A lithium iron phosphate-graphene strong coupling material and preparation method thereof
By using phosphorylated small graphene to react with iron source, lithium source, and phosphorus source under high-temperature solvothermal conditions, a lithium iron phosphate-graphene strong coupling material is formed, which solves the problem of low conductivity and Li+ diffusivity of lithium iron phosphate cathode material. problem, achieving efficient and environmentally friendly preparation and performance improvement, and is suitable for lithium-ion batteries and other fields.
Patent Information
- Application Number
- CN202210147030.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-17
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-02-17
AI Technical Summary
Lithium iron phosphate cathode material limits its application due to low conductivity and low Li+ diffusivity. The existing graphene coating method requires organic solvents and surfactants, resulting in pollution and complicated processes, making it difficult to achieve industrialization.
Phosphated small graphene is used as a nucleating agent and reacts with iron source, lithium source and phosphorus source under high-temperature solvothermal conditions to form a strong lithium iron phosphate-graphene coupling material without the need for additional organic solvents and surfactants. Embedded strong coupling.
It achieves the efficient and environmentally friendly preparation of lithium iron phosphate-graphene strong coupling materials, improves the internal conductivity and crystallinity of the material, reduces pollution, and is suitable for lithium-ion batteries and other fields.
Smart Images

Figure 220217084011 
Figure 220217084014 
Figure 220217084017
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium iron phosphate material preparation, and in particular to a lithium iron phosphate-graphene strong coupling material and a preparation method thereof. Background Art
[0002] Lithium iron phosphate cathode material is considered to be one of the most promising cathode materials for lithium-ion batteries due to its high specific capacity, high safety, good thermal stability and long cycle life, and has attracted much attention from battery manufacturers. However, this cathode material has its inherent limitations - low conductivity and low Li + Problems such as diffusion rate restrict its application.
[0003] Carbon-coated lithium battery cathode materials are an effective method to improve their electrochemical performance. Graphitized carbon materials have high electrical conductivity and can improve the conductivity of cathode materials to a certain extent. In recent years, graphene has been often used for the modification of lithium iron phosphate due to its ultra-high electrical conductivity. In conventional strategies, graphene is used as a coating material and a load material for lithium iron phosphate modification. For example, Chinese invention patent CN201410735954.7 discloses a method for preparing an interface strongly coupled graphene-lithium iron phosphate nanocomposite cathode material, in which polymer-modified lithium iron phosphate nanoparticles are deposited on the graphene surface; CN201210005494.3 discloses a method for preparing a graphene-coated olivine-type lithium iron phosphate composite material, in which lithium iron phosphate is grown in situ on the graphene surface. However, due to the poor water dispersibility of graphene itself, a large amount of organic solvents such as NMP, DMF or surfactants are usually required, while graphene oxide needs to be further reduced, which increases the process flow and also faces environmental pollution pressure, which is not conducive to large-scale production. In addition, there are also literature reports that when lithium ions pass through defect-free graphite sheets, their diffusion rate is limited, which may reduce the electrochemical performance of the positive electrode material.
[0004] In summary, in order to further expand the industrial application of lithium iron phosphate-graphene materials, it is necessary to improve the composite method of lithium iron phosphate and graphene. Summary of the invention
[0005] The technical problem to be solved by the present invention is to develop an environmentally friendly and efficient graphene embedded lithium iron phosphate-graphene strong coupling material and a preparation method thereof. Specifically, the present invention relates to a method of using phosphorylated small graphene as a nucleating agent, reacting with an iron source, a lithium source, and a phosphorus source under high temperature solvent thermal conditions, without the need to use additional organic solvents and surfactants to disperse graphene, so as to achieve efficient and environmentally friendly preparation of lithium iron phosphate-graphene strong coupling materials.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A lithium iron phosphate-graphene strong coupling material and a preparation method thereof, wherein phosphorylated small graphene is used as a nucleating agent to react with an iron source, a lithium source, and a phosphorus source, and the lithium iron phosphate-graphene strong coupling material is prepared efficiently and environmentally friendly under high-temperature solvent thermal conditions, and the specific steps are as follows:
[0008] (1) mixing the phosphorylated small graphene with an iron source solution and stirring to form a solution A;
[0009] (2) adding lithium source solution B to solution A and mixing and stirring to form solution C;
[0010] (3) Add the phosphorus source to solution C and mix and stir to form a lithium iron phosphate precursor D, place D in a high-pressure reactor for heating reaction for a period of time, and then naturally cool to room temperature. Filter, wash and dry the precipitate to obtain a lithium iron phosphate-graphene strong coupling material.
