Heat aging resistant and flexible polyolefin formulations

By preparing a polyolefin formulation of a specific composition and its thermal aging treatment, the problems of difficulty in recycling the power cable coating after cross-linking and insufficient resistance to thermal aging are solved, and a polyolefin with high flexibility and high thermal aging resistance is achieved. Materials suitable for a variety of industrial applications.

CN114585678BActive Publication Date: 2024-10-11DOW GLOBAL TECHNOLOGIES LLC +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080074439.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-18
Filing Date
2020-11-10
Publication Date
2024-10-11
Estimated Expiration
2040-11-10

AI Technical Summary

Technical Problem

Existing polyethylene polymer coatings used for medium-voltage, high-voltage or ultra-high-voltage power cables are difficult to recycle after cross-linking, and have insufficient resistance to thermal aging, affecting their flexibility and service life.

Method used

Provided is a polyolefin formulation comprising specific proportions of polypropylene homopolymer, poly(ethylene-co-1-olefin) copolymer, ethylene/propylene diblock copolymer, saturated and aromatic hydrocarbons, and antioxidants , through melt mixing and thermal aging treatment, its flexibility and resistance to thermal aging are improved, and cross-linking is not required for easy recycling.

Benefits of technology

The polyolefin formulation and its heat-aged products have improved flexibility and resistance to heat aging, a flexural modulus of less than 300MPa, an elongation at break of 550% or higher, increased tensile strength, and are recyclable and suitable for power cables and other industrial applications such as aerospace, automotive and medical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003611737360000171
    Figure BDA0003611737360000171
Patent Text Reader

Abstract

A polyolefin formulation comprising the following amounts of components (A) to (E): 15.0 wt% to 55.0 wt% (wt%) of (A) a polypropylene homopolymer; 77.9 wt% to 30.0 wt% of (B) a poly(ethylene-co-1-olefin) copolymer; 3.0 wt% to 6.5 wt% of (C) an ethylene / propylene diblock copolymer; 4.0 wt% to 8.0 wt% of (D) a saturated and aromatic (C 14 ‑C 60 ) hydrocarbon; and 0.1 wt % to 1.5 wt % of (E) an antioxidant; wherein the wt % of (B) divided by the wt % of (A) is in a mass ratio of 5.0:1.0 to 0.50:1.0; and wherein the total amount of components (A), (B) and (C) is 88.0 wt % to 95.9 wt % of the polyolefin formulation; and wherein the total amount of components (A) to (E) is 92.1 wt % to 100.0 wt % of the polyolefin formulation.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Polyolefins, formulations, and related methods and articles of manufacture. Background Art

[0002] Patent and patent application publications in or relating to this field include EP 0 617 077 A1; EP 0893801 A1; EP 0 893 802 A1; US ​​6,824,870 B2; US 6,861,143 B2; US 7,514,633 B2; US 8,378,216 B2; US8,716,400 B2; US 9,334,374 B2; US 9,404,005 B2; US 2019 / 0136026 A1; WO 00 / 041187 A1; WO 2002 / 047092 A1; WO 2007 / 048422 A1; WO 2008 / 058572 A1; WO 201I / 092533 A1; WO 2012 / 044732 A1; WO 2012 / 069864 A1; WO 2012 / 085612 A1; WO 2013 / 017916 A1; WO 2013 / 171550A1; WO 2016 / 158950 A1; and WO 2016 / 182817 A1.

[0003] Polyethylene polymers for coatings (e.g., insulating layers) of medium voltage (MV), high voltage (HV) or extra-high voltage (EHV) power cables are usually crosslinked by the decomposition of peroxide additives. The beginning of the crosslinking step requires passing the conductor of the uncrosslinked coating through a continuous vulcanization tube. After the resulting crosslinked coated conductor leaves the tube, it must be degassed to remove volatile crosslinked byproducts. The presence of crosslinking in crosslinked polyethylene polymers ("XLPE") makes the coating difficult to recycle. Summary of the invention

[0004] We provide a polyolefin formulation comprising the following amounts of components (A) to (E): 15.0 to 55.0 weight percent (wt%) of (A) a polypropylene homopolymer; 77.9 to 30.0 wt% of (B) a poly(ethylene-co-1-olefin) copolymer; 3.0 to 6.5 wt% of (C) an ethylene / propylene diblock copolymer; 4.0 to 8.0 wt% of (D) a saturated and aromatic (C 14 -C 60) hydrocarbon; and 0.1 wt % to 1.5 wt % of (E) an antioxidant; wherein the wt % of (B) divided by the wt % of (A) is in a mass ratio of 5.0:1.0 to 0.50:1.0; and wherein the total amount of components (A), (B) and (C) is 88.0 wt % to 95.9 wt % of the polyolefin formulation; and wherein the total amount of components (A) to (E) is 92.1 wt % to 100.0 wt % of the polyolefin formulation.

