A self-healing concrete crack repair inspection method

Through the self-healing concrete crack repair inspection method, the screening and performance evaluation of self-healing concrete materials are simplified, the problem of complex and high-cost self-healing performance inspection in the existing technology is solved, and rapid and economical self-healing performance is achieved. Analysis and multi-environment testing.

CN114577563BActive Publication Date: 2024-10-29NORTHWEST ENGINEERING CORPORATION LIMITED
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202210127947.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-11
Publication Date
2024-10-29
Estimated Expiration
2042-02-11

AI Technical Summary

Technical Problem

The existing technology lacks effective methods to quickly test and evaluate the self-healing performance of self-healing concrete, resulting in a complex and costly screening process for self-healing materials.

Method used

The self-healing concrete crack repair inspection method is adopted, including the preparation of self-healing concrete mortar, formwork, prefabricated cracks, standard curing and curing in different environments. The self-healing performance is evaluated through impermeability performance tests and crack width observations.

Benefits of technology

It achieves rapid screening and qualitative and quantitative analysis of self-healing concrete materials, reduces research costs, simplifies the test process, and can simulate material properties in different environments, making it suitable for large-scale testing and comparative testing in various environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114577563B_ABST
    Figure CN114577563B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of concrete material inspection, and specifically relates to a self-healing concrete crack repair inspection method. The present invention inspects the crack repair performance of self-healing concrete through six steps: preparing self-healing concrete mortar, molding, prefabricating cracks in anti-seepage specimens, standard curing, and prefabricating and repairing test tests on cured mortar specimens. The present invention is simple to operate, and simulates the real environment of the concrete structure through different test environments, meeting the needs of different concrete materials for environmental research. The adoption of the self-healing concrete crack repair inspection method of the present invention can carry out large-scale repair detection, and can qualitatively and quantitatively study the repair effects of self-healing materials of different types and dosages on concrete, which is conducive to the preliminary screening of test materials and comparative testing of multiple environments. The mold used in the present invention is simple and does not need to be customized, saving production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete material inspection, and in particular relates to a self-healing concrete crack repair inspection method. Background Art

[0002] As the most widely used man-made building material, concrete will cause micro-damage and micro-cracks when it serves in complex and harsh environments for a long time, and expand to form macro-crack diseases under continuous load, reducing the mechanical properties and durability of concrete. Studies have shown that cement concrete itself has a certain self-healing ability, but its self-healing efficiency is relatively low and cannot meet the needs of actual engineering. Therefore, self-healing concrete is prepared by adding self-healing materials to traditional concrete materials to improve the self-healing properties of concrete, also known as "self-repairing concrete". The most widely studied type of self-healing concrete material is to add specific materials in the early production process to improve the self-healing properties of concrete, such as adding fibers, active admixtures, magnesium oxide, chemical capsules, etc.

[0003] At present, there is no specific method standard for testing and evaluating the self-healing performance of various types of self-healing concrete, and most scholars evaluate the self-healing performance of concrete through damage rate level, cumulative dissipated energy level, etc. For the preliminary research and big data screening of self-healing materials, the test process and computer mechanics are relatively complicated. Therefore, a self-healing concrete crack repair test method is proposed, which can realize the rapid test of the self-healing performance of self-healing concrete, and can qualitatively and quantitatively study the repair effect of different types and dosages of self-healing materials on concrete. This method is conducive to the preliminary determination of self-healing concrete materials, and the cost of large-scale screening tests is low. Summary of the invention

[0004] The present invention provides a self-healing concrete crack repair inspection method, which aims to provide a method for quickly screening self-repairing materials of self-healing concrete and qualitatively and quantitatively analyzing self-repairing performance, thereby saving research costs.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A self-healing concrete crack repair inspection method comprises the following steps:

[0007] Step 1: preparing self-healing concrete mortar;

[0008] Step 2: Mold making

[0009] According to the preset crack repair test group and anti-seepage performance repair test group, the self-healing mortar prepared in step 1 is respectively loaded into different groups of test molds to prepare anti-seepage samples and mortar samples, and at least three samples are prepared for each group;

[0010] Step 3: Prefabricate cracks in the impermeability specimen;

[0011] Step 4: Standard maintenance

[0012] The mortar sample in step 2 and the anti-seepage sample with cracks prefabricated in step 3 are both cured at a temperature of 20±2℃ and a humidity of not less than 95%;

[0013] Step 5: Prefabricate cracks on the mortar sample cured in step 4;

[0014] Step 6: Preset Mode Maintenance

[0015] The anti-seepage specimen cured in step 4 and the mortar specimen with cracks prefabricated in step 5 are respectively placed in a standard laboratory curing environment, an underwater environment, and a dry-wet cycle environment for curing to a specified age;

[0016] Step 7: Perform repair test

[0017] For the cracked anti-seepage samples cured to the specified age under different environments in step six, an anti-seepage performance test is carried out; for the cracked mortar samples cured to the specified age under different environments in step six, a crack width observation test is carried out.

[0018] The test mold in step 2 includes a truncated cone metal test mold and a mortar test mold. The truncated cone metal test mold is used to prepare an anti-seepage test sample, and the mortar test mold is used to prepare a mortar test sample.

[0019] The specific method for prefabricating cracks in the waterproof sample in step three is as follows: insert a blade wrapped with tape with a width of 20 mm and a thickness of 0.3 to 0.35 mm into the waterproof sample mold prepared in step two, perpendicular to the sample surface, and the blade passes through the upper and lower surfaces of the sample; after 1.5 to 2.5 hours of mold filling, shake the blade to avoid sticking, and pull out the blade when final setting is reached.

[0020] The specific method for curing the anti-seepage sample and the mortar sample in the step 4 is a standard laboratory environment, the temperature is 20±2°C, the humidity is not less than 95%, and the curing time is 26-30d; in the preset curing mode in the step 6, if in a standard laboratory environment, the temperature is 20±2°C, and the humidity is not less than 95%; if in an underwater environment, the sample is immersed in water at a temperature of 20±2°C; if in a dry-wet cycle environment, the immersion time is set to 8 hours, the temperature of the immersion water is 20±2°C, the drying time is 4 hours, and the temperature in the box is 50~70°C during drying.

