A high-low temperature resistant and oil-resistant sealing rubber material and preparation method thereof

By using temperature-controlled sustained release modified inorganic filler in sealing rubber materials to load anti-aging agents and coat epoxy resin, the performance problems of nitrile rubber at low and high temperatures are solved, and the range of -42 to 140℃ is achieved The durable sealing effect improves the high temperature resistance and stability of the sealing material.

CN114561049BActive Publication Date: 2024-11-29NINGBO FENGMAO FAR EAST RUBBER
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210112421.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-29
Publication Date
2024-11-29
Estimated Expiration
2042-01-29

AI Technical Summary

Technical Problem

Nitrile rubber has increased hardness and reduced elasticity at low temperatures, and thermal oxygen aging occurs at high temperatures, making it difficult to meet the sealing requirements in extremely cold and high temperature environments at the same time, limiting its use temperature range.

Method used

Using a high and low temperature-resistant oil-resistant sealing rubber material formula, including nitrile rubber, silicone rubber, vulcanizing agent, anti-aging agent, plasticizer, inorganic filler and auxiliary agent, the anti-aging agent is loaded through temperature-controlled sustained release modified inorganic filler. The diatomaceous earth is coated with epoxy resin, and the high-temperature expansion and low-temperature shrinkage characteristics of the epoxy resin layer can be used to achieve the temperature controlled release of the anti-aging agent, avoiding the premature release of the anti-aging agent at low temperatures and effectively playing a role at high temperatures.

Benefits of technology

The long-term use of sealing materials is achieved in an environment of -42~140℃, which significantly improves the high-temperature resistance of sealing rubber materials, avoids the "frost spray" phenomenon of anti-aging agents at low temperatures, and ensures the stability of sealing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GHA0000005763880000061
    Figure GHA0000005763880000061
  • Figure GHA0000005763880000071
    Figure GHA0000005763880000071
  • Figure GHA0000005763880000072
    Figure GHA0000005763880000072
Patent Text Reader

Abstract

The present invention relates to the technical field of sealing rubber materials, and discloses a high-low temperature resistant and oil-resistant sealing rubber material and a preparation method thereof. The sealing rubber material comprises the following raw materials in parts by weight: 100 parts of nitrile rubber, 18 to 30 parts of silicone rubber, 5 to 8 parts of vulcanizing agent, 4 to 8 parts of antioxidant, 4 to 8 parts of plasticizer, 50 to 100 parts of inorganic filler, 8 to 16 parts of auxiliary agent, and 0 to 10 parts of colorant. By adopting the formula of the present invention, the sealing rubber material can have good high temperature resistance and good oil medium resistance, can meet the sealing requirements in extremely cold and high temperature environments, and can be used for a long time in an environment of -42 to 140°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sealing rubber materials, and in particular to a high-low temperature resistant and oil-resistant sealing rubber material and a preparation method thereof. Background Art

[0002] Nitrile rubber (NBR) is a random copolymer made from butene and acrylonitrile monomers by free radical initiated emulsion polymerization. As a general-purpose rubber, it has good physical and mechanical properties, and the side groups of the molecular chain are highly polar, which makes nitrile rubber have excellent tolerance to fuel oil, mineral oil and aromatic solvents. Therefore, nitrile rubber is widely used as the main material for oil-resistant sealing formulas in pipelines of media such as petroleum hydraulic oil, glycol hydraulic oil, diester lubricating oil, gasoline, water, silicone grease, silicone oil, and industrial mechanical seals. Nitrile rubber oil-resistant seals have developed into the most widely used and lowest-cost rubber sealing products.

[0003] With the advancement of technology and the expansion of customer activity areas, sealing products are required to have a wider range of uses. For example, the increase in operating temperature, the temperature difference between the north and south regions, and the influence of the contact medium have put forward higher requirements than before for products such as gaskets, sealing rings, and sealing layers in addition to being resistant to engine oil, in terms of high and low temperature resistance. However, nitrile rubber will increase in hardness and decrease in elasticity at low temperatures, and will undergo thermal oxidation aging at high temperatures, which limits the use temperature range of nitrile rubber sealing materials. Traditional NBR rubber has an operating temperature range of -40 to 100°C or -30 to 120°C, which makes it difficult to meet the sealing requirements in extremely cold and high temperature environments at the same time. Therefore, it is of great significance to broaden the use temperature range of NBR sealing materials so that they have both good oil medium resistance and high and low temperature resistance. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a high-low temperature resistant and oil-resistant sealing rubber material and a preparation method thereof. The sealing rubber material has both good oil medium resistance and high-low temperature resistance, and can meet the sealing requirements in extremely cold and high temperature environments.

[0005] The specific technical scheme of the present invention is:

[0006] A high-low temperature resistant and oil-resistant sealing rubber material comprises the following raw materials in parts by weight:

[0007] 100 parts of nitrile rubber;

[0008] Silicone rubber 15-30 parts;

[0009] 5-8 parts of vulcanizing agent;

[0010] 3-8 parts of antioxidant;

[0011] 4 to 8 parts of plasticizer;

[0012] 50-105 parts of inorganic filler;

[0013] 8-16 parts of additives;

[0014] Colorant 0-10 parts.

[0015] By adopting the formula of the present invention, the sealing rubber material can have better high temperature resistance and better oil medium resistance, can meet the sealing requirements in extremely cold and high temperature environments, and can be used for a long time in an environment of -42 to 140°C.

[0016] Preferably, the silicone rubber is a mixture of methyl vinyl silicone rubber and precipitated silica.

[0017] Preferably, the vulcanizing agent includes dicumyl peroxide and / or 1,3-bis(tert-butylperoxyisopropyl)benzene; the sealing rubber material also includes the following raw materials in parts by weight: 1 to 3 parts of triallyl isocyanurate.