[0005] The polyolefin formulations have improved (increased) flexibility and improved (increased) resistance to the flexibility-reducing effects of heat aging (collectively referred to as the "original invention benefits"). The improved (increased) flexibility is indicated by a flexural modulus of less than 300 megapascals (MPa) and optionally a lower flexural modulus relative to that of a comparative formulation. The improved (increased) resistance to the effects of heat aging is indicated by the resulting heat-aged polyolefin product of the present invention having an elongation at break of 550 percent (%) or more and, optionally, having a higher retention of elongation at break after heat aging compared to a comparative heat-aged product. The improved (increased) resistance to the effects of heat aging may also be indicated by the resulting heat-aged polyolefin product having a higher tensile strength after heat aging relative to that of a comparative heat-aged product.

[0006] The polyolefin formulations and heat-aged polyolefin products prepared therefrom by heat aging can be used in industries that benefit from flexibility and resistance to heat aging, such as, for example, as a coating (e.g., insulation) for medium voltage (MV), high voltage (HV), or extra high voltage (EHV) power cables. Advantageously, the polyolefin formulations do not have to be crosslinked in order to be used as a coating (e.g., insulation) in such power cables, and thus the materials and coatings of the invention are advantageously recyclable. The polyolefin formulations and heat-aged polyolefin products can have additional benefits and can be used in other industrial applications such as aerospace, automotive, and medical applications. DETAILED DESCRIPTION

[0007] The following are additional aspects of the invention; for ease of reference, some are numbered below.

[0008] Aspect 1. A polyolefin formulation comprising the following amounts of components (A) to (E): 15.0 wt% to 55.0 wt% (wt%) of (A) a polypropylene homopolymer; 77.9 wt% to 30.0 wt% of (B) a poly(ethylene-co-1-olefin) copolymer; 3.0 wt% to 6.5 wt% of (C) an ethylene / propylene diblock copolymer; 4.0 wt% to 8.0 wt% of (D) a saturated and aromatic (C 14 -C 60) hydrocarbon; and 0.1 wt % to 1.5 wt % of (E) an antioxidant; wherein the wt % of (B) divided by the wt % of (A) is in a mass ratio of 5.0:1.0 to 0.50:1.0; and wherein the total amount of components (A), (B) and (C) is 88.0 wt % to 95.9 wt % of the polyolefin formulation; and wherein the total amount of components (A) to (E) is 92.1 wt % to 100.0 wt % of the polyolefin formulation.

[0009] Aspect 2. The polyolefin formulation according to aspect 1, wherein the polyolefin formulation has features (i) and (ii) and optionally feature (iii): (i) a flexural modulus of less than 300 megapascals (MPa, e.g., 15 MPa to 299 MPa) measured according to ASTM D790-15e2; and (ii) an elongation at break of greater than or equal to 550% (%, alternatively greater than 600%, e.g., 605% to 850%) measured according to ASTM D638-14; and optionally (iii) a tensile strength of greater than 8.5 MPa (i.e., >1233 pounds per square inch (psi)) (e.g., 8.51 MPa to 26.9 MPa) measured according to ASTM D638-14.

[0010] Aspect 3. A polyolefin formulation according to aspect 1 or 2, wherein subjecting the unaged polyolefin formulation to heat aging at 135 degrees Celsius (° C.) for 10 days produces a heat-aged polyolefin product having characteristic (i) and optionally characteristic (ii): (i) an elongation at break greater than 350% (%, such as 355% to 700%, alternatively greater than 450%, alternatively greater than 550%, such as 550% to 695%) measured according to ASTM D638-14; and optionally, (ii) a tensile strength greater than 8.5 MPa (e.g., 8.51 MPa to 26.9 MPa) measured according to ASTM D638-14.

