A 4,4'-biphenyl bis(diphenyl phosphonate) flame retardant and preparation method thereof

By preparing 4,4'-biphenylbis(diphenylphosphonate) flame retardant, the problem of phosphoric acid or phosphonate flame retardant in the prior art affecting the mechanical properties of organic materials is solved, and in organic materials, it is realized Improves impact resistance, flexibility and fold resistance, and has the characteristics of high yield and low cost.

CN114516889BActive Publication Date: 2024-10-22韩飞
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210240312.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-10
Publication Date
2024-10-22
Estimated Expiration
2042-03-10

AI Technical Summary

Technical Problem

When existing phosphoric acid or phosphonate flame retardants are added to organic materials, it is easy to affect the mechanical properties of the material, resulting in reduced performance such as impact resistance, flexibility and fold resistance, and there are poor mixing of small molecules or large molecules. question.

Method used

Using 4,4'-biphenylbis(diphenylphosphonate) flame retardant and its preparation method, a medium molecular weight diphenyl phosphonate is prepared by Grignard reaction, oxidation and esterification steps, for use in Improve the mechanical properties of organic materials.

Benefits of technology

This flame retardant not only has good flame retardant effect, but also improves the impact resistance, flexibility and fold resistance of organic materials. At the same time, the preparation method is simple, the yield is high and the cost is low, and it is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003541262450000071
    Figure BDA0003541262450000071
  • Figure BDA0003541262450000072
    Figure BDA0003541262450000072
  • Figure BDA0003541262450000073
    Figure BDA0003541262450000073
Patent Text Reader

Abstract

The present invention relates to a kind of 4,4'-biphenyl bis (phosphonic acid diphenyl ester) flame retardant and preparation method thereof, described method comprises the following steps: 4,4'-dibromobiphenyl carries out Grignard reaction with magnesium powder in tetrahydrofuran, generates 4,4'-biphenyl bis (magnesium bromide), then adds phosphorus trichloride to react, generates 4,4'-biphenyl bis (phosphonic acid dichloride); High temperature oxidation is carried out in phenylphosphonic acid, generates 4,4'-biphenyl bis (phosphonic acid dichloride); Described 4,4'-biphenyl bis (phosphonic acid dichloride) and phenol carry out esterification reaction in catalyst and solvent, obtain described 4,4'-biphenyl bis (phosphonic acid diphenyl ester) flame retardant. The inventive method prepares a kind of novel flame retardant, can be applied to various organic materials, the flame retardant of the present invention not only has good flame retardant effect, and is used in various organic materials, can improve the mechanical properties such as impact resistance, flexibility, folding resistance of organic materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame retardants, and specifically relates to a 4,4'-biphenyl bis(diphenyl phosphonate) flame retardant and a preparation method thereof. Background Art

[0002] Phosphorus-based flame retardants have low toxicity and good flame retardant effect, and their usage is increasing. Various phosphoric acid or phosphonate flame retardants are emerging in an endless stream. Most phosphorus-based flame retardants are added to organic materials by addition, and the addition amount often reaches 10-40%. Therefore, the addition of small molecular weight phosphoric acid or phosphonate will inevitably affect the mechanical properties of organic materials, such as impact resistance, flexibility, folding resistance, etc. However, polyphosphates or polyphosphonates with too large molecular weight may affect the mechanical properties of organic materials due to poor mixing in organic materials. Therefore, from the perspective of material processing technology, phosphoric acid or phosphonate with too small or too large molecular weight will bring adverse factors to the mechanical properties of organic materials.

[0003] In view of the above reasons, the present invention is proposed. Summary of the invention

[0004] In order to solve the above problems existing in the prior art, the present invention provides a 4,4′-biphenyl bis(diphenyl phosphonate) flame retardant and a preparation method thereof. The flame retardant of the present invention can be used in various organic materials, not only has a good flame retardant effect, but also can improve the mechanical properties of organic materials such as impact resistance, flexibility, and folding resistance. It is a brand-new flame retardant.