[0018] When peroxide is used as a vulcanizing agent, the -CC- cross-linking bond energy formed is larger, thereby being able to give the sealing rubber material better heat resistance.

[0019] Preferably, the auxiliary agent includes the following components in parts by weight: 2 to 5 parts of a first auxiliary agent, 1 to 3 parts of a second auxiliary agent, and 5 to 8 parts of a third auxiliary agent; the first auxiliary agent includes ferric oxide or cerium oxide; the second auxiliary agent includes microcrystalline wax 40 / 60; and the third auxiliary agent includes QST-100 silicon-based coupling agent.

[0020] Preferably, the antioxidant includes one or more of 2,6-di-tert-butyl-p-cresol, 4,4'-methylenebis(phenyl isocyanate), 2-mercaptobenzimidazole, 2,2,4-trimethyl-1,2-dihydroquinoline polymer and 4,4'-di(phenylisopropyl)diphenylamine.

[0021] Preferably, the plasticizer includes plasticizer TP759 and / or plasticizer RS735.

[0022] Preferably, the colorant includes carbon black, which may be furnace carbon black, such as carbon black N550, carbon black N774, carbon black N330, and the like.

[0023] Preferably, the inorganic filler comprises the following components in parts by weight: 0 to 45 parts of non-modified inorganic filler and 60 to 70 parts of temperature-controlled sustained-release modified inorganic filler; the temperature-controlled sustained-release modified inorganic filler is diatomaceous earth coated with an epoxy resin layer and loaded with an antioxidant; the curing agent used in the epoxy resin layer includes a curing agent containing a DA bond.

[0024] Antioxidants can reduce the damage of heat and oxygen to rubber molecular chains, thereby improving the high temperature resistance of rubber products. However, the amount of antioxidants added is limited. When the amount of antioxidants added is too large, due to the small molecular weight of the antioxidants, they can move between the cross-linked networks of rubber macromolecules and accumulate on the rubber surface to produce the "frost spray" phenomenon. The antioxidants that migrate to the rubber surface are not only difficult to effectively play an anti-aging role, but also contaminate the substances in contact with them.

[0025] To this end, the present invention adopts a temperature-controlled slow-release modified inorganic filler, loads an antioxidant in diatomaceous earth, and coats the diatomaceous earth with an epoxy resin layer. Under the action of the epoxy resin layer and diatomaceous earth, the release of the antioxidant can be slowed down, and the temperature-controlled release of the antioxidant can be achieved by utilizing the characteristics of the epoxy resin layer that it expands at high temperature and shrinks at low temperature, as well as the characteristics that the DA bond breaks at high temperature and reforms at low temperature. Specifically: when used at a relatively low temperature, the rubber does not age and the antioxidant is not required to function. At this time, the thermal expansion coefficient of the epoxy resin layer is low, and the DA bond does not break. The epoxy resin cross-linking network is dense and has a low porosity, so the release rate of the antioxidant is very slow, which can prevent frost spraying. When used at high temperatures, the antioxidant is required to slow down the aging of the rubber. At this time, the epoxy resin layer undergoes a large degree of thermal expansion, and the porosity is greatly increased. At the same time, the DA bond breaks under the action of high temperature (122°C and above), which can further increase the porosity of the epoxy resin layer, thereby accelerating the release rate of the antioxidant, enabling it to better play an anti-aging role and improve the high temperature resistance of the sealing rubber material. Through the above method, it is possible to avoid the "frost spray" phenomenon that affects the effect of the antioxidant, while increasing the release amount of the antioxidant at high temperature, thereby improving the high temperature resistance of the sealing rubber material.

[0026] In addition, under the action of high temperature during vulcanization, although the release of antioxidants will be accelerated, due to the slow-release effect of the epoxy resin coating and the diatomaceous earth porous material, only part of the antioxidants are released during vulcanization; and, after the vulcanization is completed, the temperature drops, the epoxy resin layer shrinks, and the DA bonds are reformed.

[0027] Preferably, the preparation method of the temperature-controlled sustained-release modified inorganic filler is as follows:

[0028] (1.1) Under the protection of inert gas, N,N'-(4,4'-methylenediphenyl)bismaleimide and furfurylamine in a mass ratio of 1.2 to 1.6:1 are used as raw materials to carry out a Diels-Alder reaction, separate the product, and obtain a curing agent containing a DA bond;

[0029] (1.2) adding diatomaceous earth to an aminosilane coupling agent solution to carry out a dehydration condensation reaction, separating the product, and obtaining aminodiatomaceous earth;

[0030] (1.3) Dissolve epoxy resin, curing agent containing DA bond and triethylenetetramine in acetone in a mass ratio of 1:0.65~0.85:0.09~0.12, add aminodiatomite thereto, carry out coating reaction, separate the product, and obtain aminodiatomite@epoxy resin; (1.4) Heat and melt 2,6-di-tert-butyl-p-cresol, add aminodiatomite@epoxy resin thereto, disperse evenly, evacuate, heat to 122~130℃, stir for 25~35min, and then fill with nitrogen to a pressure of 0.13~0.20MPa. After stirring for 1.5~2.5h, separate the product and cool it to obtain a temperature-controlled sustained-release modified inorganic filler.

[0031] In the above preparation process, the epoxy resin is first coated on the surface of the diatomite, and then the antioxidant 2,6-di-tert-butyl-p-cresol is loaded. The reason is that when coating the epoxy resin, acetone is used as the reaction medium to dissolve the curing agent containing the DA bond, and 2,6-di-tert-butyl-p-cresol is soluble in acetone. If 2,6-di-tert-butyl-p-cresol is loaded first and then coated with the epoxy resin, part of the 2,6-di-tert-butyl-p-cresol loaded in the diatomite will be dissolved during the epoxy resin coating process, resulting in the weakening of the anti-aging effect of the temperature-controlled sustained-release modified inorganic filler, thereby affecting the high temperature resistance of the rubber sealing material.

