Aluminum-titanium foil rolling method and aluminum-titanium foil

The aluminum-titanium foil production method that combines multi-pass rolling and low-roughness rolls solves the problems of coarse surface lines and fractures of aluminum-titanium foil and improves production yield and quality.

CN114522978BActive Publication Date: 2024-10-22SNTO TECH GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210102697.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-27
Publication Date
2024-10-22
Estimated Expiration
2042-01-27

AI Technical Summary

Technical Problem

In the production process of aluminum titanium foil, the traditional rolling method causes the surface texture of aluminum titanium foil to be rough, the production yield rate is reduced, and it is easy to break, resulting in an increase in scrap products.

Method used

Use a multi-pass rolling method to gradually reduce the thickness of the aluminum-titanium coils, and use rolls with lower surface roughness in the fourth pass of rolling. Combined with the temperature and spraying of cooling lubricating oil, the rolling parameters are adjusted to Reduce deformation and lines.

Benefits of technology

Effectively reduce the surface lines of aluminum titanium foil, improve production yield, reduce fractures, and improve the quality and strength of aluminum titanium foil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114522978B_ABST
    Figure CN114522978B_ABST
Patent Text Reader

Abstract

The present application provides an aluminum-titanium foil rolling method and an aluminum-titanium foil, the aluminum-titanium foil rolling method comprising the steps of: a first rolling pass, placing an aluminum-titanium coil having a titanium weight percentage greater than or equal to 0.05% and less than or equal to 0.10% into a rolling mill for rolling, and spraying cooling lubricating oil on the aluminum-titanium coil during the rolling process to form an aluminum-titanium coil having a thickness greater than or equal to 99 μm and less than or equal to 101 μm. A second rolling pass, a third rolling pass, coiling and a fourth rolling pass, placing the coiled aluminum-titanium coil into a rolling mill for rolling to form an aluminum-titanium foil having a thickness greater than or equal to 5.9 μm and less than or equal to 6.7 μm. The rolling reduction in the first and second passes is higher than the conventional reduction, so the rolling reduction in the fourth pass will be lower than the conventional one. The reduction in the deformation of the aluminum-titanium coil in the fourth rolling pass can improve the yield of the aluminum-titanium foil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of aluminum-titanium foil production, and in particular to an aluminum-titanium foil rolling method and aluminum-titanium foil. Background Art

[0002] Aluminum-titanium foil is a product made by precisely adding titanium metal to aluminum alloy. Compared with traditional aluminum foil, aluminum-titanium foil increases the weight proportion of titanium, making it antibacterial and sterilizing. It is suitable for baking, cooking, grilling, freezing, wrapping, storage and other application scenarios.

[0003] Since the weight ratio of titanium in aluminum-titanium foil is higher than that of traditional aluminum foil, the hardness and strength of aluminum-titanium foil are greater than those of aluminum foil. In the production of aluminum-titanium foil, if the traditional rolling method is used, the surface texture of aluminum-titanium foil will be coarse. Even during the rolling process, the aluminum-titanium foil will break, resulting in an increase in waste and a decrease in production yield. Summary of the invention

[0004] In view of this, it is necessary to provide an aluminum-titanium foil rolling method that can reduce the surface texture of the aluminum-titanium foil and improve the yield of the aluminum-titanium foil.

[0005] The embodiment of the present application provides an aluminum-titanium foil rolling method, which includes the following steps: a first rolling pass, rolling an aluminum-titanium coil having a titanium weight percentage greater than or equal to 0.05% and less than or equal to 0.10% and a thickness greater than or equal to 218 μm and less than or equal to 222 μm, to form an aluminum-titanium coil having a thickness greater than or equal to 99 μm and less than or equal to 101 μm. A second rolling pass, rolling the aluminum-titanium coil that has undergone the first rolling pass, the thickness of the aluminum-titanium coil after rolling is greater than or equal to 41 μm and less than or equal to 43 μm. A third rolling pass, rolling the aluminum-titanium coil that has undergone the second rolling pass, the thickness of the aluminum-titanium coil after rolling is greater than or equal to 15 μm and less than or equal to 15.4 μm. Rolling, rolling two aluminum-titanium coils that have undergone the third rolling pass. In the fourth rolling process, the aluminum-titanium coil is rolled to form an aluminum-titanium foil having a thickness greater than or equal to 5.9 μm and less than or equal to 6.7 μm.