[0011] Aspect 4. The polyolefin formulation according to any one of aspects 1 to 3, wherein the polyolefin formulation has 16.0 wt% to 54.0 wt% of (A) polypropylene homopolymer; 72.0 wt% to 35.4 wt% of (B) poly(ethylene-co-1-olefin) copolymer; 4.0 to 6.0 wt% of (C) ethylene / propylene diblock copolymer; 5.0 wt% to 7.0 wt% of (D) saturated and aromatic (C 14 -C 60) hydrocarbon; and 0.1 wt% to 1.0 wt% of (E) an antioxidant; wherein the wt% of (B) divided by the wt% of (A) is in a mass ratio of 4.5:1.0 to 0.60:1.0; and wherein the total amount of components (A), (B) and (C) is 88.0 wt% to 94.9 wt% of the polyolefin formulation; and wherein the total amount of components (A) to (E) is 93.0 wt% to 100.0 wt% of the polyolefin formulation.

[0012] Aspect 5. The polyolefin formulation according to any one of aspects 1 to 4, having any one of features (i) to (v): (i) the (A) polypropylene homopolymer has a molecular weight of 0.89 to 0.93 g / cm3 (g / cm 3 )(e.g., 0.90 g / cm 3 Up to 0.92g / cm 3 ) and a melt flow rate (MFR2) of 1.0 to 10 g / 10 min (e.g., 1.5 to 4.0 g / 10 min) as measured at 230° C., 2.16 kg in accordance with ASTM D-1238; (ii) wherein the (B) poly(ethylene-co-1-olefin) copolymer is a copolymer having a density of 0.850 g / cm2 as measured in accordance with ASTM D792-13 Method B. 3 Up to 0.890g / cm 3 (For example, 0.865 g / cm 3 Up to 0.874g / cm 3 ) and a melt index (I2) of 0.1 g / 10 min to 5.0 g / 10 min as measured at 190° C., 2.16 kg according to ASTM D-1238 (e.g., a poly(ethylene-co-1-butene) copolymer of a melt index of 0.1 g / 10 min to 0.5 g / 10 min (e.g., and optionally, an olefin content of at least 85.0 wt % based on the total weight of (B)); (iii) wherein the (C) ethylene / propylene diblock copolymer has a melt flow rate (MFR2) of 4 g / 10 min to 8 g / 10 min as measured at 260° C., 2.16 kg according to ASTM D-1238; (iv) wherein the (D) saturated and aromatic (C 14 -C 60 ) hydrocarbons are saturated and aromatic (C 19 -C 23 ) hydrocarbons, alternatively saturated and aromatic (C 21) hydrocarbon, alternatively unsubstituted dibenzyltoluene; (v) wherein the antioxidant is a compound containing a sulfur atom. In some examples, the polyolefin formulation has a combination of any one of features (vi) to (xvii): (vi) (i) and (ii) both; (vii) (i) and (iii) both; (viii) (i) and (iv) both; (ix) (i) and (v) both; (x) (ii) and (iii) both; (xi) (ii) and (iv) both; (xii) (ii) and (v) both; (xiii) (iii) and (iv) both; (xiv) (iii) and (v) both; (xv) (iv) and (v) both; any four of (xvi) (i) to (v); each of (xvii) (i) to (v).

[0013] Aspect 6. A method for preparing a polyolefin formulation as described in any one of aspects 1 to 5, comprising melt mixing components (A), (B) and (C) at a temperature of 180 degrees Celsius to 220 degrees Celsius (°C) for a period of time effective for mixing to obtain a premix of components (A), (B) and (C) and excluding components (D) and (E); and soaking or absorbing components (D) and (E) into the premix at a temperature of 80°C to 100°C for an absorption effective period of time of at least 4 hours to obtain a polyolefin formulation containing components (A) to (E). The effective mixing period may be 0.1 hours to 2 hours, alternatively 0.2 hours to 1.0 hours, alternatively 0.1 hours to 0.5 hours. The atmosphere used in the melt mixing and / or soaking or absorbing step may be an inert atmosphere (e.g., a gas composed of nitrogen, argon, helium or a combination of any two or more thereof). The melt mixing step may be performed according to the melt mixing preparation method described later. The soaking or absorbing step may be performed according to the soaking or absorbing preparation method described later.