[0032] Furthermore, the specific process of step (1.1) is as follows: under the protection of inert gas, N,N'-(4,4'-methylenediphenyl)bismaleimide and furfurylamine in a mass ratio of 1.2 to 1.6:1 are dissolved in tetrahydrofuran, and after reflux reaction at 65 to 75°C for 15 to 20 hours, the product is separated to obtain a curing agent containing a DA bond.

[0033] Furthermore, in step (1.1), the mass volume ratio of furfurylamine to tetrahydrofuran is 1 g:8-15 mL.

[0034] Furthermore, in step (1.2), the concentration of the aminosilane coupling agent in the aminosilane coupling agent solution is 10-15wt%; and the mass volume ratio of the diatomaceous earth to the aminosilane coupling agent solution is 1g:6-10mL.

[0035] Furthermore, in step (1.2), the temperature of the dehydration condensation reaction is 40 to 50° C., and the time is 1 to 1.5 hours.

[0036] Preferably, the non-modified inorganic filler includes one or more of neutral white carbon black, alkaline white carbon black, neutral diatomaceous earth and alkaline diatomaceous earth.

[0037] A method for preparing the sealing rubber material comprises the following steps:

[0038] (1) adding all raw materials except silicone rubber into an internal mixer for mixing and rubber removal to obtain an NBR rubber mixture;

[0039] (2) adding the mixed rubber into an open mixer for mixing, and sheeting to obtain an NBR rubber material;

[0040] (3) Add the silicone rubber into an open mill for primary mixing, then add the NBR rubber material for secondary mixing, and sheet off to obtain a sealing rubber material.

[0041] Preferably, in step (1), the binder is discharged after the temperature reaches 115-125°C.

[0042] Preferably, in steps (2) and (3), the roller spacing of the mixing mill is 0.5 to 1 mm.

[0043] Preferably, in step (3), the temperature of the first mixing is 40-60°C, and the time is 3-5 min; the temperature of the second mixing is 40-60°C, and the time is 10-15 min.

[0044] Compared with the prior art, the present invention has the following advantages:

[0045] (1) The sealing rubber material of the present invention has both good oil medium resistance and high and low temperature resistance, can meet the sealing requirements in extremely cold and high temperature environments, and can be used for a long time in an environment of -42 to 140°C;

[0046] (2) By adding temperature-controlled slow-release modified inorganic fillers to the sealing rubber material, the characteristics of the epoxy resin layer expanding at high temperature and shrinking at low temperature, as well as the characteristics of the DA bond breaking at high temperature and reforming at low temperature, can be used to achieve temperature-controlled release of the antioxidant, thereby avoiding the "frost spray" phenomenon that affects the effect of the antioxidant and increasing the release amount of the antioxidant at high temperature, thereby improving the high temperature resistance of the sealing rubber material. DETAILED DESCRIPTION

[0047] The present invention will be further described below in conjunction with the embodiments.

[0048] Overall embodiment

[0049] A high-low temperature resistant and oil-resistant sealing rubber material comprises the following raw materials in parts by weight: 100 parts of nitrile rubber, 15-30 parts of silicone rubber, 5-8 parts of vulcanizer, 1-3 parts of cross-linking agent, 3-8 parts of antioxidant, 4-8 parts of plasticizer, 50-105 parts of inorganic filler, 8-16 parts of auxiliary agent and 0-10 parts of colorant.

[0050] The silicone rubber is a mixed rubber of methyl vinyl silicone rubber and precipitated silica.

[0051] The vulcanizing agent includes dicumyl peroxide (DCP) and / or 1,3-bis(tert-butylperoxyisopropyl)benzene (BIPB).

[0052] The cross-linking agent includes triallyl isocyanurate (TAIC).

[0053] The antioxidant includes one or more of 2,6-di-tert-butyl-p-cresol (BHT), 4,4'-methylenebis(phenyl isocyanate) (MBI), 2-mercaptobenzimidazole, 2,2,4-trimethyl-1,2-dihydroquinoline polymer (RD) and 4,4'-di(phenylisopropyl)diphenylamine (KY-405).

[0054] The plasticizer includes plasticizer TP759 and / or plasticizer RS735.

[0055] The auxiliary agent includes the following components in parts by weight: 2 to 5 parts of a first auxiliary agent, 1 to 3 parts of a second auxiliary agent, and 5 to 8 parts of a third auxiliary agent; the first auxiliary agent includes ferric oxide or cerium oxide; the second auxiliary agent includes microcrystalline wax 40 / 60; and the third auxiliary agent includes QST-100 silicon-based coupling agent.

[0056] The colorant includes carbon black.

[0057] As an embodiment, the inorganic filler includes one or more of neutral white carbon black, basic white carbon black, neutral diatomaceous earth and basic diatomaceous earth.

[0058] As an embodiment, the inorganic filler includes the following components in parts by weight: 0 to 45 parts of a non-modified inorganic filler and 60 to 70 parts of a temperature-controlled sustained-release modified inorganic filler; the non-modified inorganic filler includes one or more of neutral white carbon black, alkaline white carbon black, neutral diatomaceous earth and alkaline diatomaceous earth; the preparation method of the temperature-controlled sustained-release modified inorganic filler is as follows:

[0059] (1.1) Under the protection of inert gas, N,N'-(4,4'-methylenediphenyl)bismaleimide and furfurylamine in a mass ratio of 1.2 to 1.6:1 are dissolved in tetrahydrofuran, wherein the mass volume ratio of furfurylamine to tetrahydrofuran is 1 g:8 to 15 mL, and after reflux reaction at 65 to 75° C. for 15 to 20 hours, the product is separated to obtain a curing agent containing a DA bond;