[0021] The dry-wet cycle environment is achieved by a sulfate dry-wet cycle test machine.

[0022] The method for prefabricating cracks in the mortar sample in step five is to use a microcomputer-controlled compression and flexural resistance integrated machine to prefabricate cracks.

[0023] The specific method of prefabricating the cracks of the mortar specimen is as follows:

[0024] The first step is to place the mortar sample on the microcomputer-controlled compression and flexure resistance machine.

[0025] Place one of the prefabricated mortar samples on a microcomputer-controlled compression and flexure resistance integrated machine;

[0026] The second step is to apply a preset load to the mortar sample through a microcomputer-controlled compression and flexural strength machine and obtain a load-displacement curve;

[0027] The third step is to analyze the failure morphology and load-displacement curve characteristics of the prefabricated mortar specimens and obtain the crack width on the surface of the mortar specimens at different failure stages;

[0028] The fourth step is to determine the failure load to be used when prefabricating irregular cracks of preset width;

[0029] The fifth step is to apply the failure load determined in the fourth step to the remaining mortar samples to obtain mortar samples that meet the prefabricated crack width.

[0030] The microcomputer-controlled compression and flexure-resistant integrated machine comprises at least one loading cylinder, two supporting cylinders, a force loading part and a computer; the force loading part is used to apply a loading force to the mortar sample; the computer is connected to the force loading part by electrical signals; the two supporting cylinders are placed on the hydraulic platform of the microcomputer-controlled compression and flexure-resistant integrated machine; the upper part of the loading cylinder is fixedly connected to the force loading part and is located above the middle of the two supporting cylinders.

[0031] The specific method of the anti-seepage performance test in step seven is as follows:

[0032] Step 1: Take out the anti-seepage sample that has reached the specified repair age;

[0033] Step 2: After the surface of the impermeability sample is dry, put silicone rubber on the side of the impermeability sample, press the impermeability sample into the test mold of the impermeability tester, and make the two bottom surfaces of the impermeability sample level;

[0034] Step 3: Let the anti-seepage sample treated in the second step stand for 22-26 hours and then put it into the permeameter;

[0035] Step 4: Turn on the permeameter and control the water pressure at 0.7-0.8 MPa. When the water pressure reaches 0.4-0.6 MPa, start observing the water seepage on the sample surface.

[0036] Step 5: Observe once every preset time until the top surface of the anti-seepage sample is seeping water, and record the water seepage time (min) of each sample. Two samples form a group, and the average water seepage time of the two samples is used as the representative value of the water seepage time of the group of samples. Each batch of tests is completed after 6 hours;

[0037] Step 6: If the sample surface seeps water within 5 minutes, the water seepage time of the sample is considered to be 0. If there is no water seepage on the sample surface for 6 hours, then record 361 minutes. If water seeps water exactly for 6 hours, then record 360 minutes.

[0038] The specific method of the prefabricated crack width repair test in step 7 is as follows:

[0039] Step 1: Measure the width of the prefabricated cracks on the mortar samples prefabricated with cracks in step 5 respectively as the crack observation reference value;

[0040] Step 2: Place the mortar samples whose prefabricated crack widths have been measured in the first step into different environments preset in step 6 for curing, and take out the cured mortar samples at preset time intervals, and measure the prefabricated crack widths on the mortar samples until the preset inspection time is completed.

[0041] Beneficial effects:

[0042] 1. The present invention realizes the repair performance test of self-healing concrete in a relatively simple manner through six steps: preparing self-healing concrete mortar, forming a mold, prefabricating cracks in the anti-seepage sample, curing, and performing crack prefabrication and repair detection tests on the cured mortar sample. Compared with the commonly used repair performance evaluation method in the prior art, the principle is easy to understand and the operation is simple.

[0043] 2. The present invention can simulate the real environment of concrete materials through different test environments, meeting the needs of different material or environmental research.

[0044] 3. The present invention can be used to test the repair performance of large quantities of concrete, which is beneficial to the preliminary screening of test materials and comparative testing in various environments.

[0045] 4. The present invention uses a simple mold, which does not need to be customized and saves testing costs.

[0046] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the preferred embodiments of the present invention are described in detail below. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0048] Figure 1 It is a flow chart of the present invention;

[0049] Figure 2 It is a schematic diagram of the anti-seepage sample in the present invention;

[0050] Figure 3 It is a schematic diagram of a mortar sample of the present invention;

[0051] Figure 4 This is a graph showing the variation of the water permeability time of the self-healing mortar with the amount of the repairing agent under standard conditions of the present invention;

[0052] Figure 5 This is a graph showing the variation of the water permeability time of the self-healing mortar with the amount of the repairing agent under a dry-wet cycle environment of the present invention;

[0053] Figure 6 This is a graph showing the variation of the water permeability time of the self-healing mortar with the amount of the repairing agent in an underwater environment of the present invention;

[0054] Figure 7 This is a graph showing the variation of the crack healing difference with the amount of the repair agent when the repair age is 30 days;

[0055] Figure 8 This is a graph showing the variation of the crack healing difference with the amount of the repair agent when the repair age is 60 days;

[0056] Fig. 9 This is a graph showing the variation of the crack healing difference with the amount of the repair agent when the repair age is 90 days;

[0057] Fig.10 This is a graph showing the variation of the crack healing difference with the amount of the repair agent when the repair age is 120 days;

[0058] Fig.11 This is a graph showing the variation of the crack healing difference with the dosage of the repair agent when the repair age is 150 days.

[0059] In the figure:

[0060] 1- impermeability test sample; 2- mortar test sample; 3- prefabricated crack; 4- loaded crack.