[0014] Aspect 7. A heat-aged polyolefin product, which is made by subjecting the polyolefin formulation described in any one of Aspects 1 to 5 to heat aging conditions including a temperature of 50 degrees Celsius to 140 degrees Celsius (°C) and a heat aging effective time period of 10 days or more and an air atmosphere. The heating time period can be continuous or intermittent. The subjecting step can be performed according to the heat aging method described later. An embodiment of the polyolefin formulation described in any one of Aspects 1 to 5 can be prepared by the method described in Aspect 6. The method described in Aspect 6 makes the polyolefin formulation an "unaged" polyolefin formulation, which means a polyolefin formulation that has not been subjected to heat aging under the conditions described in Aspect 7. The difference between the method described in Aspect 6 and the heat aging conditions described in Aspect 7 is that the method described in Aspect 6 is completed in a time period much shorter than the heat aging effective time period and the method described in Aspect 6 can be carried out under an inert atmosphere, while heat aging can be carried out under an air atmosphere.

[0015] Aspect 8. An article of manufacture comprising or made from the polyolefin formulation of any one of aspects 1 to 5 or the heat-aged polyolefin product of aspect 7.

[0016] Aspect 9. A coated conductor comprising a conductive core and an insulating layer, the insulating layer comprising the polyolefin formulation of any one of aspects 1 to 5 or the heat-aged polyolefin product of aspect 7 at least partially covering the conductive core.

[0017] Aspect 10. A method of conducting electricity, the method comprising applying a voltage across a conductive core of the coated conductor according to aspect 9 to generate an electric current through the conductive core.

[0018] Aspect 11. A method for recovering a polyolefin preparation as described in any one of Aspects 1 to 5 or contained in the manufactured article as described in Aspect 8 or contained in the insulation layer of the coated conductor as described in Aspect 9, the method comprising crushing the polyolefin preparation to obtain a crushed product, and granulating the crushed product to obtain pellets of the recycled polyolefin preparation.

[0019] The polyolefin formulation has improved (increased) flexibility and improved (increased) resistance to the flexibility-reducing effects of heat aging (collectively referred to as the "original invention benefit"). The improved (increased) flexibility is indicated by a flexural modulus before heat aging of 15 MPa to 300 MPa, alternatively 15.5 MPa to 290 MPa, alternatively 120 MPa to 290 MPa, alternatively 131 MPa to 287 MPa, measured according to ASTM D790-15e2. The improved (increased) resistance to the effects of heat aging can be indicated by the resulting heat-aged polyolefin formulation having an elongation at break of at least 350%, alternatively at least 450%, alternatively at least 550%, alternatively at least 570%, measured according to ASTM D638-14. For example, embodiments of heat aged polyolefin formulations may have an elongation at break of 350% to 820%, alternatively 450% to 650%, alternatively 550% to 630%. Subsequent inventive examples of polyolefin formulations and comparative examples of comparative formulations will demonstrate that the initial inventive benefit is an unpredictable consequence of the selection of the composition of components (A) to (E) and their absolute and relative amounts.

[0020] Embodiments of polyolefin formulations may have additional benefits. For example, embodiments of polyolefin formulations may have a tensile strength greater than 8.5 MPa (i.e., greater than 1233 pounds per square inch (psi)), alternatively greater than 12.4 MPa, alternatively 12.5 MPa to 24.9 MPa, measured according to ASTM D638-14 before and / or after heat aging. Improved (increased) resistance to the effects of heat aging may also be indicated by the resulting heat-aged polyolefin product having a tensile strength greater than 8.5 MPa (e.g., 8.51 MPa to 26.9 MPa) after heat aging relative to a comparative heat-aged product.

[0021] We also provide six additional inventive embodiments identical to aspects 1 to 6 and four additional inventive embodiments identical to aspects 8 to 11 dependent on any of aspects 1 to 5, except that the polyolefin formulations of ten of the additional inventive embodiments have a flexural modulus of less than 400 MPa, alternatively 15 MPa to 399 MPa, alternatively 300.1 MPa to 399 MPa, measured according to ASTM D790-15e2. We also provide an additional inventive embodiment identical to aspect 7 and four additional inventive embodiments identical to aspects 8 to 11 dependent on aspect 7, except that subjecting the polyolefin formulation having a flexural modulus of less than 400 MPa to heat aging at 135°C for 10 days produces a heat-aged polyolefin product having a flexural modulus of less than 400 MPa, alternatively 15 MPa to 399 MPa, alternatively 300.1 MPa to 399 MPa, measured according to ASTM D790-15e2.