[0060] (1.2) adding diatomaceous earth to a 10-15 wt % aminosilane coupling agent solution, wherein the mass volume ratio of the diatomaceous earth to the aminosilane coupling agent solution is 1 g:6-10 mL, carrying out a dehydration condensation reaction at 40-50° C. for 1-1.5 h, separating the product, and obtaining aminodiatomaceous earth;

[0061] (1.3) dissolving an epoxy resin, a curing agent containing a DA bond and triethylenetetramine in a mass ratio of 1:0.65-0.85:0.09-0.12 in acetone, adding aminodiatomaceous earth thereto, wherein the mass volume ratio of the epoxy resin, aminodiatomaceous earth and acetone is 1 g:6-8 g:25-35 mL, carrying out a coating reaction at 45-55° C. for 1.5-2 h, separating the product, and obtaining aminodiatomaceous earth@epoxy resin;

[0062] (1.4) After heating and melting 2,6-di-tert-butyl-p-cresol, aminodiatomaceous earth@epoxy resin is added thereto, and after being evenly dispersed, the mixture is evacuated, heated to 122-130°C, stirred for 25-35 minutes, and then filled with nitrogen until the pressure is 0.13-0.20 MPa. After stirring for 1.5-2.5 hours, the product is separated and cooled to obtain a temperature-controlled sustained-release modified inorganic filler.

[0063] A method for preparing the above-mentioned sealing rubber material comprises the following steps:

[0064] (1) adding all raw materials except silicone rubber into an internal mixer for mixing, and discharging the rubber after the temperature reaches 115-125° C. to obtain an NBR mixed rubber;

[0065] (2) adding the mixed rubber to an open mill with a roller gap of 0.5 to 1 mm for mixing, thinning through 3 to 4 times, widening the roller gap and sheeting to obtain an NBR rubber compound;

[0066] (3) Add silicone rubber to an open mill with a roller gap of 0.5 to 1 mm, mix it once at 40 to 60° C. for 3 to 5 minutes, then add NBR rubber, mix it twice at 40 to 60° C. for 10 to 15 minutes, pass it through the mill 5 to 8 times, and sheet it to obtain a sealing rubber material.

[0067] Example 1

[0068] Using the raw materials in Table 1, a high-low temperature resistant and oil-resistant sealing rubber material is prepared by the following steps:

[0069] (1) adding all raw materials except silicone rubber into an internal mixer for mixing, and discharging the rubber after the temperature reaches 120° C. to obtain an NBR mixed rubber;

[0070] (2) adding the mixed rubber to an open mill with a roller gap of 0.5 mm for mixing, thinning through 3 times, widening the roller gap and sheeting to obtain an NBR rubber compound;

[0071] (3) Add silicone rubber to an open mill with a roller gap of 0.5 mm, mix once at 50° C. for 5 min, then add NBR rubber, mix twice at 50° C. for 10 min, pass through thinly 5 times, and sheet to obtain a sealing rubber material.

[0072] Table 1

[0073]

[0074] 1 Silicone rubber: a mixture of methyl vinyl silicone rubber and precipitated silica, purchased from Bluestar Silicones;

[0075] 2 Microcrystalline wax: purchased from Kassel International CO.STD;

[0076] 3 QST-100 silicon-based coupling agent: also known as ST-100, purchased from Zhuzi Chemical.

[0077] Example 2

[0078] Using the raw materials in Table 2, a high-low temperature resistant and oil-resistant sealing rubber material is prepared by the following steps:

[0079] (1) adding all raw materials except silicone rubber into an internal mixer for mixing, and discharging the rubber after the temperature reaches 120° C. to obtain an NBR mixed rubber;

[0080] (2) adding the mixed rubber to an open mill with a roller gap of 1 mm for mixing, thinning through 3 times, widening the roller gap and sheeting to obtain an NBR rubber compound;

[0081] (3) Add silicone rubber to an open mill with a roller gap of 1 mm, mix once at 40° C. for 3 min, then add NBR rubber, mix twice at 40° C. for 15 min, pass through 8 times, and sheet to obtain a sealing rubber material.

[0082] Table 2

[0083]

[0084] 1 Silicone rubber: a mixture of methyl vinyl silicone rubber and precipitated silica, purchased from Bluestar Silicones;

[0085] 2 Microcrystalline wax: Kassel International CO.STD;

[0086] 3 QST-100 silicon-based coupling agent: also known as ST-100, purchased from Zhuzi Chemical.

[0087] Example 3

[0088] Using the raw materials in Table 3, a high-low temperature resistant and oil-resistant sealing rubber material is prepared by the following steps:

[0089] (1) adding all raw materials except silicone rubber into an internal mixer for mixing, and discharging the rubber after the temperature reaches 120° C. to obtain an NBR mixed rubber;

[0090] (2) adding the mixed rubber to an open mill with a roller gap of 0.5 mm for mixing, thinning through 4 times, widening the roller gap and sheeting to obtain an NBR rubber compound;

[0091] (3) Add silicone rubber to an open mill with a roller gap of 0.5 mm, mix once at 40° C. for 5 min, then add NBR rubber, mix twice at 40° C. for 15 min, pass through 8 times, and sheet to obtain a sealing rubber material.

[0092] Table 3

[0093]

[0094]

[0095] 1 Silicone rubber: a mixture of methyl vinyl silicone rubber and precipitated silica, purchased from Bluestar Silicones;

[0096] 2 Microcrystalline wax: purchased from Kassel International CO.STD;

[0097] 3 QST-100 silicon-based coupling agent: also known as ST-100, purchased from Zhuzi Chemical.

