 7 are shown in Table 1:

[0097] Table 1 Preparation conditions of deposition and push-in treatment in Examples 1 to 3 and Comparative Examples 1 to 7

[0098]

[0099]

[0100] Application Examples

[0101] The ECV curves of the photovoltaic silicon wafers in Example 2 and Comparative Example 5 were tested and compared using an ECV (Electrochemical capacitance-voltage profiler) tester. Figure 2 shown. Figure 2 In the figure, the horizontal axis is the junction depth and the vertical axis is the doping concentration. Figure 2 It can be seen that the surface doping concentration of the photovoltaic silicon wafer in Example 2 is lower, and the effective doping concentration inside the silicon wafer is high.

[0102] The photovoltaic silicon wafers in Examples 1 to 3 and Comparative Examples 1 to 7 were used to prepare solar cells. After being tested by a Halm tester, the parameter performance of the cells is shown in Table 2:

[0103] Table 2 Average performance parameters of photovoltaic silicon wafers made into batteries of Examples 1 to 3 and Comparative Examples 1 to 7

[0104]

[0105] In summary, the silicon wafer of the embodiment of the present application is prepared through two deposition steps and two push-in steps, which can greatly increase the light conversion efficiency.

[0106] The above description is only an embodiment of the present application and is not intended to limit the protection scope of the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A diffusion method for silicon wafers, It is characterized in that It includes the following steps: First, the pretreated silicon wafer is subjected to a deposition treatment, and then to a secondary deposition treatment, wherein the temperature of the first deposition treatment is 700-780°C, the temperature of the secondary deposition treatment is 720-800°C, the temperature of the secondary deposition treatment is 10-30°C higher than the temperature of the first deposition treatment, the time of the first deposition treatment is 200-500s, and the time of the secondary deposition treatment is 200-500s; the silicon wafer after the first deposition treatment is oxidized, and the oxidation time is 100-240s; the oxidation temperature is greater than the temperature of the first deposition treatment and less than the temperature of the secondary deposition treatment; The silicon wafer is then subjected to an oxygen-free primary push-bonding treatment; then the silicon wafer is subjected to a secondary push-bonding treatment, wherein the temperature of the primary push-bonding treatment is 800-840° C., and the temperature of the secondary push-bonding treatment is 840-880° C.; The temperature of the first push-knot treatment is higher than the temperature of the secondary deposition, and 20~40°C lower than the temperature of the secondary push-knot treatment. The time of the first push-knot treatment is 360~700s, and the time of the secondary push-knot treatment is 200~500s. The time of the first push-knot treatment is longer than that of the secondary push-knot treatment.

2. The diffusion method for silicon wafer according to claim 1, It is characterized in that The small nitrogen flow rate of the primary deposition process is 500-1000 sccm; and / or the small nitrogen flow rate of the secondary deposition process is 500-1000 sccm, and the small nitrogen is nitrogen gas carrying phosphorus oxychloride.

3. The diffusion method for silicon wafer according to claim 1, It is characterized in that The silicon wafer pretreatment step includes: performing a pre-oxidation treatment on the silicon wafer at a temperature of 700-780° C. for a time of 200-400 seconds.

4. The diffusion method for silicon wafer according to claim 1, It is characterized in that It also includes the following steps: The silicon wafer after the secondary push-on treatment is subjected to three deposition treatments at a temperature of 760-780° C. and a small nitrogen flow rate of 1200-2500 sccm, where the small nitrogen is nitrogen gas carrying phosphorus oxychloride.

5. The diffusion method for silicon wafer according to claim 4, It is characterized in that It also includes the following steps: after the three deposition processes, the silicon wafer is subjected to post-oxidation treatment, the time is 480-640s, and the temperature is 760-780°C.

6. A photovoltaic silicon wafer, It is characterized in that The silicon wafer is obtained after being treated by the diffusion method for silicon wafer as described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Diffusing process with low temperature, low surface concentration and high sheet resistance

    CN102945797A

  • High efficient solar cell preparation method

    CN103094419A

  • Solar cell emitter doping distribution method

    CN104716232A

  • Diffusion method of solar cell silicon chip

    CN106449868A

  • Efficient and low-cost solar battery diffusion process