[0011] The phosphorylated small graphene is prepared with reference to Chinese invention patent CN201910558401.1. The preparation method is as follows: using graphite as raw material and red phosphorus as auxiliary material, high-energy ball milling and concentrated nitric acid are used to efficiently and environmentally prepare graphene materials. The specific steps are as follows:
[0012] (1) mixing red phosphorus and graphite, and performing high-energy ball milling on the mixed powder using a high-energy ball mill;
[0013] (2) adding water to the ball-milled powder and heating and stirring to 50-80° C., and then adding concentrated nitric acid to react;
[0014] (3) After the reaction is completed, the solution containing the powder is centrifuged and then dispersed and washed with water to obtain the graphene material.
[0015] The graphite is graphite ore or graphite powder, with a particle size of less than 1 cm; the red phosphorus is powder or particles, with a particle size of less than 1 cm; and the mixing ratio of the red phosphorus to the graphite is 0.5-10.
[0016] The ball milling speed of the high-energy ball mill is 1000r / min-1600r / min, the time of the high-energy ball milling is 1-10h, and the mass volume ratio of the powder after ball milling to water is 0.01g / ml-0.1g / ml.
[0017] The volume ratio of the concentrated nitric acid to the aqueous solution containing the powder is 0.25-1, the concentration of the concentrated nitric acid is 65%-95%, and the reaction time is 5-30 minutes; the rotation speed of the centrifuge is 8000-15000 r / min, and the centrifugation time is 5-15 minutes.
[0018] The iron source solution is a ferrous salt water / ethylene glycol solution, such as ferrous sulfate and its hydrated salt, ferrous oxalate, ferrous chloride, etc., and the volume ratio of water to ethylene glycol is 0.25-0.5.
[0019] The weight ratio of the phosphorylated small graphene to the iron in the iron source is 0.001-0.2, the phosphorylated small graphene and the iron source solution are mixed and stirred at a speed of 100-1000 rpm, and the stirring time is 10-60s.
[0020] The lithium source solution B is a water-soluble lithium salt solution such as LiOH, LiCl, CH3COOLi, etc. The stirring speed of the lithium source solution and solution A is 1000-2000 rpm, and the stirring time is 10-60s.
[0021] The phosphorus source is a phosphoric acid aqueous solution, and the phosphorus source and solution C are mixed and stirred at a speed of 100-1000 rpm for a stirring time of 10-30 seconds.
[0022] The Fe in the iron source, lithium source and phosphorus source 2+ :Li + :PO4 3- The molar ratio is 1:1:1~1:3.5:1.5.
[0023] The reaction temperature is 120-220°C and the reaction time is 1-12h.
[0024] The present invention uses phosphated graphene as a nucleating agent. When an iron source is added, due to charge attraction, ferrous ions are firstly adsorbed and coordinated by phosphate groups [C-(P=O)(OH)2] on the edge of the phosphated small graphene to form nucleation sites. Then, when a lithium source is added, phosphated small graphene-iron lithium seed crystals are generated. Under high-temperature solvent thermal conditions, the seeds further react with the iron source, the lithium source and the phosphorus source to promote the growth of lithium iron phosphate nanocrystals to generate a shuttle-shaped structure. Since the edges of the phosphated small graphene are covered with strong phosphate groups, the CP bonds therein are strong and will not break, and the graphene is small in thickness and size, it is easy to embed the graphene into the lithium iron phosphate nanocrystals to finally form a lithium iron phosphate-graphene strong coupling material. The strong coupling effect can be characterized by micro-Raman spectroscopy, which is manifested in that the characteristic peak of lithium iron phosphate is significantly enhanced with the embedding of the phosphated graphene, while the conventional carbon material coating will weaken the characteristic peak of lithium iron phosphate.
