Single-sided black silicon texturing method and single-sided black silicon produced thereby

By forming catalytic metal ion colloids on one side of the silicon wafer and performing metal catalytic chemical corrosion, the problems of uneven deposition and back-surface corrosion in the preparation of black silicon in the prior art are solved, and efficient single-sided black silicon velvet making is achieved. Improves the light absorption and open circuit voltage of solar cells.

CN114551615BActive Publication Date: 2024-11-15CSI CELLS CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202011332677.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-24
Publication Date
2024-11-15
Estimated Expiration
2040-11-24

AI Technical Summary

Technical Problem

In the preparation of black silicon, uneven deposition of metal catalysts leads to uneven distribution of corrosion pits, affecting the appearance and efficiency of solar cells. The double-sided fleece making method consumes a large amount of chemicals and is difficult to completely remove the back corrosion pits, affecting the battery efficiency. .

Method used

Using the single-sided black silicon velvet-making method, a colloid containing catalytic metal ions, complexing agents and reducing agents is formed on the surface of one side of the silicon wafer, and the metal catalytic chemical corrosion is carried out to form a uniform corrosion pit structure and pass through the wire mesh. Printing controls the colloid distribution to ensure that catalytic metal particles are deposited on only one side surface and avoid back-surround corrosion.

Benefits of technology

The uniform distribution of catalytic metal particles and the uniformity of corrosion pits are achieved, the back side winding corrosion problem is avoided, the fleece quality and the light absorption efficiency of solar cells are improved, and the chemical usage and waste liquid treatment cost are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114551615B_ABST
    Figure CN114551615B_ABST
Patent Text Reader

Abstract

The present invention discloses a single-sided black silicon texturing method and the single-sided black silicon produced thereby. Based on the single-sided black silicon texturing method provided by the present invention, a colloid with metal catalytic ions is only coated on one side surface of a silicon wafer, so that catalytic metal particles are also only deposited on the corresponding surface of the silicon wafer, and the produced single-sided black silicon will not have the problem of back-side corrosion; and in the specific implementation process of the method, the catalytic metal particles deposited on the surface of the silicon wafer are irrelevant to the flatness of the surface of the silicon wafer itself, and the uniform distribution of the metal catalytic particles on the surface of the silicon wafer can be achieved by only ensuring the uniform distribution of the metal catalytic ions in the colloid, thereby making it easier to make the corrosion pits on the obtained texturing surface uniformly distributed, and having a higher texturing quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of solar photovoltaics, and in particular to a single-sided black silicon texturing method and the single-sided black silicon produced by the same. Background Art

[0002] Black silicon is a new type of optoelectronic material obtained by surface modification of silicon material. Due to its good light trapping effect, black silicon can greatly improve the conversion efficiency of corresponding solar cells when it is specifically used in solar cells, so it is widely favored by battery manufacturers.

[0003] In recent years, the use of metal catalyzed chemical etching (MCCE) to prepare black silicon is a common method. A specific process for preparing black silicon in the prior art is: placing a silicon wafer in an etching solution containing a metal catalyst, allowing the metal catalyst to be deposited on the surface of the silicon wafer, and then placing the silicon wafer with the metal catalyst deposited on the surface in an acid etching solution, and the silicon wafer will be corroded at the metal catalyst deposition position to form corrosion pits, thereby obtaining black silicon. However, in this method, since the surface of the silicon wafer is not absolutely flat, there are certain differences in the deposition rate of the metal catalyst in different areas, so that the metal catalyst deposited on the surface of the silicon wafer is not uniform, and the distribution of the corrosion pits on the surface of the obtained silicon wafer is also uneven, so that the black silicon surface looks dark in part and light in part, which affects the appearance of the black silicon.