[0022] Polyolefin formulation. The polyolefin formulation comprises components (A) to (E) and is not subjected to heat aging conditions. The total amount of all components in the polyolefin formulation is 100.0 wt%. The properties of the polyolefin formulation can be compared with the same properties measured for a heat-aged polyolefin product prepared by heat aging the polyolefin formulation under heat aging conditions, the heat aging conditions being as described earlier in Aspect 7 or described later in the heat aging method.

[0023] In order to characterize the properties of the polyolefin formulation as an "unaged" polyolefin formulation, the polyolefin formulation is prepared into a substantially uniform mixture comprising the claimed amounts of components (A) to (E), for example by melt mixing or melt kneading as described herein, and once the polyolefin formulation is prepared, it is compression molded into a plaque specimen for testing. The specimen is stored in air at a temperature of 23° C. and a relative humidity of 50% until its properties can be measured.

[0024] The polyolefin formulation has an improved dispersion of components (A) to (E) relative to the dispersion of the comparative formulation having component (E) and only three of components (A) to (D). The improved dispersion can be determined by scanning electron microscopy (SEM) of slices of pellets of the formulation. As shown in SEM images (not shown) of IE1, CE1 and CE2 before and after heat aging, the polyolefin formulation of the present invention will show smaller domains of the discontinuous phase that are more uniformly dispersed in the continuous phase compared to the comparative formulation.

[0025] The polyolefin formulation may be as described in any of the numbered aspects or claims. Alternatively, the polyolefin formulation may be as described in any of the numbered aspects or claims, except that one of the features of the numbered aspects or claims is modified based on any of the inventive examples IE1 to IE4 described later. For example, the endpoints of the feature range in one of the numbered aspects or claims may be modified to the values ​​given in any of IE1 to IE4. Alternatively, the composition of the feature component in any of the numbered aspects or claims may be modified to the composition given in any of IE1 to IE4. Therefore, the examples of the present invention may serve as a clear basis for modification of the claims.

[0026] (A) polypropylene homopolymer. Component (A) is an organic macromolecule having a propylene monomer content of 100 wt % based on the weight of the polypropylene homopolymer. The (A) polypropylene homopolymer is different from components (B) to (E) in composition and function. Some embodiments of component (A) may have a melt flow rate (MFR) of 1.0 to 100.0 g / 10 min (g / 10 min) measured according to ASTM D-1238, 230° C., 2.16 kilograms (kg).

[0027] Examples of (A) are polypropylene homopolymers from Braskem, including the INSPIRE series of polypropylene homopolymers.

[0028] The polyolefin formulation may have 15.0 wt% to 55.0 wt%, alternatively 15.5 wt% to 54.4 wt%, alternatively 16.1 wt% to 54.0 wt% (e.g., 16.4 wt%, 35.1 wt%, 44.5 wt% or 53.9 wt%) of component (A). If the amount of component (A) in the polyolefin formulation exceeds 55 wt%, the polyolefin formulation may not have sufficient flexibility, i.e., the polyolefin formulation may have too high a flexural modulus, i.e., greater than 300 MPa. If the amount of component (A) in the polyolefin formulation is less than 15 wt%, the polyolefin formulation may not have sufficient tensile strength before and / or after heat aging, i.e., the polyolefin formulation may have a tensile strength of less than 8.5 MPa. If the amount of (A) in the polyolefin formulation is less than 15 wt%, the polyolefin formulation may deform (lose its shape, e.g., warp or sag) at high temperatures (e.g., 130° C. or higher).

[0029] (B) poly(ethylene-co-1-olefin) copolymer. Component (B) is an organic macromolecule having an ethylene monomer content of 99.0 wt% to 50.0 wt%, alternatively 99.0 wt% to 85.0 wt%, and a 1-olefin comonomer content of 1.0 wt% to 50.0 wt%, alternatively 1.0 wt% to 15.0 wt%, based on the weight of the poly(ethylene-co-1-olefin) copolymer. (B) poly(ethylene-co-1-olefin) copolymer differs from components (A) and (C) to (E) in composition and function. Some embodiments of component (B) may have a melt index (I2) of 0.1 g / 10 min to 50.0 g / 10 min measured according to ASTM D-1238 (190° C., 2.16 kg).

