A large-area nanowire array film and preparation method thereof
The template was removed by fluoride plasma etching technology, and the problem of unstable template dissolution and insufficient support during the preparation of nanowire array film in the template method was solved, and the stable preparation and efficient production of large-area nanowire array films were achieved.
Patent Information
- Application Number
- CN202210187658.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-11-19
- Filing Date
- 2022-02-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the preparation of nanowire arrays by template method, the template dissolution is unstable, and the template and support cannot be completely removed and it is difficult to support the nanowire array, resulting in high preparation difficulty and insufficient safety.
Aluminum trioxide, titanium dioxide or zirconium dioxide nanotube films are etched using fluoride plasma, exposing the deposited carbon, metal, alloy, and oxide fillers to form a large-area nanowire array film and pass through fluoride gas plasma. The body is cleaned and removed, and the by-products are easy to separate, reducing the difficulty of preparation.
The stable preparation of nanowire array membrane is achieved, the preparation process is simplified, the preparation difficulty is reduced, and the control of preparation parameters is improved.
Smart Images

Figure CN114538413B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of nanowires, and in particular relates to a large-area nanowire array film and a preparation method thereof. Background Art
[0002] Nanowire arrays are an ordered whole composed of a large number of independent nanowires perpendicular to the substrate, which not only retains the structure and function of a single nanowire, but also has a large-scale synergistic effect. Nanowire arrays have high surface activity due to their large specific surface area and stable crystal orientation, which improves the utilization rate of active materials. In addition, the nanowire array structure can also reduce the stress caused by volume change in the electrochemical process, so it has broad application prospects in the fields of physics and chemistry.
[0003] Among the many methods for preparing nanowire arrays, the template method has the advantages of high controllability, simple preparation process, and large-scale production, and has broad application prospects. However, since the template prepared by the template method is usually an oxide film, its oxide film must be dissolved to obtain the nanowire array, and solutions such as phosphoric acid and sodium hydroxide are usually selected. However, the process of dissolving the template is unstable, for example, it is impossible to determine the effective dissolution temperature and dissolution time, it is impossible to completely remove the template, and the dissolved nanowires cannot maintain the array structure, etc.
[0004] At present, the process of preparing nanowire arrays by template method is as follows. First, a nanotube array film is prepared, and then the nanotube array film containing a substrate is placed in a solution, and metals, alloys, oxides, etc. are filled by hydrothermal method and sol-gel method, and then a layer of support is deposited on one side of the film, and finally the template is dissolved by phosphoric acid, sodium hydroxide and other solutions to obtain a nanowire array. However, this method has many problems, such as the support cannot support the nanowires to obtain an array, the dissolution of the template is difficult to control, and the operation is not safe enough.
[0005] In recent years, plasma cleaning technology has gradually matured. Plasma, like solid, liquid or gas, is a state of matter, also called the fourth state of matter. Common atmospheres used in plasma cleaning technology include fluoride gases such as carbon tetrafluoride, nitrogen trifluoride, and sulfur hexafluoride. Fluoride gas is ignited in a vacuum chamber by a radio frequency power supply under a certain voltage to produce high-energy disordered plasma, which can bombard oxide films such as aluminum trioxide and titanium dioxide through plasma to produce aluminum trifluoride, titanium tetrafluoride, etc. Among them, aluminum trifluoride is easy to sublimate when exposed to strong heat, and titanium tetrafluoride itself has a low boiling point of 284°C. Both are easy to sublimate in a high-energy environment, thereby achieving the requirement of removing oxide films. Summary of the invention
[0006] To address the deficiencies of the prior art, the present invention provides a large-area nanowire array film and a method for preparing the same. Based on the template method, the present invention etches an oxide nanotube film such as aluminum oxide, titanium dioxide or zirconium dioxide by fluoride plasma to expose the deposited carbon, metal, alloy, oxide and other fillers therein, thereby obtaining a large-area nanowire array film, and the etching byproduct fluoride sublimates and leaves the system. The method is easy to control the progress of plasma etching, the byproducts are easy to separate, and the difficulty of preparation is reduced.