[0061] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention. DETAILED DESCRIPTION

[0062] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0063] Embodiment 1:

[0064] Reference Figure 1-Figure 3 A self-healing concrete crack repair inspection method shown includes the following steps:

[0065] Step 1: preparing self-healing concrete mortar;

[0066] Step 2: Mold making

[0067] According to the preset crack repair test group and anti-seepage performance repair test group, the self-healing mortar prepared in step 1 is respectively loaded into different groups of test molds to prepare anti-seepage samples and mortar samples, and at least three samples are prepared for each group;

[0068] Step 3: Prefabricate cracks in the impermeability specimen;

[0069] Step 4: Standard maintenance

[0070] The mortar sample in step 2 and the anti-seepage sample with cracks prefabricated in step 3 are both cured at a temperature of 20±2℃ and a humidity of not less than 95%;

[0071] Step 5: Prefabricate cracks on the mortar sample cured in step 4;

[0072] Step 6: Preset Mode Maintenance

[0073] The anti-seepage specimen cured in step 4 and the mortar specimen with cracks prefabricated in step 5 are respectively placed in a standard laboratory curing environment, an underwater environment, and a dry-wet cycle environment for curing to a specified age;

[0074] Step 7: Perform repair test

[0075] For the cracked anti-seepage samples cured to the specified age under different environments in step six, an anti-seepage performance test is carried out; for the cracked mortar samples cured to the specified age under different environments in step six, a crack width observation test is carried out.

[0076] In actual use, when preparing the self-healing concrete mortar in step 1, it is necessary to screen out the coarse aggregate from the self-healing concrete to be tested. This is because most concrete cracks appear inside the mortar, on the contact surface between the mortar and the aggregate, and inside the aggregate, but the self-healing of the self-healing concrete only exists inside the mortar. For the purpose of the test, the self-healing mortar is prepared using the self-healing concrete with the coarse aggregate screened out.

[0077] The self-healing concrete mortar in this embodiment is made of a hydraulic self-healing mortar, which has a self-healing function. The formula of the hydraulic self-healing mortar is as follows: it includes glue, aggregate, admixture, repair agent, fiber and water; the glue, aggregate, admixture, repair agent and water are mixed according to the following weight parts: 270-290 parts of glue, 700-750 parts of aggregate, 4-4.5 parts of admixture, 1.5-9 parts of repair agent, and 100-110 parts of water. The fibers are mixed by volume, and the percentage of the volume of the fibers to the total volume is 0.5% to 1.2%; the adhesive is a mixture of cement and fly ash in a mass ratio of (8 to 9): (1 to 2); the cement is PO 42.5 silicate cement, and the fly ash is fly ash of grade III or above; the aggregate is natural sand or machine-made sand in zone 2; the admixture is a mixture of a water reducer and an air entraining agent, wherein the amount of the water reducer is 4 to 4.4 parts by weight, and the amount of the air entraining agent is 0 to 0.1 parts by weight; the water reducer is a polycarboxylate water reducer; the repair agent is a cement-based permeable crystallization material; the fibers are short-cut non-continuous fibers, and the short-cut non-continuous fibers are one of steel fibers, polypropylene fibers, basalt fibers or carbon fibers.

[0078] The above-mentioned hydraulic self-healing mortar is prepared by the following method: add water to the stirring device and run it idle for several minutes, then drain the water therein to ensure that the wall of the stirring barrel is completely wetted; then put the aggregate weighed by mass and the fiber prepared by volume ratio into the stirring device treated by step one and dry mix for 110 to 130 seconds to make the fiber evenly distributed, and then add the glue and repair agent mixed evenly by mass and stir for 50 to 70 seconds; then, fully mix the admixture weighed by mass with water, pour 50% of the mixed liquid into the stirring device and stir for 55 to 65 seconds; then, add the remaining 50% of the mixed liquid after the admixture and water are fully mixed into the slurry prepared in step three, and force stir for 110 to 130 seconds before discharging.

[0079] In actual use, when preparing the self-healing concrete mortar in step 1, it is necessary to screen out the coarse aggregate from the self-healing concrete to be tested. This is because most concrete cracks appear inside the mortar, on the contact surface between the mortar and the aggregate, and inside the aggregate, but the self-healing of the self-healing concrete only exists inside the mortar. For the purpose of the test, the self-healing mortar is prepared using the self-healing concrete with the coarse aggregate screened out.

[0080] By adopting the technical solution of the present invention, the repair performance of self-healing concrete can be tested through relatively simple water resistance tests and crack observation tests. Compared with the commonly used repair performance evaluation methods in the prior art, such as damage rate level evaluation and cumulative dissipated energy level evaluation, the principle of the method of the present invention is easy to understand and the operation is simple.

[0081] The present invention can carry out large-scale repair detection, is conducive to the preliminary screening of test materials and comparative testing in various environments, uses a simple mold, does not need to be customized, and saves production costs.

[0082] Embodiment 2:

[0083] Reference Figure 1 , Figure 2 and Figure 3 A self-healing concrete crack repair inspection method is shown. Based on the first embodiment, the test mold in step two includes a truncated cone metal test mold and a mortar test mold. The truncated cone metal test mold is used to prepare an anti-seepage sample, and the mortar test mold is used to prepare a mortar sample.

[0084] In specific applications, the truncated cone metal test molds and mortar test molds used are the mortar impermeability test molds and crack observation test molds specified in the "Concrete Test Molds" (JG 237-2008), the industry standard of the construction industry of the People's Republic of China. The test molds specified in the existing specifications are used, and there is no need to customize the molds. The test method is universal and cost-effective.

[0085] Embodiment three:

[0086] Reference Figure 1 , Figure 2 and Figure 3 A self-healing concrete crack repair inspection method is shown. On the basis of Example 1, the specific method for prefabricating cracks in the anti-seepage sample in step three is: in step 2, a blade wrapped with tape with a width of 20 mm and a thickness of 0.3-0.35 mm is inserted into the anti-seepage sample in the test mold for the anti-seepage sample vertically on the sample surface, and the blade passes through the upper and lower surfaces of the sample; after molding for 1.5-2.5 hours, shake the blade to avoid sticking, and pull out the blade when initial setting is reached.

[0087] In this technical solution, the blade is shaken 1.5 to 2.5 hours after mold filling to avoid sticking. At this time, the mortar has hardened to a certain extent, but has not reached initial setting. Shaking will not cause minor damage to the inside and surface of the mortar sample. The cracks can be preformed by pulling out the blade during initial setting.