[0005] The first object of the present invention is to provide a method for preparing a 4,4′-biphenyl bis(diphenyl phosphonate) flame retardant, wherein the method comprises the following steps:

[0006] (1) Preparation of 4,4′-biphenyl bis(dichlorophosphine): 4,4′-dibromobiphenyl is subjected to a Grignard reaction with magnesium powder in tetrahydrofuran to generate 4,4′-biphenyl bis(magnesium bromide), and phosphorus trichloride is added to the 4,4′-biphenyl bis(magnesium bromide) to react to generate 4,4′-biphenyl bis(dichlorophosphine);

[0007] (2) Preparation of 4,4′-biphenyl bis(phosphonyl dichloride): the 4,4′-biphenyl bis(phosphonyl dichloride) is subjected to high temperature oxidation in phenylphosphonic acid to generate 4,4′-biphenyl bis(phosphonyl dichloride);

[0008] (3) Preparation of 4,4′-biphenyl bis(diphenyl phosphonate): The 4,4′-biphenyl bis(phosphonyl dichloride) and phenol are subjected to an esterification reaction in the presence of a catalyst and a solvent, and then subjected to alkali washing, water washing, separation, color removal, and distillation to obtain the 4,4′-biphenyl bis(diphenyl phosphonate) flame retardant.

[0009] Furthermore, in step (1), the Grignard reaction temperature is 50-65° C., and the reaction time is 7-8 hours.

[0010] Furthermore, in step (1), the molar ratio of 4,4′-dibromobiphenyl to magnesium powder is 1:2-2.1, the molar ratio of 4,4′-biphenyl bis(magnesium bromide) to phosphorus trichloride is 1:4.8-7.3, and the mass ratio of 4,4′-dibromobiphenyl to tetrahydrofuran is 100:600-810.

[0011] Furthermore, in step (1), the temperature for the reaction of 4,4′-biphenyl bis(magnesium bromide) and phosphorus trichloride is 75-81° C., and the reaction time is 5-7 hours.

[0012] Furthermore, in step (2), the temperature of high temperature oxidation is 200-250° C., the reaction time is 5-7 hours, and the mass ratio of 4,4′-biphenylbis(dichlorophosphine) to phenylphosphonic acid is 100:250-355.

[0013] Furthermore, in step (3), the mass ratio of the total mass of 4,4′-biphenyl bis(phosphonyl dichloride) and phenol to the catalyst is 100:3-7, and the molar ratio of 4,4′-biphenyl bis(phosphonyl dichloride) to phenol is 1:4-5.5.

[0014] Furthermore, the catalyst described in step (3) is one of anhydrous magnesium trichloride, anhydrous aluminum trichloride, anhydrous zinc trichloride and anhydrous magnesium bromide.

[0015] Furthermore, the solvent in step (3) is one of benzene, toluene and xylene, and the mass ratio of 4,4′-biphenyl bis(phosphonic acid dichloride) to the solvent is 100:500-650.

[0016] Furthermore, in step (3), the alkali washing is performed with a potassium carbonate aqueous solution having a mass fraction of 2-8%, and the color removal is performed with an activated carbon elution column.

[0017] The second object of the present invention is to provide a 4,4′-biphenyl bis(diphenyl phosphonate) flame retardant prepared by the method.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The 4,4′-biphenyl bis(diphenyl phosphonate) prepared by the method of the present invention is a new type of flame retardant and can be applied to various organic materials. The flame retardant of the present invention not only has a good flame retardant effect, but also can be used in various organic materials to improve the mechanical properties of the organic materials such as impact resistance, flexibility, and folding resistance. The preparation method of the present invention is simple, has a high yield, a low production cost, and can be produced on a large scale. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0021] Example 1

[0022] The preparation method of a 4,4′-biphenyl bis(diphenyl phosphonate) flame retardant of this embodiment is as follows:

[0023] (1) Preparation of 4,4′-biphenyl bis(phosphine dichloride):

