Coated cutting tools
By adopting multi-layered AlCrSi and TiSi nitride or carbonitride coatings in high-hardness steel cutting tools, and adding Nb or Cr to TiSi, the problem of insufficient durability of small-diameter tools is solved, significantly improving resistance Wearability and durability, suitable for cutting and processing of high hardness steel.
Patent Information
- Application Number
- CN202080067356.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-27
- Filing Date
- 2020-10-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-10-21
AI Technical Summary
In cutting processing of high hardness steel, the durability of small diameter tools is insufficient. There is room for improvement in the wear resistance and durability of existing AlCrSi nitride or carbon nitride-covered cutting tools when the tool diameter is less than 1 mm.
A cladding cutting tool adopts a multi-layer structure, in which layer A is composed of nitride or carbon nitride of more than 50% aluminum and 20% chromium, and layer B is composed of 70% titanium and 5% silicon nitrogen. A compound or carbon nitride is composed of, and a trace amount of Nb or Cr is added to the nitride or carbon nitride of TiSi to improve the durability of the tool.
The durability of the cladding cutting tool is significantly improved, especially in small diameter tools, which extends the delivery time of mold making, reduces dimensional changes, and improves machining accuracy and wear resistance.
Smart Images

Figure GDA0004974565230000081 
Figure GDA0004974565230000091
Abstract
Description
Technical Field
[0001] The present invention relates to a covered cutting tool such as an end mill.
[0002] This application claims priority based on Patent Application No. 2019-214083 and Patent Application No. 2019-213826 filed in Japan on November 27, 2019, and the contents of these are incorporated herein by reference. Background Art
[0003] AlCrSi nitride or carbonitride is a film type with excellent heat resistance and wear resistance, and is used for coating cutting tools. The applicant of the present application proposed in patent documents 1 to 3 that the content ratio of Si is increased to make the film structure finer. In the coated cutting tools disclosed in patent documents 1 to 3, the coated cutting tools with TiSi nitride or carbonitride provided on the upper layer have very excellent wear resistance and excellent durability in the cutting of high hardness steel.
[0004] Patent Document 1: International Publication No. 2015 / 141743
[0005] Patent Document 2: International Publication No. 2014 / 156699
[0006] Patent Document 3: Japanese Patent Publication No. 2016-078131
[0007] The present inventors have confirmed that a coated cutting tool having a TiSi nitride or carbonitride disposed on an AlCrSi nitride or carbonitride having a high Si content ratio and a fine film structure tends to show wear resistance equal to or better than that of a cBN tool in cutting high-hardness steel. However, the present inventors have confirmed that there is room for improvement in durability when applied to a small-diameter tool having a tool diameter of less than 1 mm, and further a tool diameter of less than 0.5 mm. Summary of the invention
[0008] One embodiment of the present invention is a coated cutting tool having an A layer and a B layer provided on the A layer on the surface of a substrate, wherein the A layer is composed of a nitride or a carbonitride and has a face-centered cubic lattice structure, and the nitride or the carbonitride has an aluminum (Al) content ratio of 50 atomic % or more, a chromium (Cr) content ratio of 20 atomic % or more, a total aluminum (Al) and chromium (Cr) content ratio of 85 atomic % or more, and a silicon (Si) content ratio of 4 atomic % or more and 15 atomic % or less, based on the total amount of metal (including semi-metal) elements.
[0009] The B layer is composed of nitride or carbonitride and has a face-centered cubic lattice structure, wherein the nitride or carbonitride contains 70 atomic % or more and 90 atomic % or less of titanium (Ti), 5 atomic % or more and 20 atomic % or less of silicon (Si), and 1 atomic % or more and 10 atomic % or less of niobium (Nb) or chromium (Cr), based on the total amount of metal (including semi-metal) elements.
[0010] Preferably, the thickness of the A layer is greater than 1.0 μm, and the thickness of the B layer is greater than 0.5 μm.
[0011] According to one aspect of the present invention, there is provided a coated cutting tool having excellent durability.