[0025] Beneficial effects:
[0026] Compared with the prior art, the technical method of the present invention is novel and unique, efficient and environmentally friendly, and there is no need to use organic solvents and surfactants to disperse graphene, which greatly reduces the pollution caused in the preparation process. Only by using the coordination of phosphorylated small graphene and ferrous ions to manufacture nucleation sites, and then reacting with a lithium source to form phosphorylated small graphene-iron lithium seeds, graphene can be embedded in lithium iron phosphate nanocrystals, and due to the presence of CP bonds in the graphene-lithium iron phosphate structure, this embedded structure is different from the common inclusion adsorption structure, so there is a strong coupling effect between graphene and lithium iron phosphate, and at the same time, this embedding can also cause a certain lattice distortion, so that the internal conductivity of lithium iron phosphate is improved, which is completely different from the conventional graphene coating or loading lithium iron phosphate composite structure to improve the external conductivity. At the same time, the introduction of phosphorylated small graphene can also regulate the lithium iron phosphate morphology structure, which helps to improve the crystallinity of lithium iron phosphate. This has important practical significance for the industrial application of lithium iron phosphate-graphene materials.
[0027] The lithium iron phosphate-graphene strong coupling material according to the present invention has no limitation on its application, and can be applied to currently known fields such as lithium ion batteries, optoelectronic devices, energy catalysis, biomedicine, etc. And according to its physical and chemical properties, those skilled in the art can easily think of applying it to other possible fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Electron scanning microscope photos of lithium iron phosphate nanocrystals prepared in Comparative Example 1 and Example 1.
[0029] Figure 2 This is the XRD spectrum of the lithium iron phosphate-graphene strong coupling material prepared in Example 1.
[0030] Figure 3 This is an electron scanning microscope photograph of the lithium iron phosphate-graphene strong coupling material prepared in Example 2.
[0031] Figure 4 The Raman spectra of the lithium iron phosphate-graphene strong coupling materials prepared in Example 1, Example 2, and Example 3 are shown, and the inset is the Raman spectra of the phosphorylated small graphene.
[0032] Figure 5 This is an electron scanning microscope photograph of the lithium iron phosphate-graphene strong coupling material prepared in Example 4.
[0033] Figure 6 This is the XRD spectrum of the lithium iron phosphate-graphene strong coupling material prepared in Example 5. DETAILED DESCRIPTION
[0034] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0035] The preparation method of the phosphorylated small graphene aqueous solution of the present invention is prepared by referring to the embodiment in ZL 2019 1 0558401.1. The following embodiments all adopt the phosphorylated small graphene prepared in Example 3 of the patent.
[0036] Example 1
[0037] 278 mg FeSO4•7H2O was dissolved in 1 mL deionized water and 4 mL ethylene glycol and 100 μg / mL phosphorylated small graphene aqueous solution were added and stirred at 100 rpm for 60 s to form solution A. 86 mg LiOH•H2O was dissolved in 1 mL deionized water to form solution B and added to solution A and stirred at 2000 rpm for 10 s to form solution C. 1 mmol phosphoric acid was added to solution C and stirred at 1000 rpm for 10 s to form solution D. Solution D was placed in a high-pressure reactor and reacted at 140 °C for 8 h. After natural cooling, it was filtered, washed, and dried to obtain lithium iron phosphate-graphene strong coupling material. The powder was grayish white. Due to the nucleation and regulation of phosphorylated small graphene, the growth direction of lithium iron phosphate nanocrystals was regulated, as shown in the attached Figure 1 The particles shown have a spindle-shaped structure, and the surface and background are clean, without small graphene or aggregates, indicating that the graphene has an embedded structure. Figure 2 XRD also shows that it has no impurities and good crystallinity. Figure 4 Raman spectroscopy confirmed the presence of graphene. By assembling button-type lithium batteries for testing, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g), the charge and discharge capacity increased by 10.2% at 0.1C and 5.3% at 1C.
[0038] For the assembly and performance testing methods of button-type lithium batteries, please refer to the literature: Hydrothermal preparation ofLiFePO4 nanocrystals mediated by organic acid, Journal of Power Sources 195(2010) 2877–2882, Jiangfeng Ni, Masanori Morishita, Yoshiteru Kawabe,Masaharu Watada b,Nobuhiko Takeichi, Tetsuo Sakai. The assembly and performance testing methods of button-type lithium batteries in the following embodiments are the same as those in this reference.