[0006] In the aluminum-titanium foil rolling method of the above embodiment, the rolling reduction of the first and second passes is higher than the conventional rolling reduction, so when making aluminum-titanium foil of the same thickness, the rolling reduction of the fourth pass of the present application will be lower than the conventional rolling reduction. The reduction in the deformation of the aluminum-titanium coil in the fourth rolling pass can reduce the occurrence of grain in the aluminum-titanium foil, reduce the occurrence of aluminum-titanium foil breakage, and improve the aluminum-titanium foil yield.

[0007] In at least one embodiment, the fourth rolling pass is performed by a rolling mill, and the surface roughness Ra value of the roller of the rolling mill is greater than or equal to 0.058 μm and less than or equal to 0.063 μm.

[0008] In the aluminum-titanium foil rolling method of the above embodiment, the surface roughness of the roller in the fourth rolling pass is lower than that of the traditional roller, so that the surface roughness of the aluminum-titanium foil after the fourth rolling pass is lower, effectively reducing the generation of aluminum-titanium foil texture.

[0009] In at least one embodiment, the first rolling pass, the second rolling pass, the third rolling pass, the coil closing and the fourth rolling pass all require spraying cooling lubricating oil on the aluminum-titanium coil or the aluminum-titanium coil.

[0010] In the aluminum-titanium foil rolling method of the above embodiment, the aluminum-titanium coil or aluminum-titanium coil can be cooled and the roughness can be reduced by cooling the lubricating oil, thereby improving the quality of the aluminum-titanium coil or aluminum-titanium coil after rolling.

[0011] In at least one embodiment, the temperature of the cooling lubricating oil in the first rolling pass, the second rolling pass, and the third rolling pass is greater than or equal to 30°C and less than or equal to 38°C.

[0012] In the aluminum-titanium foil rolling method of the above embodiment, the temperature is lowered and the friction coefficient is reduced by cooling the lubricating oil, so that the rolling mill can stably roll the aluminum-titanium coil.

[0013] In at least one embodiment, the temperature of the cooling lubricating oil in the fourth rolling pass is greater than or equal to 45°C and less than or equal to 52°C.

[0014] In the aluminum-titanium foil rolling method of the above embodiment, the oil temperature of the cooling lubricating oil is lower than the traditional oil temperature, which can more effectively reduce the temperature during the fourth rolling.

[0015] In at least one embodiment, the first rolling pass has a speed greater than or equal to 600 m / min and less than or equal to 800 m / min, the second rolling pass has a speed greater than or equal to 850 m / min and less than or equal to 1050 m / min, the third rolling pass has a speed greater than or equal to 1050 m / min and less than or equal to 1250 m / min, and the fourth rolling pass has a speed greater than or equal to 500 m / min and less than or equal to 800 m / min.

[0016] In at least one embodiment, the rolling force of the first rolling pass is greater than or equal to 190T and less than or equal to 210T, the rolling force of the second rolling pass is greater than or equal to 200T and less than or equal to 220T, the rolling force of the third rolling pass is greater than or equal to 250T and less than or equal to 290T, and the rolling force of the fourth rolling pass is greater than or equal to 235T and less than or equal to 265T.

[0017] In at least one embodiment, the tension before the first rolling pass is greater than or equal to 2.5 kg / mm 2 And less than or equal to 4kg / mm 2 The second rolling tension is greater than or equal to 3.0 kg / mm 2 And less than or equal to 6.0kg / mm 2 , the tension before the third rolling is greater than or equal to 4.0kg / mm 2 And less than or equal to 7.5kg / mm 2 , the tension before the fourth rolling is greater than or equal to 4.0kg / mm 2 And less than or equal to 6.5kg / mm 2 .

[0018] In at least one embodiment, the aluminum-titanium coil also includes iron, silicon, copper and aluminum, the weight percentage of iron is greater than or equal to 0.7% and less than or equal to 1.1%, the weight percentage of silicon is greater than or equal to 0.2% and less than or equal to 0.3%, and the weight percentage of copper is greater than or equal to 0.01% and less than or equal to 0.03%.