[0098] Example 4

[0099] Using the raw materials in Table 4, a high-low temperature resistant and oil-resistant sealing rubber material is prepared by the following steps:

[0100] (1) Preparation of temperature-controlled sustained-release modified inorganic filler:

[0101] (1.1) In a nitrogen atmosphere, N,N'-(4,4'-methylenediphenyl)bismaleimide and furfurylamine were dissolved in tetrahydrofuran in a mass volume ratio of 1.4 g:1 g:10 mL, and refluxed at 70°C for 18 h. After removing tetrahydrofuran by rotary evaporation, the mixture was washed with ethanol and ether in sequence and dried to obtain a curing agent containing a DA bond;

[0102] (1.2) dissolving silane coupling agent KH-550 in water to prepare a 10 wt% coupling agent solution; adding neutral diatomaceous earth to the coupling agent solution at a mass volume ratio of 1 g:10 mL, reacting at 45° C. for 1.5 h, centrifuging, washing the precipitate with water, and drying to obtain amino diatomaceous earth;

[0103] (1.3) Dissolve epoxy resin, curing agent containing DA bond and triethylenetetramine in acetone in a mass volume ratio of 1g:0.75g:0.1g:30mL, add aminodiatomite in an amount 7 times the mass of epoxy resin, reflux at 50°C for 1.5h, centrifuge, wash the precipitate with acetone and water in turn, and dry to obtain aminodiatomite@epoxy resin; (1.4) Heat 2,6-di-tert-butyl-p-cresol to 80±3°C and melt it, add aminodiatomite@epoxy resin, disperse it evenly, evacuate to 0.02MPa, heat it to 125°C, stir it for 30min, and then fill it with nitrogen to a pressure of 0.15MPa. After stirring for 2h, cool it to 80±5°C, filter it and drain it, and cool it to room temperature to obtain a temperature-controlled sustained-release modified inorganic filler;

[0104] (2) adding all raw materials except silicone rubber into an internal mixer for mixing, and discharging the rubber after the temperature reaches 120° C. to obtain an NBR mixed rubber;

[0105] (3) adding the mixed rubber to an open mill with a roller gap of 0.5 mm for mixing, thinning through 4 times, widening the roller gap and sheeting to obtain an NBR rubber compound;

[0106] (4) Add silicone rubber to an open mill with a roller gap of 0.5 mm, mix once at 40° C. for 5 min, then add NBR rubber and mix twice at 40° C. for 15 min, pass through 8 times, and sheet to obtain a sealing rubber material.

[0107] Table 4

[0108]

[0109]

[0110] Silicone rubber: a mixture of methyl vinyl silicone rubber and precipitated silica, purchased from Bluestar Silicones;

[0111] 2 Microcrystalline wax: purchased from Kassel International CO.STD;

[0112] 3 QST-100 silicon-based coupling agent: also known as ST-100, purchased from Zhuzi Chemical.

[0113] Example 5

[0114] Using the raw materials in Table 5, a high-low temperature resistant and oil-resistant sealing rubber material is prepared by the following steps:

[0115] (1) Preparation of temperature-controlled sustained-release modified inorganic filler:

[0116] (1.1) In a nitrogen atmosphere, N,N'-(4,4'-methylenediphenyl)bismaleimide and furfurylamine were dissolved in tetrahydrofuran in a mass volume ratio of 1.2 g:1 g:8 mL, and refluxed at 65°C for 20 h. After removing tetrahydrofuran by rotary evaporation, the mixture was washed with ethanol and ether in sequence and dried to obtain a curing agent containing a DA bond;

[0117] (1.2) dissolving silane coupling agent KH-550 in water to prepare a 15 wt% coupling agent solution; adding diatomaceous earth to the coupling agent solution at a mass volume ratio of 1 g:8 mL, reacting at 50° C. for 1 h, centrifuging, washing the precipitate with water, and drying to obtain aminodiatomaceous earth;

[0118] (1.3) dissolving epoxy resin, curing agent containing DA bond and triethylenetetramine in acetone in a mass volume ratio of 1 g:0.85 g:0.09 g:25 mL, adding aminodiatomaceous earth in an amount 8 times the mass of epoxy resin, and reacting at 55° C. for 2 h. After centrifugation, washing the precipitate with acetone and water in turn, and drying to obtain aminodiatomaceous earth@epoxy resin;

[0119] (1.4) After heating 2,6-di-tert-butyl-p-cresol to 80±3°C and melting it, aminodiatomaceous earth@epoxy resin was added thereto, and after being evenly dispersed, the mixture was evacuated to 0.03 MPa, heated to 130°C, stirred for 35 min, and then filled with nitrogen until the pressure was 0.20 MPa. After stirring for 1.5 h, the mixture was cooled to 80±5°C, filtered and drained, and cooled to room temperature to obtain a temperature-controlled sustained-release modified inorganic filler;

[0120] (2) adding all raw materials except silicone rubber into an internal mixer for mixing, and discharging the rubber after the temperature reaches 120° C. to obtain an NBR mixed rubber;

[0121] (3) adding the mixed rubber to an open mill with a roller gap of 0.5 mm for mixing, thinning through 4 times, widening the roller gap and sheeting to obtain an NBR rubber compound;

[0122] (4) Add silicone rubber to an open mill with a roller gap of 0.5 mm, mix once at 40° C. for 5 min, then add NBR rubber and mix twice at 40° C. for 15 min, pass through 8 times, and sheet to obtain a sealing rubber material.