[0039] Example 2
[0040] 278 mg FeSO4•7H2O was dissolved in 1 mL deionized water, and 4 mL ethylene glycol and 100 uL of 500 μg / mL phosphorylated small graphene aqueous solution were added and stirred at 500 rpm for 30 s to form solution A. 100 mg LiOH•H2O was dissolved in 1 mL deionized water to form solution B, and added to solution A and stirred at 1000 rpm for 30 s to form solution C. 1 mmol phosphoric acid was added to solution C and stirred at 500 rpm for 20 s to form solution D. Solution D was placed in a high-pressure reactor and reacted at 160 ℃ for 4 h. After natural cooling, it was filtered, washed and dried to obtain lithium iron phosphate-graphene strong coupling material, and the powder was off-white. Figure 3 The obtained structure is shown to be a spindle-shaped structure with a particle length of about 2 um, which further confirms that the introduction of phosphorylated small graphene can regulate its morphology. Figure 4 The characteristic peak of lithium iron phosphate in Raman spectrum is significantly enhanced, indicating the strong coupling between lithium iron phosphate and phosphated graphene. Through the test of assembled button lithium battery, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70mAh / g), the charge and discharge capacity at 0.1C increased by 12.3% and at 1C increased by 7.1%.
[0041] Example 3
[0042] 278 mg FeSO4•7H2O was dissolved in 1 mL deionized water, and 4 mL ethylene glycol and 100 uL 1 mg / mL phosphorylated small graphene aqueous solution were added and stirred at 500 rpm for 30 s to form solution A. 86 mg LiOH•H2O was dissolved in 1 mL deionized water to form solution B, and added to solution A and stirred at 1500 rpm for 20 s to form solution C. 1 mmol phosphoric acid was added to solution C and stirred at 1000 rpm for 20 s to form solution D. Solution D was placed in a high-pressure reactor and reacted at 160 ℃ for 6 h. After natural cooling, it was filtered, washed and dried to obtain lithium iron phosphate-graphene strong coupling material, and the powder was gray. Figure 4 Raman spectroscopy further shows that the characteristic peak of lithium iron phosphate is significantly enhanced, and compared with Examples 1 and 2, the Raman signal of phosphorylated small graphene increases with the increase in the amount of addition. At the same time, the characteristic peak of lithium iron phosphate is more obviously enhanced, further confirming the strong coupling between lithium iron phosphate and graphene. By assembling button lithium battery tests, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g), the charge and discharge capacity at 0.1C increased by 13.3%, and at 1C increased by 7.6%.
[0043] Example 4
[0044] 278 mg FeSO4•7H2O was dissolved in 1 mL deionized water, and 4 mL ethylene glycol and 100 uL of 5 mg / mL phosphorylated small graphene aqueous solution were added and stirred at 800 rpm for 40 s to form solution A. 86 mg LiOH•H2O was dissolved in 1 mL deionized water to form solution B, which was added to solution A and stirred at 2000 rpm for 10 s to form solution C. 1 mmol phosphoric acid was added to solution C and stirred at 800 rpm for 10 s to form solution D. Solution D was placed in a high-pressure reactor and reacted at 180 ℃ for 4 h. After natural cooling, it was filtered, washed and dried to obtain lithium iron phosphate-graphene strong coupling material, and the powder was dark gray. Figure 5 The particle length is about 1 um, which is significantly smaller than that in Example 2, due to the increase in the amount of added phosphated graphene, which leads to an increase in the number of nucleation seeds. The button-type lithium battery test shows that the charge and discharge capacity at 0.1C is increased by 13.1% and at 1C is increased by 6.9% compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g).
[0045] Example 5
[0046] 278 mg FeSO4•7H2O was dissolved in 1 mL deionized water, and 4 mL ethylene glycol and 500 uL of 20 mg / mL phosphorylated small graphene aqueous solution were added and stirred at 600 rpm for 30 s to form solution A. 129 mg LiOH•H2O was dissolved in 1 mL deionized water to form solution B, and added to solution A and stirred at 1200 rpm for 30 s to form solution C. 0.8 mmol phosphoric acid was added to solution C and stirred at 200 rpm for 50 s to form solution D. Solution D was placed in a high-pressure reactor and reacted at 220 ℃ for 1 h. After natural cooling, it was filtered, washed and dried to obtain lithium iron phosphate-graphene strong coupling material, and the powder was gray-black. Figure 6 XRD spectrum shows that under this condition, the prepared material has no impurities and good crystallization. Through the test of assembled button lithium battery, compared with pure lithium iron phosphate, the charge and discharge capacity at 0.1C increased by 11.3% and at 1C increased by 6.2%.