[0088] The technical solution is simple and convenient to prefabricate cracks in anti-seepage specimens, and can meet the needs of repair inspection.

[0089] Embodiment 4:

[0090] Reference Figure 1 , Figure 2 and Figure 3 A self-healing concrete crack repair inspection method is shown. On the basis of Example 1, the specific method for curing the anti-seepage sample and the mortar sample in the step 4 is a standard laboratory environment, the temperature is 20±2°C, the humidity is not less than 95%, and the curing time is 26-30d; in the preset curing mode in the step 6, if in a standard laboratory environment, the temperature is 20±2°C, and the humidity is not less than 95%; if in an underwater environment, the sample is immersed in water at a temperature of 20±2°C; if in a dry-wet cycle environment, the immersion time is set to 8 hours, the temperature of the immersion water is 20±2°C, the drying time is 4 hours, and the temperature in the box is 50~70°C during drying.

[0091] Furthermore, the dry-wet cycle environment is achieved by a sulfate dry-wet cycle test machine.

[0092] In specific applications, you can choose the corresponding curing conditions according to your own research needs. Then set the temperature and humidity accordingly. The curing time is determined by the age required for the test.

[0093] The sulfate dry-wet cycle test machine used is the existing technology.

[0094] Embodiment five:

[0095] Reference Figure 1 , Figure 2 and Figure 3 A self-healing concrete crack repair inspection method is shown. Based on the first embodiment, the method for prefabricating cracks in the mortar sample in step five is to use a microcomputer-controlled compression and flexural resistance integrated machine to prefabricate cracks.

[0096] Furthermore, the specific method of crack prefabrication is as follows:

[0097] The first step is to place the mortar sample on the microcomputer-controlled compression and flexure resistance machine.

[0098] Place one of the prefabricated mortar specimens on a three-point bending test device;

[0099] The second step is to apply a preset load to the mortar specimen through a three-point bending test device and obtain a load-displacement curve;

[0100] The third step is to analyze the failure morphology and load-displacement curve characteristics of the prefabricated mortar specimens and obtain the crack width on the surface of the mortar specimens at different failure stages;

[0101] The fourth step is to determine the failure load to be used when prefabricating irregular cracks of preset width;

[0102] The fifth step is to apply the failure load determined in the fourth step to the remaining mortar samples to obtain mortar samples that meet the prefabricated crack width.

[0103] Furthermore, the microcomputer-controlled compression and flexure-resistant integrated machine includes at least one loading cylinder, two supporting cylinders, a force loading part and a computer; the force loading part is used to apply loading force to the mortar sample; the computer is connected to the force loading part by electrical signals; the two supporting cylinders are placed on the hydraulic platform of the microcomputer-controlled compression and flexure-resistant integrated machine; the upper part of the loading cylinder is fixedly connected to the force loading part and is located above the middle of the two supporting cylinders.

[0104] The use of this technical solution to prefabricate cracks in mortar specimens can not only obtain prefabricated crack widths that meet the requirements, but also solve the problems of uniformity and fixity of crack shapes in the preparation of cracked specimens with existing concrete mortars. In particular, the prefabrication of cracks in self-healing concrete mortars can effectively avoid the influence of carbonization reactions during curing on the self-healing process of concrete.

[0105] Embodiment six:

[0106] Reference Figure 1 , Figure 2 and Figure 3 The self-healing concrete crack repair inspection method shown in the embodiment is based on the first embodiment. The specific method of the anti-seepage performance test in step six is ​​as follows:

[0107] Step 1: Take out the anti-seepage sample that has reached the specified repair age;

[0108] Step 2: After the surface of the impermeability sample is dry, put silicone rubber on the side of the impermeability sample, press the impermeability sample into the test mold of the impermeability tester, and make the two bottom surfaces of the impermeability sample level;

[0109] Step 3: Let the anti-seepage sample treated in the second step stand for 22-26 hours and then put it into the permeameter;

[0110] Step 4: Turn on the permeameter and control the water pressure at 0.7-0.8 MPa. When the water pressure reaches 0.4-0.6 MPa, start observing the water seepage on the sample surface.

[0111] Step 5: Observe once at preset intervals until the top surface of the impermeable sample is seeping with water. Record the water seepage time / (min) of each sample. Two samples form a group, and the average water seepage time of the two samples is used as the representative value of the water seepage time of the group of samples. Each batch of tests is completed after 6 hours.

[0112] For the ordinary mortar impermeability test, the pressure holding time for determining the impermeability grade is generally 1 hour. In order to determine the impermeability performance of the cracked impermeable sample after healing, a 6-hour pressure holding time is determined in this embodiment, which is sufficient to illustrate the impermeability performance of the sample.

[0113] Step 5: If the sample surface seeps water within 5 minutes, the water seepage time of the sample is considered to be 0. If there is no water seepage on the sample surface for 6 hours, then record 361 minutes. If water seeps water exactly for 6 hours, then record 360 minutes.

[0114] In actual use, if the sample seeps water on the surface within 5 minutes, it means that the sample has poor anti-seepage performance and almost no self-healing reaction of the prefabricated cracks; if the sample seeps water on the surface within 5 minutes to 360 minutes, then according to the actual seepage time record, if the sample still does not seep water after more than 6 hours, it can be considered that the sample prefabricated cracks have a good self-healing reaction, and the sample has achieved self-healing of cracks under this curing environment, and can withstand a water pressure of 0.4 to 0.6 MPa. This recording method can qualitatively analyze the self-healing of different amounts of self-healing materials at different curing ages under different curing environments.

[0115] The silicone rubber is put on the side of the anti-seepage sample to prevent water from seeping out from the side of the anti-seepage sample.

[0116] Embodiment seven:

[0117] Reference Figure 1 , Figure 2 and Figure 3 A self-healing concrete crack repair inspection method is shown. Based on the first embodiment, the specific method of the prefabricated crack width repair test in step six is ​​as follows:

[0118] Step 1: Take the mortar sample with prefabricated cracks in step 5, and measure the width of the prefabricated cracks on the mortar sample;

[0119] Step 2: Curing the measured mortar samples again, taking out the cured mortar samples at preset intervals, and measuring the width of the prefabricated cracks on them until the preset inspection time is completed.