[0019] In the aluminum-titanium foil rolling method of the above embodiment, the aluminum-titanium coil contains titanium, silicon, iron, copper and aluminum. After the aluminum-titanium foil rolling method, the aluminum-titanium foil has an antibacterial effect and better strength and ductility.

[0020] In at least one embodiment, the cooling lubricant oil includes kerosene and ester alcohol additives.

[0021] In the aluminum-titanium foil rolling method of the above embodiment, the cooling lubricating oil can not only cool down the temperature, but also reduce the friction.

[0022] An embodiment of the present application further provides an aluminum-titanium foil formed by the aluminum-titanium foil rolling method, wherein the weight proportion of titanium in the aluminum-titanium foil is greater than or equal to 0.05% and less than or equal to 0.10%.

[0023] In the aluminum-titanium foil of the above embodiment, the weight proportion of titanium is high, so that the aluminum-titanium foil has antibacterial and antimicrobial effects, and is suitable for various application scenarios such as baking, cooking, grilling, freezing, wrapping, and storage.

[0024] The aluminum-titanium foil rolling method of the present application increases the rolling reduction of the first and second passes, so that when producing aluminum-titanium foil of the same thickness, the rolling reduction of the fourth pass is reduced. This allows the product to be obtained by only four rolling passes, while reducing the generation of lines on the aluminum-titanium foil, reducing the surface roughness of the aluminum-titanium foil, and improving the aluminum-titanium foil yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a flow chart of the method for making aluminum-titanium foil of the present application. DETAILED DESCRIPTION

[0026] The technical solutions in the embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments.

[0027] It should be noted that when a component is considered to be "connected" to another component, it may be directly connected to the other component or there may be a central component at the same time. When a component is considered to be "located on" another component, it may be directly located on the other component or there may be a central component at the same time. The terms "top", "bottom", "upper", "lower", "left", "right", "front", "back", and similar expressions used herein are for illustrative purposes only.

[0028] When a parameter is greater than, equal to, or less than a certain endpoint value, it should be understood that the endpoint value is allowed to have a tolerance of ±10%. For example, if the ratio of A to B is greater than 10, it should be understood to include the case where the ratio of A to B is greater than 9, and also include the case where the ratio of A to B is greater than 11.

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0030] Some embodiments of the present application provide an aluminum-titanium foil rolling method, which includes the following steps: a first rolling pass, rolling an aluminum-titanium coil having a titanium weight percentage greater than or equal to 0.05% and less than or equal to 0.10% and a thickness greater than or equal to 218 μm and less than or equal to 222 μm, to form an aluminum-titanium coil having a thickness greater than or equal to 99 μm and less than or equal to 101 μm. A second rolling pass, rolling the aluminum-titanium coil that has undergone the first rolling pass, the thickness of the aluminum-titanium coil after rolling is greater than or equal to 41 μm and less than or equal to 43 μm. A third rolling pass, rolling the aluminum-titanium coil that has undergone the second rolling pass, the thickness of the aluminum-titanium coil after rolling is greater than or equal to 15 μm and less than or equal to 15.4 μm. Rolling, rolling two aluminum-titanium coils that have undergone the third rolling pass. In the fourth rolling process, the aluminum-titanium coil is rolled to form an aluminum-titanium foil having a thickness greater than or equal to 5.9 μm and less than or equal to 6.7 μm.

[0031] In the above-mentioned aluminum-titanium foil rolling method, the rolling reduction of the first and second passes is higher than the conventional rolling reduction, so when making aluminum-titanium foil of the same thickness, the rolling reduction of the fourth pass of the present application will be lower than the conventional rolling reduction. The reduction of the deformation of the aluminum-titanium coil in the fourth rolling pass can reduce the occurrence of grain in the aluminum-titanium foil, reduce the occurrence of aluminum-titanium foil breakage, and improve the aluminum-titanium foil yield.

[0032] Some embodiments of the present application will be described below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments may be combined with each other.