[0012] In the above method, the durability of the coated cutting tool can be improved. Therefore, even in the processing of high-hardness pre-hardened steel, for example, the lead time of mold production can be shortened, the mold can be made more precise, and the dimensional change caused by tempering can be reduced, which is extremely effective in the industry. DETAILED DESCRIPTION
[0013] The inventors have found that, for a coated cutting tool based on AlCrSi nitride or carbonitride with a finer film structure, a trace amount of Nb or Cr is added to the TiSi nitride or carbonitride provided on the upper layer, thereby further improving the durability, thereby completing the present invention. The details of the present invention are described below.
[0014] The coated cutting tool according to the embodiment of the present invention comprises: a substrate, a layer A disposed on the surface of the substrate, and a layer B disposed on layer A. In the coated cutting tool of the present embodiment, other films such as an intermediate film disposed between the substrate and the hard film, an intermediate film disposed between the layer A and the layer B, and a protective film disposed on the upper layer of the layer B may be provided as required.
[0015] The A layer is composed of nitride or carbonitride mainly composed of Al and Cr. Nitride or carbonitride mainly composed of Al and Cr is a film with excellent wear resistance and heat resistance. By applying it to the coating of cutting tools, the durability of the tool can be improved. The constituent material of the A layer is more preferably a nitride having better heat resistance than carbonitride.
[0016] Al is an element that imparts heat resistance to the hard film. In order to impart better heat resistance to the hard film, in the A layer, the content ratio (atomic %, the same below) of Al in the metal (including semi-metal, the same below) element is set to 50% or more. Furthermore, preferably, the content ratio of Al in the A layer is set to 55% or more. On the other hand, if the content ratio of Al in the A layer is too large, the close-packed hexagonal structure (hcp structure, the same below) becomes the main body, and the durability of the coated cutting tool tends to decrease. Therefore, preferably, the content ratio of Al in the A layer is set to 70% or less.
[0017] Cr is an element that sets the crystal structure of layer A to a face-centered cubic lattice structure (fcc structure, the same below), thereby improving the wear resistance and heat resistance of the coated cutting tool. If the Cr content of layer A is too low, the wear resistance and heat resistance will decrease, and the hcp structure will become the main body, and the durability of the coated cutting tool will tend to decrease. Therefore, the Cr content of layer A is set to be greater than 20%. Furthermore, preferably, the Cr content of layer A is set to be greater than 30%. On the other hand, if the Cr content of layer A is too large, the heat resistance tends to decrease. Therefore, preferably, the Cr content of layer A is set to be less than 45%.
[0018] In order to achieve both high levels of heat resistance and wear resistance in the A layer, the total content of Al and Cr is set to 85% or more. Furthermore, preferably, the total content of Al and Cr in the A layer is set to 90% or more. The total content of Al and Cr in the A layer is preferably 96% or less, and more preferably 95% or less.
[0019] Si is an important element for refining the structure of nitrides or carbonitrides mainly composed of Al and Cr. The columnar particles of AlCrN without Si and AlCrSiN with a low Si content are coarse. In a hard film with such a structure morphology, the wear of the back face of the coated cutting tool tends to increase because the grain boundaries that serve as the starting point of film destruction increase. On the other hand, the structure of AlCrSiN containing a certain amount of Si becomes finer, for example, it is difficult to observe clear columnar particles in cross-sectional observation using an electron microscope (20,000 times). In a hard film with such a structure morphology, the columnar grain boundaries that serve as the starting point of destruction decrease, which can suppress the wear of the back face of the coated cutting tool. However, if the Si content ratio of the A layer increases, the amorphous and hcp structures tend to become the main body, and the durability of the coated cutting tool decreases. In order not to reduce the durability of the coated cutting tool and to fully refine the film structure, it is important to set the Si content ratio of the A layer to be greater than 4% and less than 15%. The Si content ratio of the A layer is preferably greater than 5%. The Si content of the A layer is preferably 10% or less.
[0020] The A layer may also contain other metal elements besides Al, Cr and Si. For example, the A layer may contain one or more elements selected from the 4a, 5a and 6a groups of the periodic table and B, Cu, Y and Yb. These elements are added to the AlTiN and AlCrN hard films to improve the properties of the hard film. If the content ratio is not too high, the durability of the coated cutting tool will not be significantly reduced.