[0120] Through the above method, the self-healing concrete crack width repair test was realized simply and conveniently, laying the foundation for the preliminary screening of materials.

[0121] The measurement accuracy in this embodiment is 0.001 mm. Since the crack width is 0.2-0.4 mm, the width changes slightly during self-healing, and the measurement accuracy of 0.001 mm can more accurately show the healing status of the crack.

[0122] Embodiment eight:

[0123] Reference Figure 1-Figure 3 , a self-healing concrete crack repair inspection method, comprising the following steps: step 1: preparing self-healing concrete mortar;

[0124] The self-healing concrete to be tested was prepared by sieving out the coarse aggregate to prepare the self-healing mortar.

[0125] Step 2: Mold making

[0126] According to the preset crack repair test group and impermeability repair test group, the self-healing mortar prepared in step 1 is respectively loaded into different groups of truncated cone metal test molds and mortar test molds. The truncated cone metal test mold is used to prepare impermeability sample 1, and the mortar test mold is used to prepare mortar sample 2. Three samples are prepared in each group;

[0127] Step 3: Prefabricate cracks in the impermeability specimen;

[0128] Insert a 20mm wide and 0.3-0.35mm thick tape-wrapped blade into the anti-seepage sample 1 prepared in step 2, shake the blade after molding for 1.5-2.5 hours to avoid adhesion, and pull out the blade when initial setting is reached to obtain a prefabricated crack 3 with a width of 0.3-0.35mm running through the top and bottom;

[0129] Step 4: Maintenance

[0130] The mortar sample 2 in step 2 and the anti-seepage sample 1 with prefabricated cracks in step 3 are both cured in a standard laboratory environment for 26-30 days;

[0131] Step 5: Prefabricate cracks on the mortar sample 2 cured in step 4;

[0132] The mortar sample 2 after demoulding and standard curing for 26-30 days is subjected to three-point bending loading to obtain a loading prefabricated crack 4;

[0133] Step 6: The anti-seepage sample 1 with prefabricated cracks in step 3 and the mortar sample with prefabricated cracks in step 5 are placed in a preset environment and cured to the specified age.

[0134] The specific maintenance plan is as follows:

[0135] If it is in a standard laboratory environment, the temperature is 20±2℃ and the humidity is not less than 95%; if it is in an underwater environment, the sample is immersed in water at a temperature of 20±2℃; if it is in a dry-wet cycle environment, the immersion time is set to 8 hours, the immersion water temperature is 20±2℃, the drying time is 4 hours, and the temperature in the box is 50~70℃ during drying.

[0136] The dry-wet cycle environment is achieved through a sulfate dry-wet cycle test machine.

[0137] The corresponding curing conditions can be selected according to the test needs;

[0138] Step 7: Perform repair test

[0139] The specific steps of the crack width observation test are as follows:

[0140] Step 1: Take the mortar sample 2 with cracks prefabricated in step 5, and measure the width of the prefabricated cracks 4 on the mortar sample 2;

[0141] Step 2: Curing the measured mortar sample 2 in the same manner as step 6, and taking out the cured mortar sample 2 at preset intervals, and measuring the width of the prefabricated cracks 4 thereon until the preset inspection time is completed.

[0142] The specific steps of the crack repair test are as follows:

[0143] Step 1: Take the mortar sample 2 with cracks prefabricated in step 5, and measure the width of the loaded crack 4 on the mortar sample 2;

[0144] Step 2: The measured mortar sample 2 is cured again in the same manner as step 4, and at every preset time interval, the cured mortar sample 2 is taken out and the width of the loading crack 4 thereon is measured until the preset inspection time is completed.

[0145] The accuracy of measuring the mortar sample 2 using the crack observation instrument is 0.001mm.

[0146] Among them, the crack observation instrument adopts the existing technology. It is composed of a hardware device consisting of an adjustable high-definition camera, an adjustable control bracket, and a ruler, and uses the Supereyes measurement system to achieve high-precision measurement.

[0147] The specific steps of the anti-seepage performance repair test are as follows:

[0148] Step 1: Take out the anti-seepage sample 1 to be tested that has reached the specified repair age;

[0149] Step 2: After the surface of the anti-seepage sample 1 is dry, put silicone rubber on the side of the anti-seepage sample 1, press the anti-seepage sample 1 into the test mold of the compression tester, and make the upper and lower bottom surfaces of the anti-seepage sample 1 level;

[0150] Step 3: After standing for 24 hours, put it into the permeameter and conduct a water permeability test. Turn on the permeameter and control the water pressure at 0.75 MPa. When the water pressure reaches about 0.5 MPa, start observing the water seepage on the surface of the sample.

[0151] Step 4: Observe once every 5 minutes until the top surface of the anti-seepage sample 1 is seeping water, record the water penetration time (min) of each anti-seepage sample 1, two anti-seepage samples 1 are grouped together, and the average water penetration time of the two anti-seepage samples 1 is taken as the representative value of the water penetration time of the group of samples. Each batch of tests is completed after 6 hours;

[0152] Step 5: If the sample surface seeps water within 5 minutes, the water seepage time of the sample is considered to be 0. If there is no water seepage on the sample surface for 6 hours, then record 361 minutes. If water seeps water exactly for 6 hours, then record 360 minutes.

[0153] The truncated cone metal test mold used in this embodiment has an upper diameter of 70 mm, a lower diameter of 80 mm, and a height of 30 mm; the length of the mortar test mold is 160 mm, the width is 40 mm, and the height is 40 mm. According to the People's Republic of China Construction Industry Standard "Concrete Test Mold" (JG 237-2008); the slurry flexural strength test, crack width test test, and longitudinal wave test test all use a 40mm×40mm×160mm cubic triple plastic mold; the slurry impermeability test uses a truncated cone metal test mold with an upper diameter of 70 mm, a lower diameter of 80 mm, and a height of 30 mm.