[0004] In addition, the black silicon preparation method described in the prior art is usually suitable for double-sided texturing, that is, both sides of the silicon wafer need to form a velvet surface with corrosion pits. However, in actual application, the velvet structure on the back of the silicon wafer has no effect on the solar cell, but will affect the passivation effect on the back. In addition, the consumption of chemicals required for the wet double-sided texturing of black silicon is large, and the cost of waste liquid treatment is high. Although the prior art also has a single-sided wet texturing of black silicon, there is still a back-side corrosion phenomenon in the specific implementation process, that is, the acid corrosion liquid will go around to the back of the silicon wafer and cause corrosion to the local area on the back of the silicon wafer, thus making the back structure of the silicon wafer uneven; even if the back polishing process is added after the single-sided texturing, there will still be the problem of unclean removal of the back corrosion pit structure, which will not only affect the appearance of the back of the silicon wafer, but also be unfavorable for the back passivation, affect the opening voltage, and ultimately affect the battery efficiency.

[0005] In view of this, it is necessary to provide an improved technical solution to solve the above problems. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the prior art. To achieve the above-mentioned purpose of the invention, the present invention provides a single-sided black silicon texturing method, and its specific design is as follows.

[0007] A single-sided black silicon texturing method comprises the following steps:

[0008] Obtain silicon wafers;

[0009] Forming a layer of colloid containing catalytic metal ions, complexing agent and reducing agent on the surface of one side of the silicon wafer to be textured;

[0010] Heating the silicon wafer printed with the colloid so that the catalytic metal ions are reduced by the reducing agent to form catalytic metal particles attached to the surface of the silicon wafer;

[0011] The silicon wafer is placed in an acid etching solution for metal catalytic chemical etching, so that the surface of the silicon wafer to which the catalytic metal particles are attached forms a textured surface composed of etching pits.

[0012] Furthermore, the colloid is formed on the surface of the silicon wafer by screen printing.

[0013] Furthermore, the single-sided black silicon is used for a solar cell, and the solar cell has a metal electrode arranged on one side of the single-sided black silicon textured surface, and the colloid formed on the surface of the silicon wafer is hollowed out at the corresponding position where the metal electrode is arranged.

[0014] Further, the catalytic metal ion is Au + 、Ag + , Cu 2+ , Pt 2+ , Fe 3+ 、Ni 2+ or Pd 2+ At least one of .

[0015] Furthermore, the complexing agent contains an amine group.

[0016] Furthermore, the colloid is heated to a temperature of 80-200°C.

[0017] Furthermore, the reducing agent contains a carboxyl group.

[0018] Furthermore, the acid etching solution includes HF with a mass percentage concentration of 5%-20% and an oxidant with a mass percentage concentration of 1%-10%, and the oxidant includes at least one of H2O2, HNO3 and ozone water.

[0019] Furthermore, the texturing method also includes the step of using a solution containing H2O2 and HCl to clean the silicon wafer having the texturing surface.

[0020] The present invention also provides a single-sided black silicon, which is made by the single-sided black silicon texturing method described above.

[0021] The beneficial effects of the present invention are as follows: based on the single-sided black silicon texturing method provided by the present invention, the colloid with metal catalytic ions is only coated on one side of the silicon wafer, so that the catalytic metal particles are also only deposited on the corresponding surface of the silicon wafer, and the single-sided black silicon obtained will not have the problem of back-side corrosion; and in the specific implementation process of the method, the catalytic metal particles deposited on the surface of the silicon wafer have nothing to do with the flatness of the surface of the silicon wafer itself, and it is only necessary to ensure that the metal catalytic ions in the colloid are evenly distributed to achieve the uniform distribution of the metal catalytic particles on the surface of the silicon wafer, thereby making it easier to make the corrosion pits on the obtained texturing surface evenly distributed, with higher texturing quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0023] Figure 1 Shown is a schematic flow chart of the single-sided black silicon texturing method of the present invention. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] like Figure 1 As shown, the single-sided black silicon texturing method involved in the present invention comprises the following steps:

[0026] Obtain silicon wafers;

[0027] A colloid layer containing catalytic metal ions, complexing agent and reducing agent is formed on the surface of one side of the silicon wafer to be textured;

[0028] The silicon wafer printed with the colloid is heated so that the catalytic metal ions are reduced by the reducing agent to form catalytic metal particles attached to the surface of the silicon wafer;

[0029] The silicon wafer is placed in an acid etching solution for metal catalytic chemical etching, so that the surface of the silicon wafer with catalytic metal particles attached forms a textured surface composed of corrosion pits.