[0024] In a 500mL reactor, add 4.9g magnesium powder, 250g tetrahydrofuran, pass nitrogen, and start stirring. Heat to 50°C, slowly drop 31.2g 4,4′-dibromobiphenyl, set the reaction time to 6.0 hours, after the reaction, slowly drop into 100g phosphorus trichloride, then gradually heat to 78°C, reflux for 6 hours, filter to remove salt, then distill to remove tetrahydrofuran and excess phosphorus trichloride and other impurities, to obtain 4,4′-biphenyl bis(dichlorophosphine), molecular weight 355.98, yield 78.9%;

[0025] (2) Preparation of 4,4′-biphenyl bis(phosphonyl dichloride):

[0026] In a 500mL reactor, add 71.2g of 4,4′-biphenyl bis(dichlorophosphine) and 250g of anhydrous phenylphosphonic acid, stir with nitrogen, heat to 250°C, slowly introduce pure oxygen, observe the reflux, react for 6 hours, evaporate phenylphosphonic acid under reduced pressure, and obtain 4,4′-biphenyl bis(phosphonyl dichloride) with a molecular weight of 387.96 and a yield of 95.8%;

[0027] (3) Preparation of 4,4′-biphenyl bis(diphenyl phosphonate):

[0028] In a 500mL reactor, add 38.8g 4,4′-biphenyl bis(phosphonyl dichloride), 47g phenol, 5g anhydrous aluminum chloride, 250g benzene, pass nitrogen and stir, raise the temperature to 145°C, reflux for 8 hours, the hydrogen chloride gas generated in the process is carried by nitrogen through the tail pipe to the sodium hydroxide solution sealer, after the reaction is completed, filter to remove the solid catalyst in the liquid, and remove the solvent benzene and excess phenol under reduced pressure to obtain the crude product 4,4′-biphenyl bis(phosphonic acid diphenyl ester). Add 250g benzene to dissolve 4,4′-biphenyl bis(phosphonic acid diphenyl ester), wash with 4% potassium carbonate aqueous solution until alkaline, and then wash with deionized water until neutral, and let the extracted liquid enter the activated carbon decolorization filter column to remove the yellow substance. Benzene and a small amount of water were removed by rotary evaporation at 55°C to obtain white powder 4,4′-biphenyl bis(diphenyl phosphonate) with a molecular weight of 618.56, a yield of 94.4%, and an acid value of 0.021 mgKOH / g.

[0029] Example 2

[0030] The preparation method of a 4,4′-biphenyl bis(diphenyl phosphonate) flame retardant of this embodiment is as follows:

[0031] (1) Preparation of 4,4′-biphenyl bis(phosphine dichloride):

[0032] In a 500mL reactor, add 4.8g magnesium powder, 250g tetrahydrofuran, pass nitrogen, and start stirring. Raise the temperature to 57°C, slowly drop 31.2g 4,4′-dibromobiphenyl, set the reaction time to 7 hours, after the reaction is completed, slowly drop into 70g phosphorus trichloride, then gradually raise the temperature to 75°C, reflux for 7 hours, filter to remove salt, then distill to remove tetrahydrofuran and excess phosphorus trichloride and other impurities, and obtain 4,4′-biphenyl bis(dichlorophosphine), molecular weight 355.98;

[0033] (2) Preparation of 4,4′-biphenyl bis(phosphonyl dichloride):

[0034] In a 500mL reactor, add 71.2g of 4,4′-biphenyl bis(dichlorophosphine) and 250g of anhydrous phenylphosphonic acid, stir with nitrogen, heat to 250°C, slowly introduce pure oxygen, observe the reflux, react for 6 hours, evaporate phenylphosphonic acid under reduced pressure, and obtain 4,4′-biphenyl bis(phosphonyl dichloride) with a molecular weight of 387.96;

[0035] (3) Preparation of 4,4′-biphenyl bis(diphenyl phosphonate):