[0047] Example 6
[0048] 278 mg FeSO4•7H2O was dissolved in 1 mL deionized water and 2 mL ethylene glycol and 500 uL 10 mg / mL phosphorylated small graphene aqueous solution were added and stirred at 600 rpm for 30 s to form solution A. 43 mg LiOH•H2O was dissolved in 1 mL deionized water to form solution B and added to solution A and stirred at 1600 rpm for 40 s to form solution C. 0.8 mmol phosphoric acid was added to solution C and stirred at 200 rpm for 30 s to form solution D. Solution D was placed in a high-pressure reactor and reacted at 200 °C for 2 h. After natural cooling, it was filtered, washed, and dried to obtain lithium iron phosphate-graphene strong coupling material, and the powder was gray-black. By assembling button lithium battery tests, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g), the charge and discharge capacity at 0.1C increased by 14.5%, and at 1C increased by 7.6%.
[0049] Example 7
[0050] 198.7 mg FeCl2•4H2O was dissolved in 1 mL deionized water and 3 mL ethylene glycol and 100 uL 5 mg / mL phosphorylated small graphene aqueous solution were added and stirred at 800 rpm for 40 s to form solution A. 129 mg LiOH•H2O was dissolved in 1 mL deionized water to form solution B and added to solution A and stirred at 2000 rpm for 10 s to form solution C. 1 mmol phosphoric acid was added to solution C and stirred at 800 rpm for 10 s to form solution D. Solution D was placed in a high-pressure reactor and reacted at 120 ° C for 12 h. After natural cooling, it was filtered, washed, and dried to obtain lithium iron phosphate-graphene strong coupling material, and the powder was gray. By assembling button lithium batteries for testing, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g), the charge and discharge capacity at 0.1C increased by 8.5%, and at 1C increased by 3.6%.
[0051] Example 8
[0052] The steps of this embodiment are the same as those of Example 1, except that the stirring speed during the formation of solution A is changed to 500 rpm. This embodiment can also obtain a lithium iron phosphate-graphene strong coupling material, and the powder is grayish white. By assembling button-type lithium batteries for testing, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g), the charge and discharge capacity at 0.1C is increased by 10.5%, and at 1C it is increased by 5.2%.
[0053] Example 9
[0054] The steps of this embodiment are the same as those of Example 1, except that the stirring speed during the formation of solution A is changed to 1000 rpm. This embodiment can also obtain a lithium iron phosphate-graphene strong coupling material, and the powder is grayish white. By assembling button-type lithium batteries for testing, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g), the charge and discharge capacity at 0.1C is increased by 9.8%, and at 1C it is increased by 4.7%.
[0055] Example 10
[0056] The steps of this embodiment are the same as those of embodiment 1, except that the stirring time of the mixed solution A is changed to 30s. This embodiment can also obtain a lithium iron phosphate-graphene strong coupling material, and the powder is grayish white. By assembling button-type lithium batteries for testing, compared with pure lithium iron phosphate, the charge and discharge capacity at 0.1C is increased by 9.9%, and at 1C is increased by 5.2%.
[0057] Embodiment 11
[0058] The steps of this embodiment are the same as those of embodiment 1, except that the amount of LiOH•H2O added is changed to 43 mg. This embodiment can also obtain a lithium iron phosphate-graphene strong coupling material, and the powder is grayish white. By assembling button-type lithium batteries for testing, compared with pure lithium iron phosphate, the charge and discharge capacity at 0.1C is increased by 8.6%, and at 1C is increased by 4.2%.
[0059] Example 13
[0060] The steps of this embodiment are the same as those of embodiment 1, except that the amount of LiOH•H2O added is changed to 129 mg. This embodiment can also obtain a lithium iron phosphate-graphene strong coupling material, and the powder is grayish white. By assembling button-type lithium batteries for testing, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g), the charge and discharge capacity at 0.1C is increased by 10.7%, and at 1C it is increased by 5.5%.