[0021] However, if the A layer contains a large amount of metal elements other than Al, Cr and Si, the basic properties of the nitride or carbonitride mainly composed of Al and Cr may be impaired, resulting in a decrease in the durability of the coated cutting tool. Therefore, even if the A layer contains metal elements other than Al, Cr and Si, it is preferred that the total content ratio be 10% or less. Furthermore, even if the A layer contains metal elements other than Al, Cr and Si, it is preferred that the total content ratio be 5% or less.
[0022] The coated cutting tool of this embodiment may also be provided with an intermediate film of metal, nitride, carbonitride, carbide, etc. between the substrate and the A layer. By providing the intermediate film, the adhesion between the substrate and the hard film will be further improved. In addition, the surface of the substrate may be subjected to metal bombardment treatment to form a nano-scale modified phase. The intermediate film may be a single layer or a multilayer. The intermediate film may also be provided after the metal bombardment treatment.
[0023] It is important that the A layer in the present embodiment is an fcc structure. In the present embodiment, the fcc structure is such that, in the intensity distribution obtained from the X-ray diffraction pattern or the restricted field diffraction pattern of a transmission electron microscope, the peak intensity caused by the fcc structure shows the maximum intensity. Since the hard film whose diffraction intensity due to the hcp structure shows the maximum intensity is fragile, it lacks durability as a coated cutting tool. In particular, durability tends to decrease in wet processing. Preferably, the A layer does not have a diffraction intensity caused by the hcp structure in the X-ray diffraction pattern. Preferably, the A layer tends to show excellent durability by having a film structure whose peak intensity is the largest even in the fcc structure on the (200) plane or the (111) plane.
[0024] Regarding the A layer, if the content ratio of Si is increased, AlN with an hcp structure may exist in the microstructure. In order to quantify the amount of AlN with an hcp structure existing in the microstructure of the hard film, when observing the processed cross section of the hard film, the intensity distribution obtained from the restricted field diffraction pattern of a transmission electron microscope can be used. Specifically, in the intensity distribution of the restricted field diffraction pattern of the transmission electron microscope, the relationship of Ih×100 / Is is evaluated.
[0025] Ih = Peak intensity due to the (010) plane of hcp AlN
[0026] Is = the sum of the peak intensities due to the fcc structure, the (111) plane of AlN, the (111) plane of CrN, the (200) plane of AlN, the (200) plane of CrN, the (220) plane of AlN, and the (220) plane of CrN, and the peak intensities due to the hcp structure, the (010) plane of AlN, the (011) plane of AlN, and the (110) plane of AlN
[0027] By evaluating the above relationship, in a hard film in which no peak intensity due to AlN having an hcp structure is confirmed by X-ray diffraction, AlN having an hcp structure contained at a microscopic level can be quantitatively evaluated.
[0028] In the A layer, it is preferred to reduce the amount of AIN in the hcp structure in the microstructure to satisfy the relationship of Ih×100 / Is≤25. By satisfying the relationship of Ih×100 / Is≤25, the durability of the coated cutting tool is further improved. Furthermore, preferably, the A layer satisfies the relationship of Ih×100 / Is≤20.
[0029] Next, the B layer will be described.
[0030] Layer B is a hard film disposed on layer A. Layer B is based on nitride or carbonitride of TiSi, a film species with excellent wear resistance and heat resistance. A small amount of Nb or Cr is also added to layer B. In order to further improve the wear resistance of TiSiN, the inventors studied the addition of a third element. And, it was confirmed that the hardness of TiSiN with a suppressed Si content ratio is increased by adding a small amount of Nb or Cr, thereby improving the wear resistance of the coated cutting tool. Although the details of the mechanism of improved wear resistance are unclear, it can be speculated that this is because a part of the Ti in TiN is replaced by Nb or Cr, which causes distortion in the lattice due to the difference in atomic radius between Ti and Nb or Cr, thereby hardening.
[0031] If the Ti content of the B layer is too low or too high, the wear resistance and heat resistance of the hard film will decrease. Therefore, the Ti (titanium) content of the B layer is set to 60% or more and 90% or less based on the total amount of metal (including semi-metal) elements.