[0030] Examples of (B) are commercially available and include ENGAGE TM Series of polyolefin elastomers. ENGAGE TM The polymer is an ethylene / 1-butene or ethylene / 1-octene copolymer, which generally has the following properties: narrow to medium molecular weight distribution; I2 of <0.5 g / 10 min to 30 g / 10 min (190°C, 2.16 kg, ASTM D1238); 0.857 g / cm 3 Up to 0.910g / cm 3(ASTM D792, Method B); a glass transition temperature (Tg) of -61° to -35°C; a melting transition range (also known as the DSC melting peak (rate 10°C / min)) of 36° to 103°C; a Shore A hardness of 56 to 96 (ASTM D2240); and a flexural modulus of 3 MPa to 110 MPa (MPa, ASTM D790). SUITABLE ENGAGE TM An example of an ethylene / 1-octene copolymer is ENGAGE TM 8003, 8100, 8107, 8130, 8137, 8150, 8157, 8180, 8187, 8200, 8207, 8400, 8401, 8402, 8407, 8411, 8440, 8450, 8452, 8480, 8540 and 8842. SUITABLE ENGAGE TM An example of an ethylene / 1-butene copolymer is ENGAGE TM 7256, 7270, 7277, 7367, 7447, 7457 and 7467. DSC stands for differential scanning calorimetry.

[0031] The polyolefin formulation may have 77.9 wt% to 30.0 wt%, alternatively 34.5 wt% to 75.0 wt%, alternatively 35.0 wt% to 73.0 wt% (e.g., 72.6 wt%, 53.9 wt%, 44.5 wt%, or 35.1 wt%) of component (B). If the amount of component (B) in the polyolefin formulation exceeds 78 wt%, the polyolefin formulation may be too flexible, i.e., the polyolefin formulation may have a too low flexural modulus, i.e., less than 15 MPa. If the amount of component (B) in the polyolefin formulation is less than 35 wt%, the polyolefin formulation may not have sufficient tensile strength before and / or after heat aging, i.e., the polyolefin formulation may have a tensile strength of less than 8.5 MPa. If the amount of (B) in the polyolefin formulation is less than 35 wt%, the polyolefin formulation may have too high a flexural modulus (i.e., the polyolefin formulation may be too stiff) and / or the polyolefin formulation after heat aging may have too low an elongation at break (i.e., the polyolefin formulation may be too brittle).

[0032] (C) Ethylene / propylene diblock copolymer. Component (C) is an organic macromolecule having a first monovalent segment having an ethylene monomer content of 95 wt% to 100 wt% based on the weight of the first segment, and a second monovalent segment having a propylene comonomer content of 95 wt% to 100 wt% based on the weight of the second segment, wherein the first monovalent segment is covalently bonded to the second monovalent segment to form a diblock copolymer. (C) Ethylene / propylene diblock copolymer is different from components (A), (B), (D) and (E) in composition and function. Some embodiments of component (C) can have a melt flow rate (MFR) of 1.0 g / 10 min to 50 g / 10 min, alternatively 3 g / 10 min to 20 g / 10 min, alternatively 4.0 g / 10 min to 10.0 g / 10 min, alternatively 5 g / 10 min to 8 g / 10 min (e.g., 6.5 g / 10 min), measured according to ASTM D-1238, 230° C., 2.16 kg.

[0033] (C) An example of an ethylene / propylene diblock copolymer is the block composite described in U.S. Pat. No. 8,716,400 B2. INTUNE from The Dow Chemical Company TM Ethylene / propylene diblock copolymers of the series of olefin block copolymers are also examples of such (C).

[0034] The polyolefin formulation may have 3.0 wt% to 6.5 wt%, alternatively 3.5 wt% to 5.9 wt%, alternatively 4.2 wt% to 5.2 wt% (e.g., 4.7 wt%) of component (C). If the amount of component (C) in the polyolefin formulation exceeds 6.5 wt%, the polyolefin formulation may not have sufficient elongation at break before and / or after heat aging, i.e., the polyolefin formulation may have too low elongation at break, i.e., less than 550% before heat aging and / or less than 350% after heat aging. If the amount of component (C) in the polyolefin formulation is less than 3.0 wt%, the polyolefin formulation may not have sufficient flexibility, i.e., the polyolefin formulation may have too high a flexural modulus, i.e., greater than 300 MPa.