[0033] See also Figure 1 In one embodiment, a method for rolling an aluminum-titanium foil is provided, comprising the following steps:

[0034] S1. Casting and rolling composition adjustment

[0035] Charging: charging solid materials into the smelting furnace, including aluminum ingots and scrap aluminum;

[0036] Melting: After heating to 710-750℃, the solid material melts into high-temperature molten liquid;

[0037] Adjust the composition: add aluminum silicon alloy, iron agent, aluminum titanium alloy and copper agent according to the calculation of the composition of aluminum titanium foil, and adjust the composition of high temperature melt by adding aluminum silicon alloy, iron agent, aluminum titanium alloy and copper agent; the composition range of aluminum titanium foil is as follows by weight percentage: Fe: 0.7-1.1%, Si: 0.2-0.3%, Cu: 0.01-0.03%, Ti: 0.05-0.10%, and the balance is Al and impurities;

[0038] Sampling and testing: After stirring and slagging, samples are taken to obtain samples of the high-temperature molten solution after the composition is adjusted. The chemical composition of the samples is tested using a direct reading spectrometer to confirm whether the composition of the aluminum-titanium liquid (i.e., the high-temperature molten solution) meets the composition standards;

[0039] Preparation of aluminum-titanium coils: Pour the aluminum-titanium liquid that meets the composition standards in the smelting furnace into the holding furnace. Before pouring, confirm that the aluminum-titanium liquid temperature in the furnace is within the range of 740-755°C. Then, after refining, degassing, slagging, filtering, and casting and rolling processes, the finished aluminum-titanium coil with a thickness of 6.5-7.0mm is produced;

[0040] S2, cold rolling: the aluminum titanium coil is rolled through two passes to a thickness of 2.4±0.2mm;

[0041] S3. First annealing: Circulating air heats the aluminum-titanium coil with a thickness of 2.4±0.2mm to 540-570℃ and keeps it at that temperature for 2-4h, and then cools the aluminum-titanium coil to room temperature; the heating rate of the aluminum-titanium coil gradually decreases as the temperature difference between the aluminum-titanium coil and the furnace increases, that is, the heating rate gradually decreases as the temperature increases;

[0042] S4, cold rolling intermediate pass: the aluminum titanium coil after the first annealing is rolled through two passes to a thickness of 0.55±0.05mm;

[0043] S5. Second annealing: heat the aluminum-titanium coil with a thickness of 0.55±0.05mm with circulating air to 280-340℃ and keep it warm for 1.5-3.5h, and then cool the aluminum-titanium coil to room temperature;

[0044] S6, cold rolling finished product pass: the aluminum titanium coil after the second annealing is rolled through one pass, and the rolling thickness is 0.24±0.02mm;

[0045] S7, finishing and trimming: send the aluminum-titanium coil after the cold rolling pass to the re-coiling equipment for shearing to produce aluminum-titanium coils of required width;

[0046] S8, first rolling: put the aluminum titanium coil after finishing and trimming into the rolling mill for rough rolling, and spray cooling lubricating oil on the aluminum titanium coil during the rough rolling process to form a thickness of 0.1±0.01mm. The rolling force of the rolling mill on the aluminum titanium coil is greater than or equal to 190T and less than or equal to 230T.

[0047] Optionally, in some embodiments, the rolling force of the rolling mill on the aluminum-titanium coil is 220T. It can be understood that the rolling force of the rolling mill on the aluminum-titanium coil is not limited to this, and can also be 200T, 225T, 228.3T, etc.

[0048] The tension before the first rolling is greater than or equal to 2.5kg / mm 2 And less than or equal to 4kg / mm 2.

[0049] Optionally, in some embodiments, the tension before the first rolling is 3.0 kg / mm 2 It is understandable that the tension before the first rolling can also be 2.8, 3.3, 3.67 kg / mm 2 wait.

[0050] The speed of the first rolling pass is greater than or equal to 600 m / min and less than or equal to 800 m / min.

[0051] Optionally, in some embodiments, the speed of the first rolling pass is 700 m / min. It is understandable that the speed of the first rolling pass is not limited thereto, and may also be 650, 750 m / min, etc.