[0032] If the Si content of the B layer is too low, the film structure is not sufficiently refined, and the wear resistance of the hard film is reduced. In addition, if the Si content of the B layer is too high, the film structure becomes too fine and close to amorphous, so the wear resistance of the hard film is reduced. Therefore, with respect to the B layer, the Si (silicon) content is set to 5% or more and 20% or less based on the total amount of metal (including semi-metal) elements.
[0033] If the content ratio of Nb or Cr in the B layer is too low, the improvement effect of the wear resistance of the hard film is insufficient. On the other hand, if the content ratio of Nb or Cr in the B layer is too high, a large amount of fragile Nb or Cr concentrated phases will precipitate, and the wear resistance of the hard film will decrease. Therefore, with respect to the B layer, the content ratio of Nb (niobium) or Cr (chromium) is set to be greater than 1% and less than 10% based on the total amount of metal (including semi-metal) elements. Furthermore, the content ratio of Nb or Cr in the B layer is preferably greater than 2%. The content ratio of Nb or Cr in the B layer is preferably less than 8%. The content ratio of Nb or Cr in the B layer is more preferably less than 6%.
[0034] It is important that the B layer in the present embodiment is an fcc structure. In the present embodiment, the fcc structure is such that, in the intensity distribution obtained from the X-ray diffraction pattern or the restricted field diffraction pattern of a transmission electron microscope, the peak intensity caused by the fcc structure shows the maximum intensity. Since the hard film whose diffraction intensity due to the hcp structure shows the maximum intensity is fragile, it lacks durability as a coated cutting tool. In particular, durability tends to decrease in wet processing. Preferably, the B layer does not have a diffraction intensity caused by the hcp structure in the X-ray diffraction pattern. Preferably, the B layer tends to show excellent durability by having a membrane structure whose peak intensity of the (200) plane is the largest even in the fcc structure.
[0035] Regarding layer B, it is preferred that the average crystal grain size of the hard film constituting layer B is greater than 5nm and less than 50nm. If the microstructure of the hard film becomes too fine, the structure of the hard film is close to amorphous, so the toughness and hardness of the hard film decrease. In order to improve the crystallinity of the hard film and reduce the fragile amorphous phase, the average crystal grain size of the hard film is set to more than 5nm. In addition, if the microstructure of the hard film becomes too coarse, the hardness of the hard film decreases, and the durability of the coated cutting tool tends to decrease. In order to impart high hardness to the hard film and improve the durability of the coated cutting tool, the average crystal grain size of the hard film is set to less than 50nm. Furthermore, the average crystal grain size of the hard film is preferably less than 30nm.
[0036] The average crystal grain size of the hard film can be measured from the half value width of X-ray diffraction.
[0037] The B layer may be disposed directly above the A layer. In order to further improve the adhesion, a laminated film containing the composition of the A layer and the B layer may be disposed between the A layer and the B layer. In addition, a hard film other than the composition of the A layer and the B layer may be disposed between the A layer and the B layer. Another hard film may be disposed on the B layer.
[0038] The coated cutting tool according to the embodiment of the present invention is preferably applied to a small-diameter end mill with a tool diameter of 2 mm or less, thereby more effectively exerting the effect of improving durability. Furthermore, it is preferred to apply the structure of the coated cutting tool according to the embodiment of the present invention to a small-diameter end mill with a tool diameter of 1 mm or less.
[0039] In the coated cutting tool according to the embodiment of the present invention, it is preferred that layer A is a film thicker than layer B. By making layer A disposed on the substrate side a film thicker than layer B, the durability of the coated cutting tool is improved. In addition, it is preferred that layer A has a film thickness greater than 1.0 μm and layer B has a film thickness greater than 0.5 μm.
[0040] For any layer of the A layer and the B layer, if the film thickness is too large, peeling is likely to occur, and the durability of the coated cutting tool is reduced. The upper limit of the film thickness of the A layer and the B layer varies depending on the structure of the hard film including the intermediate layer and the surface layer. If an example is given, preferably, the upper limit of the film thickness of the A layer is less than 4 μm, the upper limit of the film thickness of the B layer is less than 3.5 μm, and the upper limit of the combined film thickness of the A layer and the B layer is set to 5 μm or less.