[0030] The present invention also provides a single-sided black silicon, which is made by the above single-sided black silicon texturing method.

[0031] Based on the single-sided black silicon texturing method provided by the present invention, since the colloid with metal catalytic ions only covers one side of the silicon wafer, when the silicon wafer printed with the colloid is heated, the catalytic metal particles obtained by the reduction reaction are also only deposited on the corresponding side of the silicon wafer. In this way, during the metal catalytic chemical corrosion process, the acid corrosion liquid will only corrode the side of the surface where the catalytic metal particles are attached, and there will be no problem of back-side corrosion.

[0032] In addition, in the specific implementation process of the single-sided black silicon texturing method of the present invention, the catalytic metal particles deposited on the surface of the silicon wafer have nothing to do with the flatness of the surface of the silicon wafer itself. It is only necessary to ensure that the metal catalytic ions in the colloid are evenly distributed to achieve the uniform distribution of the metal catalytic particles on the surface of the silicon wafer. Then, during the metal catalytic chemical corrosion, the corrosion pits on the obtained texturing surface are evenly distributed, and the texturing quality is relatively high.

[0033] As a specific embodiment of the present invention, the colloid is formed on the surface of the silicon wafer by screen printing. Specifically, the colloid containing the catalytic metal ions, the complexing agent and the reducing agent is placed on the screen printing plate, and the colloid is printed on one side of the silicon wafer by scraping the colloid with a scraper. In the specific implementation process, the thickness of the colloid printed on the surface of the silicon wafer can be adjusted by controlling the opening rate of the screen printing plate, the scraper pressure, the distance between the screen printing plate and the silicon wafer and other parameters, which will not be further expanded here.

[0034] The single-sided black silicon involved in the present invention is used for solar cells. The solar cell has a metal electrode arranged on one side of the single-sided black silicon textured surface. As a preferred embodiment of the present invention, the colloid formed on the surface of the silicon wafer is hollowed out at the corresponding position where the metal electrode is arranged. Based on this arrangement, no catalytic metal particles will be formed on the surface of the silicon wafer at the corresponding position where the metal electrode is arranged, and further, during metal catalytic chemical corrosion, the textured surface of the silicon wafer will not be corroded by the acid etching solution at the corresponding position where the metal electrode is arranged.

[0035] For solar cells made of single-sided black silicon of the present invention, the area on the surface of the texturized side of the silicon wafer where the metal electrode is not provided is used to receive sunlight; accordingly, due to the obstruction of the metal electrode, the area on the surface of the texturized side of the silicon wafer corresponding to the metal electrode cannot absorb sunlight. In this way, based on the above setting method of the present invention, texturizing in the area that can receive sunlight can ensure that the silicon wafer has a better light absorption effect and improve the short-circuit current; and the area of ​​the silicon wafer corresponding to the metal electrode has a smaller surface area (no corrosion pits), which can minimize surface recombination and is beneficial to improving the open circuit voltage of the solar cell.

[0036] In the specific implementation process of the present invention, the catalytic metal ion involved is Au + 、Ag + , Cu 2+ , Pt2+ , Fe 3+ 、Ni 2+ or Pd 2+ At least one of .

[0037] Furthermore, in some specific embodiments of the present invention, the complexing agent involved contains an amine group, such as ammonia. The amine group protects the corresponding catalytic metal ions from reacting with the reducing agent at room temperature through complexation with the catalytic metal ions.

[0038] Furthermore, in the embodiment where the complexing agent contains an amine group, the temperature of the heated colloid is 80-200° C. At this temperature, the complexing agent decomposes due to heat and cannot prevent the catalytic metal ions from reacting with the reducing agent. At this time, the catalytic metal ions react with the reducing agent to form catalytic metal particles attached to the surface of the silicon wafer.