[0035] (D) saturated and aromatic (C 14 -C 60 ) hydrocarbons. Saturated and aromatic (C 14 -C 60 ) hydrocarbon is an organic compound consisting of 1 to 6 saturated carbon atoms and 1 to 4 aromatic groups independently selected from phenyl, naphthyl and biphenyl groups, and does not contain carbon-carbon double bonds and carbon-carbon triple bonds. (D) saturated and aromatic (C 14 -C 60) hydrocarbons differ in composition and function from components (A) to (C) and (E). Component (D) may be saturated and aromatic (C 31 -C 60 ) hydrocarbons, saturated and aromatic (C 20 -C 40 ) hydrocarbons, saturated and aromatic (C 14 -C 30 ) hydrocarbons or saturated and aromatic (C 16 -C 22 ) hydrocarbons. Component (D) may be saturated and aromatic (C 19 -C 23 ) hydrocarbons, alternatively saturated and aromatic (C 21 ) hydrocarbon, alternatively unsubstituted dibenzyltoluene. Component (D) may be composed of one or more compounds of formula (I): CH 4-x (R 1 )(R 2 )(R 3 ) x (I), wherein the subscript x is an integer of 3 or 4; CH 4-x It is a multivalent free radical of benzene, where the valence is equal to the sum of x+2; R 1 is a (C1-C3)alkyl group; and R 2 and R 3 Independently (C7-C 10 ) aralkyl group. Component (D) may be benzyltoluene, dibenzyltoluene, tribenzyltoluene or a combination of any two or more thereof. Component (D) may be dibenzyltoluene; alternatively dibenzyltoluene selected from 1,2-dibenzyl-3-methylbenzene, 1,3-dibenzyl-4-methylbenzene and 1,4-dibenzyl-5-methylbenzene; alternatively dibenzyltoluene selected from 1,2-dibenzyl-3-methylbenzene and 1,3-dibenzyl-5-methylbenzene. Component (D) may be 1,2-dibenzyl-3-methylbenzene.

[0036] The polyolefin formulation may have 4.0 wt% to 8.0 wt%, alternatively 4.5 wt% to 7.4 wt%, alternatively 4.0 wt% to 6.4 wt%, alternatively 5.5 wt% to 6.9 wt%, alternatively 5.5 wt% to 6.4 wt%, alternatively 5.9 wt% to 6.1 wt% (e.g., 6.0 wt%) of component (D). If the amount of component (D) in the polyolefin formulation exceeds 8 wt%, the polyolefin formulation may ooze component (D), i.e., component (D) may exceed the amount that can remain dispersed in the polyolefin formulation, and excess (D) may migrate to the surface of the polyolefin formulation. If the amount of component (D) in the polyolefin formulation is less than 4 wt%, the polyolefin formulation may not have sufficient flexibility as indicated by the flexural modulus and / or resistance to heat aging as indicated by the elongation at break after heat aging.

[0037] (E) Antioxidant. Component (E) is an organic molecule that inhibits oxidation, or a collection of such molecules. The (E) antioxidant is different in composition and function from components (A) to (D). The function of the (E) antioxidant is to provide antioxidant properties to the polyolefin formulation and its heat-aged products. Examples of suitable (E) are bis(4-(1-methyl-1-phenylethyl)phenyl)amine (e.g., NAUGARD 445); 2,2′-methylene-bis(4-methyl-6-tert-butylphenol) (e.g., VANOX MBPC); 2,2′-thiobis(2-tert-butyl-5-methylphenol (CAS No. 90-66-4; 4,4′-thiobis(2-tert-butyl-5-methylphenol) (also known as 4,4′-thiobis(6-tert-butyl-m-cresol), CAS No. 96-69-5, commercially available as LOWINOX TBM-6); 2,2′-thiobis(6-tert-butyl-4-methylphenol (CAS No. 90-66-4, commercially available as LOWINOX TBP-6); tris[(4-tert-butyl-3-hydroxy-2,6-dimethylphenyl)methyl]-1,3,5-triazine-2,4,6-trione (e.g., CYANOX 1790); pentaerythritol tetrakis(3-(3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl)propionate (e.g., IRGANOX 1010, CAS No. 6683-19-8); 2,2′-dithiodiethylene 3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropionate (e.g., IRGANOX 1035, CAS No. 41484-35-9); distearyl thiodipropionate (“DSTDP”); dilauryl thiodipropionate (e.g., IRGANOX PS 800); stearyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (e.g., IRGANOX 1076); 2,4-bis(dodecylthiomethyl)-6-methylphenol (IRGANOX 1726); 4,6-bis(octylthiomethyl)-o-cresol (e.g., IRGANOX 1520); and 2′,3-bis[[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionyl]]propionohydrazide (IRGANOX 1024). (E) may be a compound containing a sulfur atom or a combination of any two or more thereof (i.e., an organic molecule containing a covalent C-S bond, for example, any one or more of the aforementioned compounds having "sulfo" in the name). (E) may be 4,6-bis(octylthiomethyl)-o-cresol (i.e., 4,6-bis(octylthiomethyl)-2-methylphenol or 4,6-bis(octylthiomethyl)-2-methylphenol). The combination of compounds containing a sulfur atom may be 4,6-bis(octylthiomethyl)-o-cresol and distearyl thiodipropionate.