[0007] The technical solution provided by the present invention is as follows:
[0008] A method for preparing a large-area nanowire array film, the method comprising the following steps:
[0009] Step 1: Anodizing the pretreated pure aluminum sheet, titanium sheet or zirconium sheet, which includes the following steps:
[0010] 1) Pretreatment of pure aluminum, titanium or zirconium sheets:
[0011] The oxide layer on the surface of the pure titanium sheet to be processed is removed by mechanical processing, wherein the pure aluminum sheet, titanium sheet or zirconium sheet is a flat sheet with a thickness of 0.1 to 1 mm;
[0012] 2) Preparation of electrolyte:
[0013] 0.2-0.5M oxalic acid aqueous solution, 0.25-1wt.% NH4F ethylene glycol solution and 0.5-2wt.% NH4F glycerol-glycerol solution are respectively prepared as electrolytes for anodic oxidation of pure aluminum sheets, titanium sheets or zirconium sheets;
[0014] 3) Placing the pretreated pure aluminum sheet, titanium sheet, or zirconium sheet in the electrolyte for anodization reaction to obtain a primary preliminary product of aluminum oxide, titanium dioxide, or zirconium dioxide nanotube array membrane:
[0015] The pretreated pure aluminum sheet, titanium sheet or zirconium sheet is used as the anode, and the stainless steel foil electrode, copper foil, titanium foil, platinum foil or graphite electrode is used as the cathode, and the pretreated pure aluminum sheet, titanium sheet and zirconium sheet are anodic oxidized by using a DC power supply with a voltage of 10-50V, 20-110V and 20-80V, respectively, at an oxidation temperature of 0-30°C and an oxidation time of 1-168h;
[0016] Step 2: immediately taking out the primary preliminary product from the electrolyte and washing it with deionized water, and then putting it into a methanol solution of liquid bromine, wherein the volume ratio of liquid bromine to methanol is 1:1-1:9, and reacting it at room temperature for 12-96 hours to dissolve and remove the aluminum, titanium, and zirconium metal matrices to obtain an aluminum oxide, titanium dioxide, or zirconium dioxide nanotube array film;
[0017] Step 3: After the obtained secondary preliminary product is cleaned with anhydrous ethanol, it is placed in a critical CO2 atmosphere drying oven for drying to obtain a tertiary preliminary product with a barrier layer at the bottom;
[0018] Step 4: using physical or chemical methods to deposit carbon, metal, alloy or oxide fillers into the aluminum oxide, titanium dioxide or zirconium dioxide nanotube array film to obtain a fourth-level preliminary product of a nanotube array film having deposited fillers in the tube;
[0019] Step 5: Place the four-stage preliminary product bottom-side up into a plasma cleaning instrument containing fluoride gas for template etching at a power of 1-50 kW and a placement time of 2h-24h. After the reaction, the large-area nanowire array film is obtained.
[0020] In the above technical solution, after depositing carbon, metal, alloy, oxide and other fillers on the aluminum oxide, titanium dioxide or zirconium dioxide nanotube array film, fluoride gas is used to plasma etch the template. The etching process is easy to control, and the by-products are easy to separate, which reduces the difficulty of preparation.
[0021] Specifically, the purity of the pure aluminum sheet, titanium sheet or zirconium sheet is greater than 99.9%, and the shape is rectangular or circular.
[0022] Specifically, the metal element in the carbon, metal, alloy or oxide is one or more of magnesium, indium, tin, lead, arsenic, antimony or bismuth.
[0023] Specifically, the physical or chemical method in step 4) is one of atomic layer vapor deposition, magnetron sputtering, sol-gel method, electrodeposition method, and physical hydraulic method. After deposition, the excess sediment can be removed by physical methods, such as physical stripping, ultrasonic cleaning, adhesive removal, etc., or a combination of these methods.
[0024] Specifically, the fluoride gas in step 4) is a mixed gas of any one or more of carbon tetrafluoride, nitrogen trifluoride, and sulfur hexafluoride.
[0025] Specifically, the area of the finished product described in step 5) is 1-100cm 2 .
[0026] The present invention also provides a large-area nanowire array film prepared by the above preparation method.
[0027] The finished product can be used as a sensing, photoelectric conversion or conductive material.
[0028] The present invention realizes the etching of aluminum oxide, titanium dioxide or zirconium dioxide templates by a simple method of plasma cleaning of fluoride gas. In the plasma etching of fluoride gas, due to the presence of fluoride ions, fluoride ions will react with Al3+ 、Ti 4+ 、Zr 4+ The easily vaporized AlF3, TiF4, ZrF4 and other substances are generated, and then the barrier layer at the bottom of the aluminum oxide, titanium dioxide or zirconium dioxide array film is removed to form a nanowire array film structure. The method has a simple preparation process, easy control of preparation parameters, and good etching effect on the template, thereby reducing the difficulty of obtaining a large-area nanowire array film. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 In obtained in Example 1 of the present invention 0.9 Sn 0.1 Scanning electron microscopy image of the nanowire array film.
[0030] Figure 2 This is a scanning electron microscope image of the C nanowire array film obtained in Example 2 of the present invention.