[0154] The method used to test the crack repair results of self-healing mortar is not only simple but also highly practical. It provides a strong guarantee for the prevention of macro cracks and repair of micro cracks in concrete matrix under different environments, an effective method to improve the durability of concrete structures, and its application in engineering fields such as concrete structure reinforcement and repair and disaster prevention and mitigation.

[0155] Embodiment nine:

[0156] Reference Figure 4-Figure 11 , a self-healing concrete crack repair inspection method

[0157] This example provides a self-healing mortar, which is composed of cement, fly ash, sand, steel fiber, repair agent, water reducer, air entraining agent and water, wherein water is 105 parts, cement is 224 parts, fly ash is 56 parts, sand is 731 parts, water reducer is 4.2 parts, air entraining agent is 0.04 parts, steel fiber volume content is 0.5%, and repair agent is 0 parts. The water reducer is a polycarboxylate water reducer, and the repair agent is a cement-based permeable crystallization material.

[0158] The crack repairing ability of the above self-healing mortar was tested through the following steps.

[0159] The sample preparation specifications are as follows: the anti-seepage sample 1 with an upper diameter of 70 mm, a lower diameter of 80 mm, a height of 30 mm, a crack with a width of 0.3 mm reserved on the upper surface, and the mortar sample 2 with a length of 160 mm, a width of 40 mm, and a height of 40 mm.

[0160] 2) Conventional standard pre-curing: Place the prepared anti-seepage sample 1 and mortar sample 2 in a standard laboratory environment for curing for 26 to 30 days;

[0161] 3) The pre-cured mortar test mold 2 is subjected to a three-point bending loading prefabricated crack method to obtain a loaded prefabricated crack 4;

[0162] 4) Preset curing: The prefabricated crack waterproof specimen 1 and the mortar specimen 2 are placed in a standard laboratory environment (temperature of 20±2℃, humidity not less than 95%); underwater environment (underwater temperature of 20±2℃); dry-wet cycle environment (immersion in water at 20±2℃ for 8 hours, drying in a box at 50~70℃ for 4 hours), and the curing age is 30d, 60d, 90d, 120d, and 150d.

[0163] 5) Carry out repair detection test

[0164] (1) Anti-seepage performance repair test

[0165] The specific steps of the anti-seepage performance repair test are as follows:

[0166] Step 1: Take out the anti-seepage samples 1 to be tested with a curing age of 30d, 60d, 90d, 120d, and 150d;

[0167] Step 2: After the surface of the impermeability sample 1 is dried, silicone rubber is put on the side of the impermeability sample 1, and then it is pressed into the test mold of the impermeability tester, and the upper and lower bottom surfaces of the impermeability sample 1 are level;

[0168] Step 3: After standing for 24 hours, put it into the permeameter and conduct a water permeability test. Turn on the permeameter and control the water pressure at 0.75 MPa. When the water pressure is applied to about 0.5 MPa, start observing the surface water seepage of the anti-seepage sample 1 at different curing ages;

[0169] Step 4: Observe once every 5 minutes until the top surface of the anti-seepage sample 1 is seeping water, record the water penetration time (min) of each anti-seepage sample 1, two anti-seepage samples 1 are grouped together, and the average water penetration time of the two anti-seepage samples 1 is taken as the representative value of the water penetration time of the group of samples. Each batch of tests is completed after 6 hours;

[0170] Step 5: If the sample surface seeps water within 5 minutes, the water seepage time of the sample is considered to be 0. If there is no water seepage on the sample surface for 6 hours, then record 361 minutes. If water seeps water exactly for 6 hours, then record 360 minutes.

[0171] (2) Crack repair test

[0172] The specific steps are as follows:

[0173] Step 1: Take the mortar sample 2 with prefabricated cracks, and measure the width of the prefabricated cracks on the mortar sample 2 as the crack observation reference value;

[0174] Step 2: The measured mortar sample 2 is cured in different environments again, and the cured mortar sample 2 is taken out every 30 days, and the width of the prefabricated cracks is measured and recorded, until the measurement of the mortar sample 2 with a curing age of 150 days is completed.

[0175] Among them, the crack observation instrument is a hardware device composed of an adjustable high-definition camera, an adjustable control bracket, and a ruler, and high-precision measurement is achieved by the Supereyes measurement system.

[0176] The anti-seepage performance repair test of mortar was used to evaluate the anti-seepage performance of the self-healing mortar, and the micro-crack observation method was used to quantify the self-repairing effect of cracks. A simple and practical method for testing self-healing concrete was obtained.

[0177] 4) See Table 1 and Table 2 for test results.

[0178] Embodiment ten:

[0179] Reference Figure 3-Figure 10 This example provides a self-healing mortar, which is composed of cement, fly ash, sand, steel fiber, repair agent, water reducer, air entraining agent and water, wherein there are 105 parts of water, 224 parts of cement, 56 parts of fly ash, 731 parts of sand, 4.2 parts of water reducer, 0.04 parts of air entraining agent, 0.5% by volume of steel fiber, and 1.7 parts of repair agent, wherein the water reducer is a polycarboxylate water reducer, and the repair agent is a cement-based permeable crystallization material.

[0180] The test process of the crack repair ability of the above self-healing mortar is the same as that of Example 9. The test results are shown in Tables 1 and 2.

[0181] Embodiment eleven:

[0182] Reference Figure 3-Figure 10 This example provides a self-healing mortar, which is composed of cement, fly ash, sand, steel fiber, repair agent, water reducer, air entraining agent and water, wherein there are 105 parts of water, 224 parts of cement, 56 parts of fly ash, 731 parts of sand, 4.2 parts of water reducer, 0.04 parts of air entraining agent, 0.5% by volume of steel fiber, and 3.4 parts of repair agent, wherein the water reducer is a polycarboxylate water reducer, and the repair agent is a cement-based permeable crystallization material.

[0183] The test process of the crack repair ability of the above self-healing mortar is the same as that of Example 9. The test results are shown in Tables 1 and 2.