[0036] In a 500mL reactor, add 38.8g 4,4′-biphenyl bis(phosphonyl dichloride), 52g phenol, 3.5g anhydrous magnesium chloride, 250g toluene, pass nitrogen and stir, raise the temperature to 165°C, reflux for 6 hours, the hydrogen chloride gas generated in the process is carried by nitrogen through the tail pipe to the sodium hydroxide solution sealer, after the reaction is completed, filter to remove the solid catalyst in the liquid, and evaporate the solvent benzene and excess phenol under reduced pressure to obtain the crude product 4,4′-biphenyl bis(phosphonic acid diphenyl ester). Add 250g toluene to dissolve 4,4′-biphenyl bis(phosphonic acid diphenyl ester), wash with 2% potassium carbonate aqueous solution until alkaline, and then wash with deionized water until neutral, and let the extracted liquid enter the activated carbon decolorization filter column to remove the yellow substance. Toluene and a small amount of water were removed by rotary evaporation at 55°C to obtain white powder 4,4′-biphenyl bis(diphenyl phosphonate) with a molecular weight of 618.56, a yield of 94.4%, and an acid value of 0.021 mgKOH / g.

[0037] Example 3

[0038] The preparation method of a 4,4′-biphenyl bis(diphenyl phosphonate) flame retardant of this embodiment is as follows:

[0039] (1) Preparation of 4,4′-biphenyl bis(phosphine dichloride):

[0040] In a 500mL reactor, add 5.04g magnesium powder and 190g tetrahydrofuran, pass nitrogen, start stirring, heat to 65°C, slowly drop 31.2g 4,4′-dibromobiphenyl, set the reaction time to 7 hours, after the reaction, slowly drop into 90g phosphorus trichloride, then gradually heat to 81°C, reflux for 5 hours, filter to remove salt, then distill to remove tetrahydrofuran and excess phosphorus trichloride and other impurities, to obtain 4,4′-biphenyl bis(dichlorophosphine), molecular weight 355.98;

[0041] (2) Preparation of 4,4′-biphenyl bis(phosphonyl dichloride):

[0042] In a 500mL reactor, add 71.2g of 4,4′-biphenyl bis(dichlorophosphine) and 180g of anhydrous phenylphosphonic acid, stir with nitrogen, heat to 225°C, slowly introduce pure oxygen, observe the reflux, react for 5 hours, evaporate phenylphosphonic acid under reduced pressure, and obtain 4,4′-biphenyl bis(phosphonyl dichloride) with a molecular weight of 387.96;

[0043] (3) Preparation of 4,4′-biphenyl bis(diphenyl phosphonate):

[0044] In a 500mL reactor, add 38.8g 4,4′-biphenyl bis(phosphonyl dichloride), 47g phenol, 4.8g anhydrous zinc chloride, 200g xylene, and stir with nitrogen. Raise the temperature to 145°C and reflux for 8 hours. The hydrogen chloride gas generated in the process is carried by nitrogen through the tail pipe to the sodium hydroxide solution sealer. After the reaction is completed, remove the solid catalyst in the liquid by suction filtration, and remove the solvent benzene and excess phenol under reduced pressure to obtain the crude product 4,4′-biphenyl bis(phosphonic acid diphenyl ester). Add 250g xylene to dissolve 4,4′-biphenyl bis(phosphonic acid diphenyl ester), wash with 8% potassium carbonate aqueous solution until it is alkaline, and then wash with deionized water until it is neutral. The extracted liquid enters the activated carbon decolorization filter column to remove the yellow substance. Xylene and a small amount of water were removed by rotary evaporation at 55°C to obtain white powder 4,4′-biphenyl bis(diphenyl phosphonate) with a molecular weight of 618.56, a yield of 94.4%, and an acid value of 0.021 mgKOH / g.