[0123] Table 5

[0124]

[0125] 1 Silicone rubber: a mixture of methyl vinyl silicone rubber and precipitated silica, purchased from Bluestar Silicones;

[0126] 2Microcrystalline wax: purchased from Kassel International CO.STD;

[0127] 3 QST-100 silicon-based coupling agent: also known as ST-100, purchased from Zhuzi Chemical;

[0128] Example 6

[0129] Using the raw materials in Table 6, a high-low temperature resistant and oil-resistant sealing rubber material is prepared by the following steps:

[0130] (1) Preparation of temperature-controlled sustained-release modified inorganic filler:

[0131] (1.1) In a nitrogen atmosphere, N,N'-(4,4'-methylenediphenyl)bismaleimide and furfurylamine were dissolved in tetrahydrofuran in a mass volume ratio of 1.6 g:1 g:15 mL, refluxed at 75°C for 15 h, and then the tetrahydrofuran was removed by rotary evaporation, and then washed with ethanol and ether in sequence, and dried to obtain a curing agent containing a DA bond;

[0132] (1.2) dissolving silane coupling agent KH-550 in water to prepare a 13 wt% coupling agent solution; adding diatomaceous earth to the coupling agent solution at a mass volume ratio of 1 g:6 mL, reacting at 40° C. for 1.5 h, centrifuging, washing the precipitate with water, and drying to obtain aminodiatomaceous earth;

[0133] (1.3) Dissolve epoxy resin, curing agent containing DA bond and triethylenetetramine in acetone in a mass volume ratio of 1g:0.65g:0.12g:35mL, add aminodiatomite in an amount 6 times that of epoxy resin, and reflux at 45°C for 1.5h. After centrifugation, wash the precipitate with acetone and water in turn, and dry it to obtain aminodiatomite@epoxy resin; (1.4) Heat 2,6-di-tert-butyl-p-cresol to 80±3°C and melt it, add aminodiatomite@epoxy resin, disperse it evenly, evacuate it to 0.01MPa, heat it to 122°C, stir it for 25min, and then fill it with nitrogen to a pressure of 0.13MPa. After stirring for 2.5h, cool it to 80±5°C, filter it and drain it, and cool it to room temperature to obtain a temperature-controlled sustained-release modified inorganic filler;

[0134] (2) adding all raw materials except silicone rubber into an internal mixer for mixing, and discharging the rubber after the temperature reaches 120° C. to obtain an NBR mixed rubber;

[0135] (3) adding the mixed rubber to an open mill with a roller gap of 0.5 mm for mixing, thinning through 4 times, widening the roller gap and sheeting to obtain an NBR rubber compound;

[0136] (4) Add silicone rubber to an open mill with a roller gap of 0.5 mm, mix once at 40° C. for 5 min, then add NBR rubber and mix twice at 40° C. for 15 min, pass through 8 times, and sheet to obtain a sealing rubber material.

[0137] Table 6

[0138]

[0139] 1 Silicone rubber: a mixture of methyl vinyl silicone rubber and precipitated silica, purchased from Bluestar Silicones;

[0140] 2 Microcrystalline wax: purchased from Kassel International CO.STD;

[0141] 3 QST-100 silicon-based coupling agent: also known as ST-100, purchased from Zhuzi Chemical.

[0142] Comparative Example 1

[0143] This comparative example uses a conventional sealing rubber material formula, and the raw materials are shown in Table 7. The sealing rubber material is prepared by the following steps:

[0144] (1) adding all raw materials into an internal mixer for mixing, and discharging the rubber after the temperature reaches 120° C. to obtain an NBR compound rubber;

[0145] (2) The mixed rubber is added to an open mill with a roller gap of 0.5 mm for mixing, thinned through three times, and the roller gap is adjusted to widen the sheet to obtain a sealing rubber material.

[0146] Table 7

[0147]

[0148]

[0149] Comparative Example 2

[0150] The difference between this comparative example and Example 4 is that: 65 parts of the temperature-controlled sustained-release modified inorganic filler in Example 4 are replaced with 55 parts of aminodiatomite@epoxy resin and 10 parts of 2,6-di-tert-butyl-p-cresol; the aminodiatomite@epoxy resin is prepared according to steps (1.1) to (1.3) in Example 4. The remaining raw materials and preparation process are the same as those in Example 4.

[0151] Comparative Example 3

[0152] The difference between this comparative example and Example 4 is that the temperature-controlled slow-release modified inorganic filler in Example 4 is replaced with a slow-release modified inorganic filler of equal mass; the slow-release modified inorganic filler is prepared according to step (1.4) in Example 4, and the aminodiatomite@epoxy resin in step (1.4) is replaced with neutral diatomite of equal mass. The remaining raw materials and preparation process are the same as those in Example 4.

[0153] Comparative Example 4

[0154] The difference between this comparative example and Example 4 is that the curing agent containing DA bonds in step (1.3) of Example 4 is replaced with ethylenediamine in an equal amount. The remaining raw materials and preparation process are the same as those of Example 4.

[0155] Comparative Example 5

[0156] The difference between this comparative example and Example 4 is that the temperature-controlled sustained-release modified inorganic filler used in this comparative example is prepared according to the following steps:

[0157] (1.1) In a nitrogen atmosphere, N,N'-(4,4'-methylenediphenyl)bismaleimide and furfurylamine were dissolved in tetrahydrofuran in a mass volume ratio of 1.4 g:1 g:10 mL, and refluxed at 70°C for 18 h. After removing tetrahydrofuran by rotary evaporation, the mixture was washed with ethanol and ether in sequence and dried to obtain a curing agent containing a DA bond;

[0158] (1.2) After 2,6-di-tert-butyl-p-cresol is heated to 80±3°C and melted, neutral diatomaceous earth is added thereto, and after being evenly dispersed, the mixture is evacuated to 0.02 MPa, heated to 125°C, stirred for 30 min, and then filled with nitrogen until the pressure is 0.15 MPa. After stirring for 2 h, the mixture is cooled to 80±5°C, filtered and drained, and cooled to room temperature to obtain loaded diatomaceous earth;

[0159] (1.3) dissolving silane coupling agent KH-550 in water to prepare a 10 wt% coupling agent solution; adding supported diatomaceous earth to the coupling agent solution at a mass volume ratio of 1 g:10 mL, reacting at 45° C. for 1.5 h, centrifuging, washing the precipitate with water, and drying to obtain supported amino diatomaceous earth;

[0160] (1.4) An epoxy resin, a curing agent containing a DA bond and triethylenetetramine are dissolved in acetone in a mass volume ratio of 1 g:0.75 g:0.1 g:30 mL, and a supported aminodiatomaceous earth having a mass that is 7 times that of the epoxy resin is added thereto. The mixture is refluxed at 50°C for 1.5 h. After centrifugation, the precipitate is washed with acetone and water in turn, and dried to obtain a temperature-controlled sustained-release modified inorganic filler.