[0031] Figure 3 This is a scanning electron microscope image of the PbO2 nanowire array film obtained in Example 3 of the present invention. DETAILED DESCRIPTION
[0032] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0033] Example 1
[0034] A 5cm long square aluminum sheet (purity greater than or equal to 99.9%, thickness 0.2mm) was processed by conventional mechanical processing to remove the oxide layer on the surface. The electrolyte was prepared by oxalic acid and water, and the content of oxalic acid was 0.3M. The treated aluminum sheet was placed in a reaction device, and the diameter of the aluminum sheet exposed to the electrolyte was 4cm. The electrolyte temperature was fixed at 5°C using a refrigerator, and platinum foil was used as the cathode. Anodization was performed for 2 hours under an anode voltage of 40V to obtain a nanotube array membrane with an average pore size of 60nm. After the reaction was completed, the sample was immediately taken out of the electrolyte and washed with deionized water, and then placed in a methanol solution of liquid bromine, with a volume ratio of liquid bromine to methanol of 1:5. The reaction was carried out at room temperature for 12 hours to remove the aluminum substrate. After taking out the sample from the methanol solution of liquid bromine, it was cleaned with anhydrous ethanol and placed in a critical CO2 atmosphere drying oven for drying to obtain an aluminum oxide nanotube array membrane with a barrier layer at the bottom.
[0035] In prepared by physical hydraulic method 0.9 Sn 0.1 The specific steps are as follows: the aluminum oxide nanotube array film prepared previously is placed face up in a vacuum hydraulic device, and then the melted In 0.9 Sn 0.1Press it into a sheet and place it on top of the array membrane. Turn on the vacuum pump and raise the device temperature to 170°C, slightly higher than the melting point of the alloy. Keep it for 10 minutes, and the alloy will melt and spread on the surface of the array membrane. Then apply a liquid pressure to inject the alloy into the nanotube array membrane. After it cools to room temperature, peel off the remaining In 0.9 Sn 0.1 The slices were then ultrasonically cleaned for 16 h.
[0036] The bottom of the membrane was placed upward in a sulfur hexafluoride plasma cleaning instrument for template etching at a power of 40 kW for 24 hours. 0.9 Sn 0.1 Nanowire array membrane, structure such as Figure 1 shown.
[0037] Example 2
[0038] A circular titanium sheet with a diameter of 2 cm (purity greater than or equal to 99.9%, thickness of 0.2 mm) was processed by conventional machining to remove the oxide layer on the surface. The electrolyte was prepared by NH4F and ethylene glycol, and the content of NH4F was 0.5wt.%. The treated titanium sheet was placed in a reaction device, and the diameter of the titanium sheet exposed to the electrolyte was 1 cm. The electrolyte temperature was fixed at 5°C using a refrigerator, and a graphite electrode was used as the cathode. Anodization was performed for 12 hours under an anode voltage of 60V to obtain a nanotube array membrane with an average pore size of 80nm. After the reaction was completed, the sample was immediately taken out of the electrolyte and washed with deionized water, and then placed in a methanol solution of liquid bromine, with a volume ratio of liquid bromine to methanol of 1:5. The reaction was carried out at room temperature for 24 hours to remove the titanium substrate. After taking out the sample from the methanol solution of liquid bromine, it was cleaned with anhydrous ethanol and placed in a critical CO2 atmosphere drying oven for drying to obtain a titanium dioxide nanotube array membrane with a barrier layer at the bottom.
[0039] The C nanowires were prepared by chemical vapor deposition. The specific steps are as follows: the titanium dioxide nanotube array film was placed in a tube furnace, and under air conditions, the temperature was raised from room temperature to a set temperature of 450°C at 2°C / min, then kept warm for 3 hours, and then dropped to room temperature at 2°C / min. The crystallized titanium dioxide nanotube sample and a certain amount of urea and polyvinyl alcohol were placed in a graphite tank, vacuumed, and in a nitrogen atmosphere, the temperature was raised from room temperature to a set temperature of 600°C at 1°C / min, then kept warm for 3 hours, and then dropped to room temperature at 1°C / min to obtain a titanium dioxide nanotube array film filled with carbon nanowires. Then ultrasonic cleaning was performed for 24 hours.
[0040] The bottom of the membrane was placed upward in a sulfur hexafluoride plasma cleaning instrument for template etching at a power of 50 kW for 16 hours. After the reaction, a C nanowire array membrane was obtained with the structure shown in FIG. Figure 2 shown.