[0041] Example
[0042] (Example 1)
[0043] <Film forming device>
[0044] The hard film is formed using an arc ion plating device. This device consists of multiple cathodes (arc evaporation sources), a vacuum container, and a substrate rotating mechanism.
[0045] This device has three cathodes C1, C2, and C3. C1 is a cathode equipped with a coil magnet on the outer periphery of the target. C2 and C3 are cathodes equipped with permanent magnets on the back and outer periphery of the target. In C2 and C3, the magnetic flux density in the vertical direction of the target is 14mT or more near the center of the target. The composition of the target mounted on C2 and C3 changes depending on the sample.
[0046] The vacuum container is evacuated by a vacuum pump. Film forming gas is introduced into the vacuum container from a supply port. A bias power supply is connected to each substrate placed in the vacuum container. The bias power supply applies a negative DC bias voltage to each substrate.
[0047] The substrate rotation mechanism has a planet carrier, plate-shaped clamps on the planet carrier, and tubular clamps on the plate-shaped clamps. The planet carrier rotates at a speed of three revolutions per minute. The plate-shaped clamps and the tubular clamps rotate around their own axes and revolve respectively.
[0048] <Substrate>
[0049] As substrates for physical evaluation and cutting tests, double-edged ball end mills made of cemented carbide with a composition of WC(bal.)-Co(8 mass%)-Cr(0.5 mass)-VC(0.3 mass%), an average WC grain size of 0.6 μm, and a hardness of 93.9 HRA were prepared. In addition, WC represents tungsten carbide, Co represents cobalt, Cr represents chromium, and VC represents vanadium carbide.
[0050] <Heating and vacuum evacuation process>
[0051] Each substrate was fixed to the tubular clamp in the vacuum chamber, and the following film-forming pretreatment was carried out. First, the inside of the vacuum chamber was evacuated to 8×10 -3 Pa or less. Then, it was heated to a substrate temperature of 500 °C by a heater installed in the vacuum chamber, and vacuum evacuation was carried out. Thus, the substrate temperature was set to 500 °C, and the pressure inside the vacuum chamber was set to 8×10 -3 Pa or less.
[0052] <Ar bombardment process>
[0053] Then, Ar gas was introduced into the vacuum chamber, and the internal pressure of the chamber was set to 0.67 Pa. After that, a current of 35 A was supplied to the filament electrode, and a bias voltage of -200 V was applied to the substrate, and Ar bombardment was carried out for 4 minutes.
[0054] <Ti bombardment process>
[0055] Then, vacuum evacuation was carried out to make the pressure inside the vacuum chamber become 8×10 -3 Pa or less. Next, a bias voltage was applied to the substrate, and an arc current of 150 A was supplied to C1 equipped with a Ti target, thereby performing Ti bombardment treatment. Through the Ti bombardment treatment, carbides containing W and Ti were formed on the surface of the substrate with a thickness of 1 nm or more and 10 nm or less. The composition of the carbides formed by the Ti bombardment treatment is: based on the content ratio of metal elements, W is 60 atomic% or more and 90 atomic% or less, and Ti is 10 atomic% or more and 40 atomic% or less.
[0056] <Film-forming process>
[0057] After Ti bombardment, the power supply to C1 was immediately interrupted. Then, the gas in the vacuum container was replaced with nitrogen, the pressure in the vacuum container was set to 5 Pa, and the substrate setting temperature was set to 520°C. 150A of power was supplied to C2 equipped with the AlCrSi target, the negative pressure bias voltage applied to the substrate was set to 120V, the cathode voltage was set to 30V, and the A layer was coated.
[0058] After coating the A layer, the B layer was coated. In the coating of the B layer, a TiSiNb target, a TiSiW target, a TiSiTa target, or a TiSi target was used as a target of C3 according to the sample. 150A of power was supplied to the C3 equipped with the above targets, the bias voltage of the negative pressure applied to the substrate was set to 50V, the cathode voltage was set to 25V, and the B layer was coated. Then, the substrate was cooled to below about 250°C and taken out of the vacuum container. Then, the blade tip of each sample after coating was polished by sandblasting.