[0161] The remaining raw materials and preparation process are the same as those in Example 4.

[0162] Test Example 1: Performance Test

[0163] The sealing rubber materials obtained in Examples 1 to 6 and Comparative Examples 1 to 5 were heated and vulcanized (175° C., 15 min) to make standard test pieces. After being placed at room temperature for 3 months, performance tests were performed. The test items and methods are shown in Table 8, and the results are shown in Tables 9 to 10.

[0164] Table 8

[0165]

[0166] Table 9

[0167]

[0168] Table 10

[0169]

[0170] Data Analysis and Conclusions:

[0171] (1) Compared with Comparative Example 1, the high temperature resistance and low temperature resistance of the sealing rubber materials of Examples 1 to 4 are significantly improved, especially the compression permanent deformation is significantly reduced, indicating that the formula of the present invention can improve the high and low temperature resistance of the sealing rubber material and meet the sealing requirements in extremely cold and high temperature environments.

[0172] (2) Compared with Example 3 and Comparative Example 2, the high temperature resistance of the sealing rubber material of Example 4 is significantly improved, indicating that compared with not adding the temperature-controlled slow-release modified inorganic filler, or dispersing and adding the antioxidant with the aminodiatomite@epoxy resin, loading the antioxidant in the aminodiatomite@epoxy resin to prepare the temperature-controlled slow-release modified inorganic filler is helpful to improve the high temperature resistance of the sealing rubber material. The reason is presumed to be that when the antioxidant is dispersed and added with the aminodiatomite@epoxy resin, the antioxidant is easy to migrate to the surface of the material during the storage of the sealing rubber material, causing the high temperature resistance of the material to decrease. When added in the form of temperature-controlled slow-release modified inorganic filler, the temperature of the sealing rubber material is low during storage, the thermal expansion coefficient of the epoxy resin layer is low, and the DA bond does not break, so the release rate of the antioxidant is very slow, which can prevent the antioxidant from migrating to the surface of the material and becoming ineffective; when the sealing rubber material is in a high temperature environment, the epoxy resin layer undergoes a large degree of thermal expansion, and the DA bond breaks, which accelerates the release rate of the antioxidant, thereby improving the high temperature resistance of the sealing rubber material.

[0173] (3) Compared with Comparative Example 3, the sealing rubber material of Example 4 has better high temperature resistance, indicating that the high temperature resistance of the sealing rubber material can be improved by coating the diatomite loaded with an epoxy resin layer. The reason is speculated to be that when the epoxy resin layer is not coated, the difference in the release rate of the antioxidant at high temperature and low temperature is small, and the amount released during the storage of the sealing rubber material is large. The released antioxidant migrates to the surface of the material and becomes ineffective, thereby causing the high temperature resistance of the material to decrease. After coating the epoxy resin layer, the temperature-controlled release of the antioxidant can be achieved, so that the loss during storage is less, and more antioxidant can be released under high temperature environment, thereby improving the high temperature resistance of the sealing rubber material.

[0174] (4) Compared with Comparative Example 4, the sealing rubber material of Example 4 has better high temperature resistance, indicating that the high temperature resistance of the sealing rubber material can be improved by using a curing agent containing a DA bond in the epoxy resin layer. The reason is presumed to be that the DA bond has the characteristics of breaking at high temperature and reforming at low temperature, based on which the porosity of the epoxy resin layer can be adjusted, thereby increasing the difference in the release rate of the antioxidant at low temperature and high temperature, thereby improving the high temperature resistance of the sealing rubber material.

[0175] (5) Compared with Comparative Example 5, the sealing rubber material of Example 4 has better high temperature resistance, indicating that in the process of preparing the temperature-controlled slow-release modified inorganic filler, compared with first loading the antioxidant and then coating the epoxy resin, the method of first coating and then loading can improve the high temperature resistance of the sealing rubber material. The reason is speculated to be that when coating the epoxy resin, acetone is used as the reaction medium to dissolve the curing agent containing the DA bond, and 2,6-di-tert-butyl-p-cresol is soluble in acetone. If 2,6-di-tert-butyl-p-cresol is loaded first and then coated with the epoxy resin, part of the 2,6-di-tert-butyl-p-cresol loaded in the diatomite will be dissolved during the epoxy resin coating process, resulting in the weakening of the anti-aging effect of the temperature-controlled slow-release modified inorganic filler, thereby affecting the high temperature resistance of the rubber sealing material.

[0176] Test Example 2: Sealing Test

[0177] The sealing rubber materials prepared in Examples 1 to 6 and Comparative Examples 1 to 5 were respectively used to prepare 5 sealing rings each, which were installed in a sealing pump.

[0178] The sealing pump was placed in a -42°C low-temperature box for low-temperature treatment for up to 24 hours. After being taken out, a sealing test was quickly carried out at room temperature. The performance test results and appearance description are as follows: none of the five sealing rings of Examples 1 to 6 and Comparative Examples 4 to 5 leaked, and four of the sealing rings of Comparative Example 3 leaked; the appearance of all the sealing rings of each Example and Comparative Example was not damaged.

[0179] The sealed pump was placed in a high-temperature aging box at 140°C for hot air aging for up to 200 hours. After being taken out, it was cooled at room temperature for 1 hour, and then a sealing test was performed at room temperature. The performance test results and appearance description are as follows: all five sealing rings of Examples 1 to 6 and Comparative Examples 2 to 5 did not leak, and all five sealing rings of Comparative Example 1 leaked; all five sealing rings of Examples 1 to 6 and Comparative Examples 2 to 5 had no damage in appearance, and all five sealing rings of Comparative Example 1 were broken.