[0045] Example 4

[0046] The preparation method of a 4,4′-biphenyl bis(diphenyl phosphonate) flame retardant of this embodiment is as follows:

[0047] (1) Preparation of 4,4′-biphenyl bis(dichlorophosphine): same as step (1) of Example 1;

[0048] (2) Preparation of 4,4′-biphenyl bis(phosphonoyl dichloride): Same as step (2) of Example 1;

[0049] (3) Preparation of 4,4′-biphenyl bis(diphenyl phosphonate):

[0050] In a 500mL reactor, add 38.8g 4,4′-biphenyl bis(phosphonyl dichloride), 42g phenol, 5.5g anhydrous magnesium bromide, 230g xylene, pass nitrogen and stir, raise the temperature to 145°C, reflux for 8 hours, the hydrogen chloride gas generated in the process is carried by nitrogen through the tail pipe to the sodium hydroxide solution sealer, after the reaction is completed, filter to remove the solid catalyst in the liquid, and evaporate the solvent benzene and excess phenol under reduced pressure to obtain the crude product 4,4′-biphenyl bis(phosphonic acid diphenyl ester). Add 250g xylene to dissolve 4,4′-biphenyl bis(phosphonic acid diphenyl ester), wash with 6% potassium carbonate aqueous solution until alkaline, and then wash with deionized water until neutral, and let the extracted liquid enter the activated carbon decolorization filter column to remove the yellow substance. Xylene and a small amount of water were removed by rotary evaporation at 55°C to obtain white powder 4,4′-biphenyl bis(diphenyl phosphonate) with a molecular weight of 618.56, a yield of 94.4%, and an acid value of 0.021 mgKOH / g.

[0051] Test Example 1

[0052] Control sample 1: dimethyl methylphosphonate (DMMP);

[0053] Test sample 1-4 is the 4,4′-biphenyl bis(diphenyl phosphonate) flame retardant prepared in Example 1-4.

[0054] Different PMMA samples were prepared by mixing control sample 1 and test samples 1-4 at a ratio of 40% with methyl methacrylate under the initiation of 0.1% ammonium persulfate initiator, and were recorded as control sample 1 and test samples 1-4 respectively.

[0055] (1) Flame retardancy test

[0056] The limiting oxygen index of PMMA samples was measured with reference to GB / T2406-2008 “Test method for combustion performance of plastics – oxygen index method”. The results are shown in Table 1.

[0057] Table 1

[0058] sample Test sample 1 Test sample 2 Test sample 3 Test sample 4 Control sample 1 LOI 43 42 44 41 31

[0059] LOI 28 is the flame retardant limiting oxygen index. From the data in Table 1, it can be seen that the performance of the PMMA sample prepared by using the flame retardant of the present invention is significantly better than that of dimethyl methylphosphonate.

[0060] (2) Impact resistance test

[0061] The PMMA materials made from the test samples 1-4 and the control sample 1 were respectively made into dumbbell-shaped specimens, and the simply supported beam notched impact strength (KJ / m2) of the samples was measured with reference to GB / T1043-92 "Hard Plastic Simply Supported Beam Impact Test Method". The results are shown in Table 2.

[0062] Table 2

[0063]

[0064] It can be seen from Table 2 that PMMA filled with 4,4′-biphenyl bis(diphenyl phosphonate) of the present invention has better impact strength than PMMA filled with dimethyl methylphosphonate (DMMP).

[0065] (3) Heat resistance test

[0066] The Vicat softening points of the PMMA samples were measured for the test samples 1-4 and the control sample 1 respectively according to GB / T1633-2000 "Determination of Vicat softening temperature (VST) of thermoplastics". The results are shown in Table 3.

[0067] Table 3

[0068]

[0069] It can be seen from Table 3 that the heat resistance of PMMA filled with 4,4′-biphenyl bis(diphenyl phosphonate) of the present invention is significantly better than that filled with dimethyl methylphosphonate (DMMP).

[0070] (4) Tensile Strength Test The PMMA materials prepared from the test samples 1-4 and the control sample 1 were respectively made into tensile specimens, and the tensile strength (Mpa) of the samples was measured with reference to GB / T1040.1-2018 “Test for Tensile Properties of Plastics”. The results are shown in Table 4.