[0059] The composition of the hard film was measured by wavelength dispersive electron probe microanalysis (WDS-EPMA). The measurement conditions were: acceleration voltage 10 kV, sample current 5×10 -8 A. Capture time 10 seconds, analysis area diameter 1μm, analysis depth about 1μm, and 5 points are measured, and the average value is calculated.
[0060] The crystal structure was confirmed using an X-ray diffraction device (EMPYREAN vertical range finder manufactured by Spectris Co., Ltd.) The measurement conditions were: tube voltage 45 kV, tube current 40 mA, X-ray source Cukα (λ=0.15418 nm), X-ray incident angle 3 degrees, divergence slit 1 / 2°, collimator 0.27 mm, 2θ=20 to 70 degrees.
[0061] Cutting was performed using the coated cutting tools of the prepared samples, and the durability of the coated cutting tools was evaluated based on the exposed area of the base material after cutting. The cutting conditions are as follows.
[0062] (condition)
[0063] Tool: Double-edged super-hard ball end mill
[0064] Model: EPDBEH2003-0.5-TH3 spherical radius 0.15mm
[0065] Cutting method: Cavity processing (1mm×3mm×depth 0.4mm)
[0066] Workpiece: ASP23 (64HRC)
[0067] Cutting depth: axial 0.013mm, radial 0.013mm
[0068] Cutting speed: 37.7m / min
[0069] Single-edge feed rate: 0.0045mm / edge
[0070] Cutting oil: spray (oily)
[0071] ·Number of processing: 7 cavities
[0072] Evaluation method: After cutting, the exposed area of the base material was observed using a scanning electron microscope at a magnification of 600 times, and the exposed area of the superhard substrate of the tool was calculated. The exposed area of the base material was calculated using commercially available image analysis software. The evaluation results are summarized in Table 1.
[0073]
Table 1
[0074]
[0075] In any of the examples of the present invention and the comparative examples, both the A layer and the B layer are single phases of fcc structure in XRD diffraction. In addition, regarding the A layer, when the intensity distribution of the restricted field diffraction pattern of the A layer is evaluated by the same method as Japanese Patent No. 6410797, the value of Ih×100 / Is of the A layer is less than 20. In addition, the peak intensity of the fcc (200) plane of the B layer is the largest, and the average crystal grain size is greater than 5 nm and less than 50 nm.
[0076] Inventive Examples 1 to 3, in which a small amount of Nb is added to the upper layer of the A layer, i.e., the B layer, which contains a certain amount of Si and refines the film structure, all have small exposed areas of the base material and exhibit excellent durability. In particular, in the inventive Example 3, in which the total film thickness of the A layer and the B layer is thick, the exposed area of the base material is small and exhibits more excellent durability.
[0077] On the other hand, although a small amount of Nb is added to the B layer of Comparative Example 1, since the Si content is high, the exposed area of the base material is larger than that of the present invention example.
[0078] In Comparative Examples 2 and 3, although Nb was replaced with trace amounts of W (tungsten) and Ta (tantalum), the hardening of the B layer was insufficient, and the exposed area of the base material became larger than that of the present invention example.
[0079] In Comparative Example 4, since a small amount of Nb is not added to the B layer, the exposed area of the base material is larger than that of the present invention example.
[0080] In Comparative Example 5, since the Si content ratio of the A layer is small, the columnar particles of the film structure are large, and even if the B layer is provided similar to that of Inventive Example 1, the base material exposed area becomes large.
[0081] In Comparative Example 6, since the Nb content ratio of the B layer is large, the Nb concentrated phase becomes coarser and the base material exposed area becomes larger.
[0082] (Example 2)
[0083] In Example 2, a hard film consisting of layer A and layer B was formed on a substrate using the same film forming apparatus as in Example 1, thereby producing a coated cutting tool. In Example 2, a TiSiN-based film containing Cr was formed as layer B. The substrate of Example 2 was the same type as that of Example 1.
[0084] In the hard film forming step in Example 2, the heating and vacuum exhausting step, the Ar bombardment step, and the Ti bombardment step are performed similarly to Example 1, and then the film forming step is performed. In the film forming step, as a target for forming the B layer, a TiSiCr target is used instead of the TiSiNb target of Example 1.