[0052] Second rolling: The aluminum-titanium coil after rough rolling is put into the rolling mill again for a second rough rolling, and cooling lubricating oil is sprayed on the aluminum-titanium coil during the second rough rolling. After the second rough rolling, the thickness of the aluminum-titanium coil is 0.042mm±0.001mm.

[0053] Optionally, in some embodiments, the thickness of the aluminum-titanium coil after the second rough rolling is 0.042 mm. It is understandable that the thickness of the aluminum-titanium coil after the second rough rolling is not limited thereto, and may also be 0.0415 mm, 0.04235 mm, etc.

[0054] The rolling force of the rolling mill on the aluminum-titanium coil in the second rough rolling is greater than or equal to 200T and less than or equal to 220T.

[0055] Optionally, in some embodiments, the rolling force of the rolling mill for the second rough rolling of the coil is 210T, which is the same as the rolling force of the first rough rolling. It is understandable that the rolling force of the rolling mill for the second rough rolling of the coil is not limited thereto, and can also be 205T, 215T, 218.3T, etc.

[0056] The tension before the second rolling is greater than or equal to 3.0kg / mm 2 And less than or equal to 6.0kg / mm 2 .

[0057] Optionally, in some embodiments, the tension before the second rolling is 4.0 kg / mm 2 It is understandable that the tension before the second rolling can also be 3.8, 4.3, 5.67 kg / mm 2 wait.

[0058] The speed of the second rolling pass is greater than or equal to 850 m / min and less than or equal to 1050 m / min.

[0059] Optionally, in some embodiments, the speed of the first rolling pass is 1000 m / min. It is understandable that the speed of the first rolling pass is not limited thereto, and may also be 900, 950 m / min, etc.

[0060] The third rolling pass: the aluminum-titanium coil that has undergone the second rolling pass is placed in the rolling mill for intermediate rolling and sprayed with cooling lubricating oil. The thickness of the aluminum-titanium coil after the intermediate rolling is 15.2μm±0.2μm.

[0061] Optionally, in some embodiments, the thickness of the aluminum-titanium coil after medium rolling is 15.2 μm. It is understandable that the thickness of the aluminum-titanium coil after medium rolling is not limited thereto, and may also be 15.25 μm, 15.3 μm, etc.

[0062] The rolling force of the aluminum-titanium coil rolled by the rolling mill is greater than or equal to 290T and less than or equal to 250T.

[0063] Optionally, in some embodiments, the rolling force of the coil rolled by the rolling mill is 270 T. It is understandable that the rolling force of the coil rolled by the rolling mill is not limited thereto, and may also be 260 T, 275 T, 280.3 T, etc.

[0064] The tension before medium rolling is greater than or equal to 4.0kg / mm 2 And less than or equal to 7.5kg / mm 2 .

[0065] Optionally, in some embodiments, the tension before medium rolling is 6.0 kg / mm 2 It is understandable that the tension before medium rolling can also be 5.0, 5.5, 7.0 kg / mm 2 wait.

[0066] The speed of the intermediate rolling is greater than or equal to 1050 m / min and less than or equal to 1250 m / min.

[0067] Optionally, in some embodiments, the speed of the intermediate rolling is 1100 m / min. It is understandable that the speed of the intermediate rolling is not limited thereto, and may also be 1088, 1200 m / min, etc.

[0068] The temperature of the cooling lubricating oil in the rough rolling and the intermediate rolling is greater than or equal to 30°C and less than or equal to 38°C.

[0069] S9, coiling: the two aluminum-titanium coils after the third rolling are coiled on a coiling device, and lubricating oil is applied to the contacting side of the two aluminum-titanium coils during the coiling process;

[0070] S10, the fourth rolling pass: the aluminum-titanium coil after coiling is placed in a rolling mill for finish rolling, and cooling lubricating oil is sprayed on it. After the finish rolling, an aluminum-titanium foil is formed, and the thickness of the aluminum-titanium foil is 6.3±0.4 μm.

[0071] Optionally, in some embodiments, the thickness of the aluminum-titanium foil after fine rolling is 6.3 μm. It is understandable that the thickness of the aluminum-titanium foil after fine rolling is not limited thereto, and may also be 6.0 μm, 6.56 μm, etc.

[0072] The rolling force of the aluminum-titanium coil finished by the rolling mill is greater than or equal to 235T and less than or equal to 265T.