[0061] Embodiment 14
[0062] The steps of this embodiment are the same as those of embodiment 1, except that the concentration of phosphorylated graphene is changed to 500 ug / mL. This embodiment can also obtain lithium iron phosphate-graphene strong coupling material, and the powder is grayish white. By assembling button lithium batteries for testing, compared with pure lithium iron phosphate, the charge and discharge capacity at 0.1C is increased by 12.7%, and at 1C is increased by 6.7%.
[0063] Embodiment 15
[0064] The steps of this embodiment are the same as those of Example 1, except that the concentration of phosphorylated graphene is changed to 5 mg / mL. This embodiment can also obtain a lithium iron phosphate-graphene strong coupling material, and the powder is gray. By assembling button-type lithium batteries for testing, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g), the charge and discharge capacity at 0.1C is increased by 13.7%, and at 1C it is increased by 7.5%.
[0065] Example 16
[0066] The steps of this embodiment are the same as those of Example 1, except that the reaction temperature is changed to 120°C. This embodiment can also obtain a lithium iron phosphate-graphene strong coupling material, and the powder is grayish white. By assembling button-type lithium batteries for testing, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g), the charge and discharge capacity at 0.1C is increased by 8.3%, and at 1C it is increased by 3.7%.
[0067] Embodiment 17
[0068] The steps of this embodiment are the same as those of Example 1, except that the reaction temperature is changed to 180 °C. This embodiment can also obtain a lithium iron phosphate-graphene strong coupling material, and the powder is grayish white. By assembling button-type lithium batteries for testing, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g), the charge and discharge capacity at 0.1C is increased by 12.5%, and at 1C it is increased by 6.6%.
[0069] Embodiment 18
[0070] The steps of this embodiment are the same as those of Example 1, except that the amount of phosphoric acid added is changed to 0.8 mmol. This embodiment can also obtain a lithium iron phosphate-graphene strong coupling material, and the powder is grayish white. By assembling button-type lithium batteries for testing, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g), the charge and discharge capacity at 0.1C is increased by 9.4%, and at 1C it is increased by 4.6%.
[0071] Embodiment 19
[0072] The steps of this embodiment are the same as those of embodiment 1, except that the stirring speed is changed to 1000 rpm when B is added to A. This embodiment can also obtain a lithium iron phosphate-graphene strong coupling material, and the powder is grayish white. By assembling button lithium batteries for testing, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g), the charge and discharge capacity at 0.1C is increased by 9.9%, and at 1C it is increased by 4.8%.
[0073] Embodiment 20
[0074] The steps of this embodiment are the same as those of embodiment 1, except that the stirring time when adding B to A is changed to 60s. This embodiment can also obtain a lithium iron phosphate-graphene strong coupling material, and the powder is grayish white. By assembling button lithium batteries for testing, compared with pure lithium iron phosphate (pure lithium iron phosphate 0.1C 90 mAh / g, 1C 70 mAh / g), the charge and discharge capacity at 0.1C is increased by 10.1%, and at 1C it is increased by 5.0%.
[0075] Comparative Example 1
[0076] 278 mg FeSO4•7H2O was dissolved in 1 mL deionized water and 4 mL ethylene glycol was added and mixed evenly to form solution A. 86 mg LiOH•H2O was dissolved in 1 mL deionized water to form solution B and added to solution A and stirred at 2000 rpm for 10 s to form solution C. 1 mmol phosphoric acid was added to solution C and stirred at 1000 rpm for 10 s to form solution D. Solution D was placed in a high-pressure reactor and reacted at 140 ℃ for 8 h. After natural cooling, it was filtered, washed and dried to obtain lithium iron phosphate powder, which was off-white.
[0077] Comparative Example 2
[0078] 278 mg FeSO4•7H2O was dissolved in 1 mL deionized water, and 4 mL ethylene glycol and 10 mg pure graphene powder with a size of about 50 nm were added and stirred at 600 rpm for 30 s to form solution A. 129 mg LiOH•H2O was dissolved in 1 mL deionized water to form solution B, and added to solution A and stirred at 1200 rpm for 30 s to form solution C. 0.8 mmol phosphoric acid was added to solution C and stirred at 200 rpm for 50 s to form solution D. Solution D was placed in a high-pressure reactor and reacted at 220 ℃ for 1 h. After natural cooling, graphene floated on the surface of the product. During the washing process, due to the hydrophobic effect of graphene, graphene and lithium iron phosphate were completely separated, and lithium iron phosphate-graphene composite materials could not be effectively formed.