[0085] The heating and vacuum exhaust process, the Ar bombardment process, and the Ti bombardment process are the same as those in Example 1, and thus the description thereof is omitted.
[0086] <Film Forming Process>
[0087] After Ti bombardment, the power supply to C1 was immediately interrupted. In addition, the gas in the vacuum container was replaced with nitrogen, the pressure in the vacuum container was set to 5 Pa, and the substrate setting temperature was set to 520° C. 150A of power was supplied to C2 equipped with the AlCrSi target, the negative pressure bias voltage applied to the substrate was set to 120V, the cathode voltage was set to 30V, and the A layer was coated.
[0088] After coating the A layer, the B layer was coated. In coating the B layer, a TiSiCr target, a TiSiW target, a TiSiTa target, or a TiSi target was used as a target of C3 according to the sample. A power of 150A was supplied to the C3 equipped with the above targets, the negative bias voltage applied to the substrate was set to 50V, the cathode voltage was set to 25V, and the B layer was coated. Then, the substrate was cooled to below about 250°C and taken out of the vacuum container. In addition, the blade tip of each sample after coating was polished by sandblasting.
[0089]
Table 2
[0090]
[0091] In Example 2, the A layer and the B layer in any of the present invention examples and comparative examples are single phases of fcc structure in XRD diffraction. In addition, when the intensity distribution of the restricted field diffraction pattern of the A layer is evaluated by the same method as Japanese Patent No. 6410797, the value of Ih×100 / Is of the A layer is 20 or less. In addition, the peak intensity of the fcc (200) plane of the B layer is the largest, and the average crystal grain size is 5 nm or more and 50 nm or less.
[0092] Inventive Examples 21 to 23, in which a trace amount of Cr was added to the upper layer of the A layer, i.e., the B layer, which contained a certain amount of Si and made the film structure finer, all had a small exposed area of the base material and showed excellent durability. In particular, the exposed area of the base material of Inventive Example 23, in which the total film thickness of the A layer and the B layer was thick, was small, and showed more excellent durability.
[0093] On the other hand, although a small amount of Cr is added to the B layer of Comparative Example 21, since the Si content is high, the exposed area of the base material is larger than that of the present invention example.
[0094] In Comparative Examples 22 and 23, Cr was replaced with trace amounts of W (tungsten) and Ta (tantalum) added, but the hardening of the B layer was insufficient, and the exposed area of the base material became larger than that of the present invention example.
[0095] In Comparative Example 24, since a trace amount of Cr is not added to the B layer, the exposed area of the base material is larger than that of the present invention example.
[0096] In Comparative Example 25, since the Si content ratio of the A layer is small, the columnar particles of the film structure are large, and even if the B layer is provided like that of Inventive Example 21, the exposed area of the base material becomes large.
[0097] In Comparative Example 26, since the content ratio of Cr in the B layer is large, the Cr concentrated phase becomes coarser and the base material exposed area becomes larger.
Claims
1. A coated cutting tool, characterized in that: A layer A and a layer B provided directly on the layer A are provided on the surface of the substrate, the layer A is composed of a nitride or a carbonitride and has a face-centered cubic lattice structure, the nitride or the carbonitride contains, based on the total amount of metal elements, an aluminum Al content of 50 atomic % or more and a chromium Cr content of 20 atomic % or more and a chromium Cr content of 85 atomic % or more and a silicon Si content of 4 atomic % or more and a 15 atomic % or less, The B layer is composed of nitride or carbonitride and has a face-centered cubic lattice structure, wherein the nitride or carbonitride contains 70 atomic % or more and 90 atomic % or less of titanium Ti, 5 atomic % or more and 20 atomic % or less of silicon Si, and 1 atomic % or more and 10 atomic % or less of niobium Nb or chromium Cr, based on the total amount of metal elements. The metal element includes a semi-metal element, The average crystal grain size of the hard film constituting the B layer is 5 nm or more and 50 nm or less, The film thickness of the A layer is greater than 1.0 μm and less than 4 μm, and the film thickness of the B layer is greater than 0.5 μm and less than 3.5 μm.