[0071] Table 4

[0072]

[0073] It can be seen from Table 4 that PMMA filled with 4,4′-biphenyl bis(diphenyl phosphonate) of the present invention has better tensile strength than PMMA filled with dimethyl methylphosphonate (DMMP).

[0074] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing a 4,4'-biphenyl bis(diphenyl phosphonate) flame retardant, characterized in that: The method comprises the following steps: (1) Preparation of 4,4'-biphenyl bis(dichlorophosphine): 4,4'-dibromobiphenyl is subjected to a Grignard reaction with magnesium powder in tetrahydrofuran to generate 4,4'-biphenyl bis(magnesium bromide), and phosphorus trichloride is added to the 4,4'-biphenyl bis(magnesium bromide) to react to generate 4,4'-biphenyl bis(dichlorophosphine); (2) Preparation of 4,4'-biphenyl bis(phosphonyl dichloride): the 4,4'-biphenyl bis(phosphonyl dichloride) is subjected to high temperature oxidation in phenylphosphonic acid to generate 4,4'-biphenyl bis(phosphonyl dichloride); (3) Preparation of 4,4'-biphenyl bis(diphenyl phosphonate): the 4,4'-biphenyl bis(phosphonyl dichloride) and phenol are subjected to an esterification reaction in a catalyst and a solvent, followed by alkali washing, water washing, separation, color removal, and distillation to obtain the 4,4'-biphenyl bis(diphenyl phosphonate) flame retardant; In step (1), the molar ratio of 4,4'-dibromobiphenyl to magnesium powder is 1:2-2.1, the molar ratio of 4,4'-biphenyl bis(magnesium bromide) to phosphorus trichloride is 1:4.8-7.3, and the mass ratio of 4,4'-dibromobiphenyl to tetrahydrofuran is 100:600-810; the Grignard reaction temperature is 50-65°C, and the reaction time is 7-8 hours; In step (2), the temperature of high temperature oxidation is 200-250° C., the reaction time is 5-7 hours, and the mass ratio of 4,4'-biphenylbis(dichlorophosphine) to phenylphosphonic acid is 100:250-355; In step (3), the molar ratio of 4,4'-biphenyl bis(phosphonic acid dichloride) to phenol is 1:4-5.

5.

2. The method for preparing a 4,4'-biphenyl bis(diphenyl phosphonate) flame retardant according to claim 1, characterized in that: In step (1), the temperature for the reaction of 4,4'-biphenyl bis(magnesium bromide) and phosphorus trichloride is 75-81° C., and the reaction time is 5-7 hours.

3. The method for preparing a 4,4'-biphenyl bis(diphenyl phosphonate) flame retardant according to claim 1, characterized in that: In step (3), the mass ratio of the total mass of 4,4'-biphenyl bis(phosphonic acid dichloride) and phenol to the mass ratio of the catalyst is 100:3-7.

4. The method for preparing a 4,4'-biphenyl bis(diphenyl phosphonate) flame retardant according to claim 1, characterized in that: The catalyst described in step (3) is one of anhydrous magnesium trichloride, anhydrous aluminum trichloride, anhydrous zinc trichloride and anhydrous magnesium bromide.

5. The method for preparing a 4,4'-biphenyl bis(diphenyl phosphonate) flame retardant according to claim 1, characterized in that: The solvent described in step (3) is one of benzene, toluene and xylene, and the mass ratio of 4,4'-biphenyl bis(phosphonic acid dichloride) to the solvent is 100:500-650.

6. The method for preparing a 4,4'-biphenyl bis(diphenyl phosphonate) flame retardant according to claim 1, characterized in that: In step (3), the alkali washing adopts a potassium carbonate aqueous solution with a mass fraction of 2-8%, and the color removal adopts an activated carbon elution column.

7. A 4,4'-biphenyl bis(diphenyl phosphonate) flame retardant prepared by the method of any one of claims 1 to 6.