Claims
1. A method for preparing a lithium iron phosphate-graphene strong coupling material, characterized in that: The steps are as follows: (1) mixing the phosphorylated small graphene with an iron source solution and stirring to form a solution A, wherein the weight ratio of the phosphorylated small graphene to the iron in the iron source is 0.001, the phosphorylated small graphene and the iron source solution are mixed and stirred at a speed of 100-1000 rpm, and the stirring time is 10-60 s; (2) adding lithium source solution B to solution A and mixing to form solution C; (3) adding a phosphorus source to solution C and mixing to form a lithium iron phosphate precursor D, placing D in a high-pressure reactor for heating and reacting for a period of time, and then naturally cooling to room temperature, filtering, washing, and drying the precipitate to obtain a lithium iron phosphate-graphene strong coupling material, wherein the reaction temperature is 120-220° C., and the reaction time is 1-12 h; The method for preparing phosphorylated small graphene is as follows: using graphite as raw material and red phosphorus as auxiliary material, high-energy ball milling and concentrated nitric acid are used to efficiently and environmentally prepare graphene materials. The specific steps are as follows: (a) mixing red phosphorus and graphite, and performing high-energy ball milling on the mixed powder using a high-energy ball mill; (b) adding water to the ball-milled powder and heating with stirring to 50-80° C., followed by adding concentrated nitric acid to react; (c) After the reaction is completed, the solution containing the powder is centrifuged and then dispersed and washed with water to obtain the graphene material; The graphite is graphite ore or graphite powder with a particle size of less than 1 cm; the red phosphorus is powder or granules with a particle size of less than 1 cm; the mixing ratio of the red phosphorus to the graphite is 0.5-10; The high-energy ball milling speed is 1000 r / min-1600 r / min, the high-energy ball milling time is 1-10 hours, and the mass volume ratio of the ball-milled powder to water is 0.01 g / ml-0.1 g / ml; The volume ratio of the concentrated nitric acid to the aqueous solution containing the powder is 0.25-1, the concentration of the concentrated nitric acid is 65%-95%, and the reaction time is 5-30 minutes; the centrifugal speed is 8000-15000 r / min, and the centrifugal time is 5-15 minutes.
2. The method according to claim 1, characterized in that The iron source solution is a water / ethylene glycol solution of ferrous salt; The ferrous salt is ferrous sulfate and its hydrated salt, ferrous oxalate, or ferrous chloride; The volume ratio of water to ethylene glycol is 0.25~0.
5.
3. The method according to claim 1, characterized in that The lithium source solution B is a water-soluble lithium salt solution of LiOH, LiCl, and CH3COOLi. The stirring speed of the lithium source solution and solution A is 1000-2000 rpm, and the stirring time is 10-60s.
4. The method according to claim 1, wherein The phosphorus source is a phosphoric acid aqueous solution, and the phosphorus source and solution C are mixed and stirred at a speed of 100-1000 rpm for 10-30 seconds.
5. The method according to claim 1, wherein The Fe in the iron source, lithium source and phosphorus source 2+ :Li + :PO4 3- The molar ratio is 1:1:1~1:3.5:1.
5.
6. A lithium iron phosphate-graphene strong coupling material, characterized in that: It is prepared by the method according to any one of claims 1 to 5.
Citation Information
Patent Citations
Method for preparing graphene-coated olivine type lithium ferric phosphate composite material
CN102544489A
Method for synthesizing graphene-doped nanometer manganese-rich lithium iron phosphate under conditions of normal pressure and water phase
CN103956464A
Preparation method of interface strong coupling graphene-lithium iron phosphate nano-composite positive electrode material
CN104393265A
Synthesis method of lithium iron phosphate of graphene in-situ nucleation
CN105826524A
Nanosheet piled lithium iron phosphate / graphene composite material and preparation method thereof
CN106410168A