[0184] Embodiment 12:

[0185] Reference Figure 3-Figure 10 This example provides a self-healing mortar, which is composed of cement, fly ash, sand, steel fiber, repair agent, water reducer, air entraining agent and water, wherein water is 105 parts, cement is 224 parts, fly ash is 56 parts, sand is 731 parts, water reducer is 4.2 parts, air entraining agent is 0.04 parts, steel fiber volume content is 0.5%, and repair agent is 5 parts. The water reducer is a polycarboxylate water reducer, and the repair agent is a cement-based permeable crystallization material.

[0186] The test process of the crack repair ability of the above self-healing mortar is the same as that of Example 9. The test results are shown in Tables 1 and 2.

[0187] Embodiment 13:

[0188] Reference Figure 3-Figure 10 This example provides a self-healing mortar, which is composed of cement, fly ash, sand, steel fiber, repair agent, water reducer, air entraining agent and water, wherein there are 105 parts of water, 224 parts of cement, 56 parts of fly ash, 731 parts of sand, 4.2 parts of water reducer, 0.04 parts of air entraining agent, 0.5% by volume of steel fiber, and 6.7 parts of repair agent; the water reducer is a polycarboxylate water reducer, and the repair agent is a cement-based permeable crystallization material.

[0189] The test process of the crack repair ability of the above self-healing mortar is the same as that of Example 9. The test results are shown in Tables 1 and 2.

[0190] Embodiment 14:

[0191] Reference Figure 3-Figure 10 This example provides a self-healing mortar, which is composed of cement, fly ash, sand, steel fiber, repair agent, water reducer, air entraining agent and water, wherein there are 105 parts of water, 224 parts of cement, 56 parts of fly ash, 731 parts of sand, 4.2 parts of water reducer, 0.04 parts of air entraining agent, 0.5% by volume of steel fiber, and 8.4 parts of repair agent; the water reducer is a polycarboxylate water reducer, and the repair agent is a cement-based permeable crystallization material.

[0192] The test process of the crack repair ability of the above self-healing mortar is the same as that of Example 9. The test results are shown in Tables 1 and 2.

[0193] In Example 9 to Example 14, the self-healing mortar anti-seepage sample 1 was used as the object of investigation for the self-repairing anti-seepage performance, and the microscopic crack observation method was used to quantify the self-repairing effect of the cracks in the mortar sample 2. The water seepage time of the self-healing mortar anti-seepage samples under different environments and with different repair agent dosages at different ages is shown in Table 1, and the crack width of the self-healing mortar samples under different environments and with different repair agent dosages at different ages is shown in Table 2.

[0194] Table 1 Water seepage time of different types of self-healing slurry samples at different ages under different environments

[0195]

[0196] Table 2 Crack widths of different types of self-healing slurry samples at different ages under different environments

[0197]

[0198] The following conclusions can be drawn from the above test results:

[0199] The self-healing mortar used in the present invention has certain self-diagnosis and self-repair capabilities and good anti-seepage performance. The steel fiber can reduce shrinkage cracks generated during mortar molding, and the repair agent can repair micro cracks inside the mortar. The two can work together in the mortar.

[0200] Through the self-healing mortar crack repair test method, it can be seen that the best environment for self-healing slurry crack repair is underwater environment. When the dosage of the repair agent is 8.4 parts, the crack repair effect is significant. When the repair age is 150d, the average value of the maximum repairable crack is 0.16mm, and the penetration time reaches more than 360min, and continues to increase with the increase of the repair age.

[0201] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

[0202] In the absence of conflicts, technicians in this field can combine the relevant technical features in the above examples according to actual conditions to achieve corresponding technical effects. The specific combinations are not described here one by one.

[0203] It should be noted that all directional indications (such as up, down, left, right, front, back, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0204] The above are only preferred embodiments of the present invention. The present invention will not be limited to the embodiments shown herein, but should conform to the widest scope consistent with the principles and novel features disclosed herein. Any simple modification, equivalent changes and modifications made to the above embodiments according to the technical essence of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A self-healing concrete crack repair inspection method, It is characterized in that The following steps are included: Step 1: preparing self-healing concrete mortar; Step 2: Mold making According to the preset crack repair test group and anti-seepage performance repair test group, the self-healing mortar prepared in step 1 is respectively loaded into different groups of test molds to prepare anti-seepage samples and mortar samples, and at least three samples are prepared for each group; Step 3: Prefabricate cracks in the impermeability specimen; Step 4: Standard maintenance The mortar sample in step 2 and the anti-seepage sample with cracks prefabricated in step 3 are both cured at a temperature of 20±2℃ and a humidity of not less than 95%; Step 5: Prefabricate cracks on the mortar sample cured in step 4; Step 6: Preset Mode Maintenance The anti-seepage specimen cured in step 4 and the mortar specimen with cracks prefabricated in step 5 are respectively placed in a standard laboratory curing environment, an underwater environment, and a dry-wet cycle environment for curing to a specified age; Step 7: Perform repair test For the cracked anti-seepage samples cured to the specified age under different environments in step 6, an anti-seepage performance test is conducted; for the cracked mortar samples cured to the specified age under different environments in step 6, a crack width observation test is conducted to achieve a preliminary determination of the self-healing concrete material; The formula of the self-healing concrete mortar is as follows: it includes adhesive, aggregate, admixture, repair agent, fiber and water; the adhesive, aggregate, admixture, repair agent and water are mixed according to the following weight parts: 270-290 parts of adhesive, 700-750 parts of aggregate, 4-4.5 parts of admixture, 1.5-9 parts of repair agent, and 100-110 parts of water; the fiber is mixed by volume, and its volume accounts for 0.5%-1.2% of the total volume; the adhesive is made of cement and fly ash in a mass ratio of 8-9:1-2; the cement adopts PO 42.5 Portland cement, fly ash is fly ash of grade III or above; aggregate is natural sand or machine-made sand in zone 2; admixture is a mixture of water reducer and air entraining agent, wherein the amount of water reducer is 4-4.4 parts by weight, and the amount of air entraining agent is 0-0.1 parts by weight; the water reducer is polycarboxylate water reducer; the repair agent is cement-based permeable crystallization material; the fiber is short-cut non-continuous fiber, and the short-cut non-continuous fiber is one of steel fiber, polypropylene fiber, basalt fiber or carbon fiber; The self-healing concrete mortar is prepared by the following method: adding water to the stirring device and running it idle for several minutes, then draining the water therein to ensure that the wall of the stirring barrel is completely wetted; then the aggregate weighed by mass and the fiber prepared by volume ratio are put into the stirring device treated by step one for dry mixing for 110 to 130 seconds to make the fiber evenly distributed, and then the glue and the repair agent are evenly mixed by mass and stirred for 50 to 70 seconds; then, the admixture weighed by mass is fully mixed with water, and 50% of the mixed liquid is poured into the stirring device and stirred for 55 to 65 seconds; then, the remaining 50% of the mixed liquid after the admixture and water are fully mixed is added to the slurry prepared in step three, and the material is discharged after forced stirring for 110 to 130 seconds; When preparing the self-healing concrete mortar, the self-healing concrete to be tested is screened to remove the coarse aggregate therein; The method for prefabricating cracks in the mortar sample in step 5 is to use a microcomputer-controlled compression and flexure resistance integrated machine to prefabricate cracks; The specific method of prefabricating the cracks of the mortar specimen is as follows: The first step is to place the mortar sample on the microcomputer-controlled compression and flexure resistance machine. One of the prefabricated mortar samples is placed in a microcomputer-controlled compression and flexure resistance integrated machine; The second step is to apply a preset load to the mortar sample through a microcomputer-controlled compression and flexural strength machine and obtain a load-displacement curve; The third step is to analyze the failure morphology and load-displacement curve characteristics of the prefabricated mortar specimens and obtain the crack width on the surface of the mortar specimens at different failure stages; The fourth step is to determine the failure load to be used when prefabricating irregular cracks of preset width; The fifth step is to apply the failure load determined in the fourth step to the remaining mortar samples to obtain mortar samples that meet the prefabricated crack width.