[0073] Optionally, in some embodiments, the rolling force of the rolling mill for finishing rolling is 250 T. It is understandable that the rolling force of the rolling mill for finishing rolled coils is not limited thereto, and may also be 240 T, 244 T, 260.3 T, etc.

[0074] The tension before finishing rolling is greater than or equal to 4.0kg / mm 2 And less than or equal to 6.5kg / mm 2 .

[0075] Optionally, in some embodiments, the tension before finishing rolling is 5.5 kg / mm 2 It is understandable that the tension before finishing rolling can also be 4.3, 5.8, 6.3 kg / mm 2 wait.

[0076] The speed of the finish rolling is greater than or equal to 500 m / min and less than or equal to 800 m / min.

[0077] Optionally, in some embodiments, the finishing rolling speed is 750 m / min. It will be appreciated that the finishing rolling speed is not limited thereto, and may also be 600, 700 m / min, etc.

[0078] The surface roughness Ra value of the roller of the finishing rolling mill is greater than or equal to 0.058μm and less than or equal to 0.063μm. The surface roughness of the roller of the finishing rolling mill is lower than that of the traditional one, which can improve the smoothness of the surface of the aluminum titanium foil and reduce or even eliminate the grain of the aluminum titanium foil. The temperature of the cooling lubricating oil is greater than or equal to 48℃ and less than or equal to 55℃.

[0079] Optionally, in some embodiments, the temperature of the cooling lubricating oil for finishing rolling is 52° C. It is understandable that the temperature of the cooling lubricating oil is not limited thereto, and may also be 49, 53° C., etc.

[0080] The temperature of the cooling lubricant can affect the overall size of the rolling force, tension and speed. When the temperature decreases, the rolling force, tension and speed can be reduced as a whole. For example, when the temperature of the cooling lubricant decreases, the rolling force and tension can remain unchanged while the speed decreases. Or the tension and speed remain unchanged while the rolling force decreases.

[0081] The temperature of the cooling lubricating oil in S10 is lower than that of the oil in conventional finishing rolling, thereby improving the quality of the aluminum-titanium foil by affecting the overall rolling force, tension and speed.

[0082] S11, slitting: feeding the aluminum-titanium foil roll into a slitting machine, and slitting the aluminum-titanium foil roll into required specifications and models by the slitting machine;

[0083] S12. Third annealing: anneal the aluminum-titanium foil coil after slitting, heat the aluminum-titanium foil to 190-220°C with circulating air and keep it warm for 5-10 hours, and then air-cool the aluminum-titanium foil to room temperature.

[0084] The specific parameters of the aluminum-titanium foil rolling method provided in this application are shown in Table 1:

[0085]

[0086] To summarize, an aluminum-titanium foil rolling method is provided in an embodiment of the present application. By increasing the rolling reduction in the first and second passes, the rolling reduction in the third and fourth passes can be reduced, and a roller with a lower surface roughness is used in the fourth rolling pass, thereby reducing the occurrence of lines on the surface of the aluminum-titanium foil, reducing the roughness of the product surface, and improving the yield of the aluminum-titanium foil.

[0087] The embodiment of the present application also provides an aluminum-titanium foil, which is formed by the aluminum-titanium foil rolling method of any of the above embodiments, and thus has the advantages of less texture and high quality. The aluminum-titanium foil includes titanium, iron, silicon, copper and aluminum, wherein the weight percentage of titanium is greater than or equal to 0.05% and less than or equal to 0.10%. The weight percentage of iron is greater than or equal to 0.7% and less than or equal to 1.1%, the weight percentage of silicon is greater than or equal to 0.2% and less than or equal to 0.3%, and the weight percentage of copper is greater than or equal to 0.01% and less than or equal to 0.03%.

[0088] In addition, those skilled in the art should recognize that the above embodiments are only used to illustrate the present application, and are not intended to limit the present application. As long as they are within the spirit of the present application, appropriate changes and modifications to the above embodiments are within the scope of the present application.