[0041] Example 3
[0042] A 4cm long square zirconium sheet (purity greater than or equal to 99.9%, thickness 0.3mm) was processed by conventional machining to remove the oxide layer on the surface. The electrolyte was prepared by NH4F, glycerol, and glycerol, glycerol and glycerol were mixed in a ratio of 1:1, and the content of NH4F was 1wt.%. The treated zirconium sheet was placed in a reaction device, and the diameter of the titanium sheet exposed to the electrolyte was 3cm. At room temperature, a graphite electrode was used as a cathode, and anodization was performed for 3 hours under an anode voltage of 50V to obtain a nanotube array membrane with an average pore size of 100nm. After the reaction was completed, the sample was immediately taken out of the electrolyte and washed with deionized water, and then placed in a methanol solution of liquid bromine, with a volume ratio of liquid bromine to methanol of 1:6, and reacted at room temperature for 36h to remove the zirconium substrate. After taking out the sample from the methanol solution of liquid bromine, it was cleaned with anhydrous ethanol and placed in a critical CO2 atmosphere drying oven for drying to obtain a zirconium dioxide nanotube array membrane with a barrier layer at the bottom.
[0043] The PbO2 nanowires were deposited by sol-gel method. The specific steps were as follows: 0.005 mol of lead nitrate was taken and dissolved in 10 ml of deionized water by magnetic stirring to form solution A; 0.005 mol of citric acid was weighed and dissolved in 10 ml of deionized water by magnetic stirring to form solution B; solution B was slowly added to solution A to form a mixed solution. The solution was magnetically stirred for 1 hour at 60°C, and the pH was adjusted to between 5 and 6 with ammonia water; the water in the solution was heated to evaporate, and when the solution became a hydrosol, the washed and dried zirconium dioxide nanotube array membrane was immersed in it and kept warm in a 60°C water bath for 2 hours. The zirconium dioxide nanotube array membrane was taken out, the sol on the surface was wiped off, and after drying at 80°C for 1 hour, it was placed in a muffle furnace and heated to 800°C for annealing for 2 hours. The zirconium dioxide nanotube array membrane with PbO2 nanowires was obtained. Then it was ultrasonically cleaned for 24 hours.
[0044] The bottom of the membrane was placed upward in a carbon tetrafluoride plasma cleaning instrument for template etching at a power of 45 kW for 18 hours. After the reaction, a PbO2 nanowire array membrane was obtained with the following structure: Figure 3 shown.
[0045] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An In 0.9 Sn 0.1 A method for preparing a nanowire array film, It is characterized in that The method comprises the following steps: removing the oxide layer on the surface of a square aluminum sheet with a length of 5 cm by mechanical processing; preparing an electrolyte with oxalic acid and water, and the content of oxalic acid is 0.3 M; placing the treated aluminum sheet in a reaction device, and the diameter of the aluminum sheet exposed to the electrolyte is 4 cm; fixing the temperature of the electrolyte at 5°C by using a refrigerator, using a platinum foil as a cathode, and performing anodization for 2 hours under the condition of an anode voltage of 40 V to obtain a nanotube array membrane with an average pore size of 60 nm; immediately taking out a sample from the electrolyte after the reaction is completed, washing it with deionized water, and then putting it into a methanol solution of liquid bromine, wherein the volume ratio of liquid bromine to methanol is 1:5, reacting at room temperature for 12 hours, and removing the aluminum substrate; taking out the sample from the methanol solution of liquid bromine, washing it with anhydrous ethanol, and placing it into a critical CO 2 The aluminum oxide nanotube array film with a barrier layer at the bottom was obtained by drying in an atmosphere drying oven; In 0.9 Sn 0.1 The specific steps are as follows: the aluminum oxide nanotube array film prepared previously is placed face up in a vacuum hydraulic device, and then the melted In 0.9 Sn 0.1 Press into a sheet and place it on top of the array membrane; turn on the vacuum pump, raise the device temperature to 170°C, keep it for 10 minutes, the alloy melts and spreads on the surface of the array membrane, then apply a liquid pressure to inject the alloy into the nanotube array membrane; after cooling to room temperature, peel off the remaining In 0.9 Sn 0.1 The film was then ultrasonically cleaned for 16 hours; the bottom of the film was placed upward in a sulfur hexafluoride plasma cleaning instrument for template etching, with a power of 40kW and a placement time of 24 hours. After the reaction, In 0.9 Sn 0.1 Nanowire array membrane.