2. A self-healing concrete crack repair inspection method as claimed in claim 1, Features: The test mold in step 2 includes a truncated cone metal test mold and a mortar test mold. The truncated cone metal test mold is used to prepare an anti-seepage test sample, and the mortar test mold is used to prepare a mortar test sample.

3. A self-healing concrete crack repair inspection method as claimed in claim 1, Features: The specific method for prefabricating cracks in the waterproof sample in step three is as follows: insert a blade wrapped with tape with a width of 20 mm and a thickness of 0.3 to 0.35 mm into the waterproof sample mold prepared in step two, perpendicular to the sample surface, and the blade passes through the upper and lower surfaces of the sample; after 1.5 to 2.5 hours of mold filling, shake the blade to avoid sticking, and pull out the blade when final setting is reached.

4. A self-healing concrete crack repair inspection method as claimed in claim 1, It is characterized in that The specific method for curing the anti-seepage sample and the mortar sample in the step 4 is a standard laboratory environment, the temperature is 20±2°C, the humidity is not less than 95%, and the curing time is 26-30d; in the preset curing mode in the step 6, if in a standard laboratory environment, the temperature is 20±2°C, and the humidity is not less than 95%; if in an underwater environment, the sample is immersed in water at a temperature of 20±2°C; if in a dry-wet cycle environment, the immersion time is set to 8 hours, the temperature of the immersion water is 20±2°C, the drying time is 4 hours, and the temperature in the box is 50~70°C during drying.

5. A self-healing concrete crack repair inspection method as claimed in claim 4, Features: The dry-wet cycle environment is achieved by a sulfate dry-wet cycle test machine.

6. A self-healing concrete crack repair inspection method as claimed in claim 1, Features: The microcomputer-controlled compression and flexure-resistant integrated machine comprises at least one loading cylinder, two supporting cylinders, a force loading part and a computer; the force loading part is used to apply a loading force to the mortar sample; the computer is connected to the force loading part by electrical signals; the two supporting cylinders are placed on the hydraulic platform of the microcomputer-controlled compression and flexure-resistant integrated machine; the upper part of the loading cylinder is fixedly connected to the force loading part and is located above the middle of the two supporting cylinders.

7. A self-healing concrete crack repair inspection method as claimed in claim 1, It is characterized in that The specific method of the anti-seepage performance test in step seven is as follows: Step 1: Take out the anti-seepage sample that has reached the specified repair age; Step 2: After the surface of the impermeability sample is dry, put silicone rubber on the side of the impermeability sample, press the impermeability sample into the test mold of the impermeability tester, and make the two bottom surfaces of the impermeability sample level; Step 3: Let the anti-seepage sample treated in the second step stand for 22-26 hours and then put it into the permeameter; Step 4: Turn on the permeameter and control the water pressure at 0.7-0.8 MPa. When the water pressure reaches 0.4-0.6 MPa, start observing the water seepage on the sample surface. Step 5: Observe once every preset time until the top surface of the anti-seepage sample is seeping water, and record the water seepage time (min) of each sample. Two samples form a group, and the average water seepage time of the two samples is used as the representative value of the water seepage time of the group of samples. Each batch of tests is completed after 6 hours; Step 6: If the sample surface seeps water within 5 minutes, the water seepage time of the sample is considered to be 0. If there is no water seepage on the sample surface for 6 hours, then record 361 minutes. If water seeps water exactly for 6 hours, then record 360 minutes.

8. A self-healing concrete crack repair inspection method as claimed in claim 1, It is characterized in that The specific method of the prefabricated crack width repair test in step 7 is as follows: Step 1: Measure the width of the prefabricated cracks on the mortar samples prefabricated with cracks in step 5 respectively as the crack observation reference value; Step 2: Place the mortar samples whose prefabricated crack widths have been measured in the first step into different environments preset in step 6 for curing, and take out the cured mortar samples at preset time intervals, and measure the prefabricated crack widths on the mortar samples until the preset inspection time is completed.

Citation Information

Patent Citations

  • Evaluation method of self-repairing effect of self-repairing cement-based material

    CN105300801A

  • Internal crack self-healing effect evaluation method for cement-based material

    CN108256151A

  • Test method for researching concrete crack chemical excitation healing

    CN110220778A

  • Preparation method of crack self-repairing material for concrete

    CN110294609A

  • Self-healing concrete and preparation method thereof