Claims

1. A method for rolling aluminum-titanium foil, It is characterized in that The steps include: In the first rolling pass, an aluminum-titanium coil having a titanium weight percentage greater than or equal to 0.05% and less than or equal to 0.10% and a thickness greater than or equal to 218 μm and less than or equal to 222 μm is rolled, and cooling lubricating oil is sprayed to form an aluminum-titanium coil having a thickness greater than or equal to 99 μm and less than or equal to 101 μm, a rolling force of the first rolling pass greater than or equal to 190 T and less than or equal to 210 T, and a temperature of the cooling lubricating oil in the first rolling pass greater than or equal to 30° C. and less than or equal to 38° C.; The second rolling process is to roll the aluminum-titanium coil that has been rolled in the first rolling process and spray the cooling lubricating oil, wherein the thickness of the aluminum-titanium coil after rolling is greater than or equal to 41 μm and less than or equal to 43 μm, the rolling force of the second rolling process is greater than or equal to 200 T and less than or equal to 220 T, and the temperature of the cooling lubricating oil in the second rolling process is greater than or equal to 30° C. and less than or equal to 38° C.; The third rolling process is to roll the aluminum-titanium coil that has been rolled in the second rolling process and spray the cooling lubricating oil, the thickness of the aluminum-titanium coil after rolling is greater than or equal to 15 μm and less than or equal to 15.4 μm, the rolling force of the third rolling process is greater than or equal to 250 T and less than or equal to 290 T, and the temperature of the cooling lubricating oil in the third rolling process is greater than or equal to 30° C. and less than or equal to 38° C.; Coiling, combining the two aluminum-titanium coils after the third rolling process; In the fourth rolling pass, the aluminum-titanium coil is rolled after being rolled together, and the cooling lubricating oil is sprayed to form an aluminum-titanium foil with a thickness greater than or equal to 5.9 μm and less than or equal to 6.7 μm. The rolling force of the fourth rolling pass is greater than or equal to 235 T and less than or equal to 265 T. The temperature of the cooling lubricating oil in the fourth rolling pass is greater than or equal to 45°C and less than or equal to 52°C.

2. The aluminum-titanium foil rolling method according to claim 1, It is characterized in that The fourth rolling process is performed by a rolling mill, and the surface roughness Ra value of the rollers of the rolling mill is greater than or equal to 0.058 μm and less than or equal to 0.063 μm.

3. The aluminum-titanium foil rolling method according to claim 1, It is characterized in that The coiling requires spraying cooling lubricating oil on the aluminum-titanium coil.

4. The aluminum-titanium foil rolling method according to claim 1, It is characterized in that The speed of the first rolling pass is greater than or equal to 600 m / min and less than or equal to 800 m / min, the speed of the second rolling pass is greater than or equal to 850 m / min and less than or equal to 1050 m / min, the speed of the third rolling pass is greater than or equal to 1050 m / min and less than or equal to 1250 m / min, and the speed of the fourth rolling pass is greater than or equal to 500 m / min and less than or equal to 800 m / min.

5. The aluminum-titanium foil rolling method according to claim 1, It is characterized in that The tension before the first rolling pass is greater than or equal to 2.5 kg / mm 2 And less than or equal to 4kg / mm 2 The second rolling tension is greater than or equal to 3.0 kg / mm 2 And less than or equal to 6.0kg / mm 2 , the tension before the third rolling is greater than or equal to 4.0kg / mm 2 And less than or equal to 7.5kg / mm 2 , the tension before the fourth rolling is greater than or equal to 4.0kg / mm 2 And less than or equal to 6.5kg / mm 2 .

6. The aluminum-titanium foil rolling method according to claim 1, It is characterized in that The aluminum-titanium coil also includes iron, silicon and copper, the weight percentage of the iron is greater than or equal to 0.7% and less than or equal to 1.1%, the weight percentage of the silicon is greater than or equal to 0.2% and less than or equal to 0.3%, and the weight percentage of the copper is greater than or equal to 0.01% and less than or equal to 0.03%.

7. An aluminum titanium foil, It is characterized in that The aluminum-titanium foil is formed by the aluminum-titanium foil rolling method as claimed in any one of claims 1 to 6, wherein the weight proportion of titanium in the aluminum-titanium foil is greater than or equal to 0.05% and less than or equal to 0.10%.