2. A method for preparing a C nanowire array film, It is characterized in that The method comprises the following steps: removing the oxide layer on the surface of a circular titanium sheet with a diameter of 2 cm by mechanical processing; the electrolyte is NH 4 F, prepared with ethylene glycol, NH 4 The content of F is 0.5wt.%; the treated titanium sheet is placed in the reaction device, and the diameter of the titanium sheet exposed to the electrolyte is 1cm; the electrolyte temperature is fixed at 5°C in a refrigerator, and a graphite electrode is used as a cathode. Anodization is performed for 12 hours at an anode voltage of 60V to obtain a nanotube array membrane with an average pore size of 80nm; after the reaction is completed, the sample is immediately taken out from the electrolyte and washed with deionized water, and then placed in a methanol solution of liquid bromine, with a volume ratio of liquid bromine to methanol of 1:5, and reacted at room temperature for 24h to remove the titanium substrate; after taking out the sample from the methanol solution of liquid bromine, it is cleaned with anhydrous ethanol and placed in a critical CO 2 The titanium dioxide nanotube array film was dried in an atmosphere drying oven to obtain a titanium dioxide nanotube array film with a barrier layer on the bottom; the C nanowires were prepared by chemical vapor deposition, and the specific steps were as follows: the titanium dioxide nanotube array film was placed in a tube furnace, and under air conditions, the temperature was raised from room temperature to a set temperature of 450°C at a rate of 2°C / min, then kept warm for 3 hours, and then dropped to room temperature at a rate of 2°C / min; the crystallized titanium dioxide nanotube sample, urea and polyvinyl alcohol were placed in a graphite tank, evacuated, and in a nitrogen atmosphere, the temperature was raised from room temperature to a set temperature of 600°C at a rate of 1°C / min, then kept warm for 3 hours, and then dropped to room temperature at a rate of 1°C / min to obtain a titanium dioxide nanotube array film filled with carbon nanowires; then ultrasonic cleaning was performed for 24 hours; the bottom of the membrane was placed upward in a sulfur hexafluoride plasma cleaner for template etching, with a power of 50kW and a placement time of 16 hours. After the reaction, a C nanowire array film was obtained.
3. A PbO 2 A method for preparing a nanowire array film, It is characterized in that The method comprises the following steps: removing the oxide layer on the surface of a 4 cm square zirconium sheet by mechanical processing; the electrolyte is NH 4 F, glycerol, glycerol, glycerol and glycerol are mixed in a ratio of 1:1, NH 4 The content of F is 1wt.%; the treated zirconium sheet is placed in the reaction device, and the diameter of the titanium sheet exposed to the electrolyte is 3cm; at room temperature, a graphite electrode is used as a cathode, and anodization is performed for 3 hours at an anode voltage of 50V to obtain a nanotube array membrane with an average pore size of 100nm; after the reaction is completed, the sample is immediately taken out from the electrolyte and washed with deionized water, and then placed in a methanol solution of liquid bromine, the volume ratio of liquid bromine to methanol is 1:6, and the reaction is carried out at room temperature for 36h to remove the zirconium substrate; after taking out the sample from the methanol solution of liquid bromine, it is cleaned with anhydrous ethanol and placed in a critical CO 2 Drying in an atmosphere drying oven to obtain a zirconium dioxide nanotube array film with a barrier layer at the bottom; PbO 2 Nanowires, the specific steps are as follows: take 0.005 mol lead nitrate, dissolve it in 10 ml deionized water by magnetic stirring to form solution A; weigh 0.005 mol citric acid, dissolve it in 10 ml deionized water by magnetic stirring to form solution B; slowly add solution B to solution A to form a mixed solution; the solution is magnetically stirred for 1 hour at 60°C, and the pH is adjusted to between 5 and 6 with ammonia water; continue to heat and evaporate the water in the solution, and when the solution becomes a hydrosol, immerse the washed and dried zirconium dioxide nanotube array membrane in it, and keep it warm in a water bath at 60°C for 2 hours; take out the zirconium dioxide nanotube array membrane, wipe off the sol on the surface, dry it at 80°C for 1 hour, put it in a muffle furnace and heat it to 800°C for annealing for 2 hours; obtain PbO 2 The zirconium dioxide nanotube array film was deposited with nanowires; then ultrasonic cleaning was performed for 24 hours; the bottom of the film was placed upward in a carbon tetrafluoride plasma cleaning instrument for template etching, with a power of 45kW and a placement time of 18 hours. After the reaction, PbO 2 Nanowire array membrane.
Citation Information
Patent Citations
Preparation method of bi-pass large-area TiO* nanotube array film
CN101550581A
Method for preparing Pd doped TiO2 nanotube array composite material
CN101591001A
Cylindrical and barrel-shaped titanium dioxide nanotube arrays and preparation method and application thereof
CN101768771A
Preparation method of nanowire array
CN105668540A
Preparation method of cobaltosic oxide nanowire array negative electrode material
CN112331845A