[0039] In some specific embodiments, the reducing agent contains a carboxyl group, such as formic acid.

[0040] In some specific embodiments, the acid etching solution involved in the present invention includes HF with a mass percentage concentration of 5%-20% and an oxidant with a mass percentage concentration of 1%-10%, and the oxidant includes at least one of H2O2, HNO3 and ozone water. In a specific embodiment, the acid etching solution is prepared by hydrofluoric acid stock solution, hydrogen peroxide stock solution, and deionized water in a volume ratio of 1-6:1-4:8-16, wherein the mass percentage concentration of HF in the hydrofluoric acid stock solution is 40%, and the mass percentage concentration of HNO3 in the hydrogen peroxide stock solution is 60%.

[0041] Furthermore, the texturing method of the present invention also includes the step of using a solution containing H2O2 and HCl to clean the silicon wafer with the texturing surface. In a specific embodiment, the cleaning solution is prepared by hydrogen peroxide stock solution, hydrochloric acid stock solution, and deionized water in a volume ratio of 1:1:4-6, wherein the mass percentage concentration of H2O2 in the hydrogen peroxide stock solution is 30%, and the mass percentage concentration of HCl in the hydrochloric acid stock solution is 36%.

[0042] In the specific implementation process, the silicon wafers cleaned with the above cleaning solution need to be cleaned with deionized water and dried before entering the next step of solar cell manufacturing.

[0043] It should be understood that although this specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

[0044] The series of detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present invention. They are not intended to limit the scope of protection of the present invention. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A single-sided black silicon texturing method, It is characterized in that The following steps are involved: Obtain silicon wafers; A layer of colloid containing catalytic metal ions, a complexing agent and a reducing agent is formed by printing on the surface of one side of the silicon wafer to be textured, wherein the complexing agent protects the catalytic metal ions from reacting with the reducing agent at room temperature; The silicon wafer printed with the colloid is heated, and the complexing agent is decomposed at high temperature so that the catalytic metal ions are reduced by the reducing agent to form catalytic metal particles attached to the surface of the silicon wafer; The silicon wafer is placed in an acid etching solution for metal catalytic chemical etching, so that the surface of the silicon wafer to which the catalytic metal particles are attached forms a textured surface composed of corrosion pits; the single-sided black silicon is used for solar cells, and the solar cell has a metal electrode arranged on one side of the single-sided black silicon textured surface, and the colloid formed on the surface of the silicon wafer is hollowed out at the corresponding position where the metal electrode is set.

2. The single-sided black silicon texturing method according to claim 1, It is characterized in that The catalytic metal ion is Au + 、Ag + , Cu 2+ , Pt 2+ , Fe 3+ 、Ni 2+ or Pd 2+ At least one of .

3. The single-sided black silicon texturing method according to claim 1, It is characterized in that The complexing agent contains an amine group.

4. The single-sided black silicon texturing method according to claim 3, It is characterized in that The temperature of heating the colloid is 80-200°C.

5. The single-sided black silicon texturing method according to claim 1, It is characterized in that The reducing agent contains a carboxyl group.

6. The single-sided black silicon texturing method according to claim 1, It is characterized in that The acid etching solution includes HF with a mass percentage concentration of 5%-20% and an oxidant with a mass percentage concentration of 1%-10%, wherein the oxidant includes H 2 O 2 , HNO 3 and at least one of ozone water.

7. The single-sided black silicon texturing method according to claim 1, It is characterized in that The texturing method further comprises using a 2 O 2 , a step of cleaning the silicon wafer with a textured surface using a solution of HCl.

8. A single-sided black silicon, It is characterized in that It is made by the single-sided black silicon texturing method described in any one of claims 1-7.

Citation Information

Patent Citations

  • Polishing and texturing process for polycrystalline black silicon PERC battery

    CN108447942A

  • Pure black assembly single crystal PERC battery and preparation process thereof

    CN110581183A

  • Polycrystalline wet black silicon texturing process with high stability

    CN110911527A

  • Silicon silicon chip is deceived to single face wet process

    CN207781620U