[0180] The sealed pump was placed in a high-temperature aging box at 150°C for hot air aging for up to 300 hours. After being taken out, it was cooled at room temperature for 1 hour, and then a sealing test was performed at room temperature. The performance test results and appearance description are as follows: all five sealing rings of Examples 4 to 6 did not leak, all five sealing rings of Comparative Example 1 leaked, 4, 4, and 5 of the sealing rings of Examples 1 to 3 leaked, and 4, 3, 2, and 3 of the sealing rings of Comparative Examples 2 to 5 leaked; the appearance of the five sealing rings of Examples 4 to 6 was not damaged, all five sealing rings of Comparative Example 1 were broken, 2, 2, and 3 of the sealing rings of Examples 1 to 3 were broken, and 2, 0, 0, and 1 of the sealing rings of Comparative Examples 2 to 5 were broken.

[0181] Conclusion: The sealing rubber material prepared by the formula of the present invention can be used for a long time in an environment of -42 to 140°C; and when a temperature-controlled sustained-release modified inorganic filler is used, the high temperature resistance of the sealing rubber material can be further improved, so that it can be used for a long time at 150°C.

[0182] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0183] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A high-low temperature resistant and oil-resistant sealing rubber material, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of nitrile rubber; Silicone rubber 15~30 parts; 5~8 parts of vulcanizing agent; 3~8 parts of antioxidant; Plasticizer 4~8 parts; 50~105 parts of inorganic filler; 8~16 parts of additives; Colorant 0~10 parts; The inorganic filler comprises the following components in parts by weight: 0-45 parts of non-modified inorganic filler and 60-70 parts of temperature-controlled sustained-release modified inorganic filler; the temperature-controlled sustained-release modified inorganic filler is diatomaceous earth coated with an epoxy resin layer and loaded with an antioxidant; the curing agent used in the epoxy resin layer comprises a curing agent containing a DA bond.

2. The sealing rubber material according to claim 1, characterized in that: The silicone rubber is a mixed rubber of methyl vinyl silicone rubber and precipitated silica.

3. The sealing rubber material according to claim 1, characterized in that: The vulcanizing agent includes dicumyl peroxide and / or 1,3-bis(tert-butylperoxyisopropyl)benzene; the sealing rubber material also includes the following raw materials in parts by weight: 1 to 3 parts of triallyl isocyanurate.

4. The sealing rubber material according to claim 1, characterized in that: The auxiliary agent includes the following components in parts by weight: 2-5 parts of a first auxiliary agent, 1-3 parts of a second auxiliary agent, and 5-8 parts of a third auxiliary agent; the first auxiliary agent includes ferric oxide or cerium oxide; the second auxiliary agent includes microcrystalline wax 40 / 60; and the third auxiliary agent includes QST-100 silicon-based coupling agent.

5. The sealing rubber material according to claim 1, characterized in that: The antioxidant includes one or more of 2,6-di-tert-butyl-p-cresol, 4,4'-methylenebis(phenyl isocyanate), 2-mercaptobenzimidazole, 2,2,4-trimethyl-1,2-dihydroquinoline polymer and 4,4'-di(phenylisopropyl)diphenylamine.

6. The sealing rubber material according to claim 1, characterized in that: The preparation method of the temperature-controlled sustained-release modified inorganic filler is as follows: (1.1) Under the protection of inert gas, N,N'-(4,4'-methylenediphenyl)bismaleimide and furfurylamine in a mass ratio of 1.2 to 1.6:1 are used as raw materials to carry out a Diels-Alder reaction, separate the product, and obtain a curing agent containing a DA bond; (1.2) adding diatomaceous earth to an aminosilane coupling agent solution to carry out a dehydration condensation reaction, separating the product, and obtaining aminodiatomaceous earth; (1.3) dissolving epoxy resin, a curing agent containing a DA bond and triethylenetetramine in acetone in a mass ratio of 1:0.65-0.85:0.09-0.12, adding aminodiatomaceous earth thereto, carrying out a coating reaction, separating the product, and obtaining aminodiatomaceous earth@epoxy resin; (1.4) After heating and melting 2,6-di-tert-butyl-p-cresol, add aminodiatomaceous earth@epoxy resin into it, disperse it evenly, evacuate it, heat it to 122~130℃, stir it for 25~35min, and then fill it with nitrogen until the pressure is 0.13~0.20MPa. After stirring for 1.5~2.5h, separate the product and cool it to obtain a temperature-controlled sustained-release modified inorganic filler.

7. The sealing rubber material according to claim 6, characterized in that: In step (1.2), the temperature of the dehydration condensation reaction is 40-50° C., and the time is 1-1.5 h.

8. The sealing rubber material according to claim 6, characterized in that: In step (1.3), the coating reaction temperature is 45-55°C and the time is 1.5-2h.

9. The sealing rubber material according to claim 1, characterized in that: The non-modified inorganic filler includes one or more of neutral white carbon black, alkaline white carbon black, neutral diatomaceous earth and alkaline diatomaceous earth.

10. A method for preparing a sealing rubber material according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Add all raw materials except silicone rubber into an internal mixer for mixing and rubber removal to obtain NBR compound rubber; (2) adding the mixed rubber into an open mixer for mixing and sheeting to obtain an NBR rubber compound; (3) Add the silicone rubber into an open mixer for primary mixing, then add the NBR rubber material for secondary mixing, and sheet the mixture to obtain a sealing rubber material.

Citation Information

Patent Citations

  • High-strength low-temperature-resistant nitrile butadiene rubber O-shaped sealing ring

    CN111171419A