[0038] The amount of (E) antioxidant may be 0.1 wt% to 1.0 wt%, alternatively 0.15 wt% to 0.5 wt%, alternatively 0.25 wt% to 0.34 wt% (e.g., 0.3 wt%) of the polyolefin formulation. If the amount of component (E) in the polyolefin formulation exceeds 1.0 wt%, the polyolefin formulation may not have sufficient flexibility as measured by flexural modulus. If the amount of component (E) in the polyolefin formulation is less than 0.1 wt%, the polyolefin formulation may not have sufficient resistance to heat aging.

[0039] Some embodiments of the polyolefin formulations may further comprise one or more optional additives. The optional additive may be component (F): a hindered amine stabilizer for stabilizing the polyolefin formulation against the effects of ultraviolet (UV) light. The component (F) hindered amine stabilizer differs in composition from components (A) to (E). Component (F) may be a hindered amine light stabilizer (HALS). Examples are hindered amine light stabilizers (HALS), benzophenones, or benzotriazoles. The (F) UV stabilizer may be a molecule containing a basic nitrogen atom bonded to at least one sterically bulky organic group and acting as an inhibitor of degradation or decomposition, or a collection of such molecules. A HALS is a compound having a sterically hindered amino functional group and inhibiting oxidative degradation. Examples of suitable (F) are dimethyl succinate, polymer with 4-hydroxy-2,2,6,6-tetramethyl-1-piperidin-ethanol (CAS No. 65447-77-0, commercially available as LOWILITE 62); and N,N′-bisformyl-N,N′-bis(2,2,6,6-tetramethyl-4-piperidinyl)-hexamethylenediamine (CAS No. 124172-53-8, commercially available as Uvinul 4050H). The formulations and products may be free of (F). When present, the (F) UV stabilizer may be 0.001 wt% to 1.5 wt%, alternatively 0.002 wt% to 1.0 wt%, alternatively 0.05 wt% to 0.1 wt% of the polyolefin formulation.

[0040] The polyolefin formulation may be free of certain additives. For example, the polyolefin formulation may be free of peroxides and / or fillers and / or alkenyl functional additives. Examples of such peroxides are those used for crosslinking polyolefins, such as those described in WO 2018 / 160402 A1, such as diisopropylbenzene peroxide. Examples of such fillers are carbon black, quartz, silica, talc, and titanium dioxide. Examples of such alkenyl functional additives are triallyl cyanurate (TAC); triallyl isocyanurate (TAIC); triallyl trimellitate ("TATM"); N,N,N',N',N",N"-hexaallyl-1,3,5-triazine-2,4,6-triamine ("HATATA"; also known as N 2 , N 2, N 4 , N 4 , N 6 , N 6 -hexaallyl-1,3,5-triazine-2,4,6-triamine); triallyl orthoformate; pentaerythritol triallyl ether; triallyl citrate; and triallyl aconitate.

[0041] Embodiments of the polyolefin formulation are not peroxide crosslinkable and / or are not crosslinked. The polyolefin formulation of such embodiments is thermoplastic and does not contain peroxide and does not contain olefin functional coagents. The thermoplastic polyolefin formulation can be used as a coating (e.g., insulation layer) in power cables and is recyclable.

[0042] Other embodiments of the polyolefin formulation further comprise an organic peroxide (e.g., dicumyl peroxide) and are thus peroxide crosslinkable. Such embodiments may further comprise an olefin functional coagent. In some embodiments, such peroxide crosslinkable polyolefin formulations are heated to prepare the crosslinked polyolefin products of the present invention.

[0043] Any compound, composition, formulation, mixture or product herein may be free of any one of the chemical elements selected from the group consisting of H, Li, Be, B, C, N, O, F, Na, Mg, Al, Si, P, S, Cl, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Se, Br, Rb, Sr, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, I, Cs, Ba, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Tl, Pb, Bi, lanthanides, and actinides; with the proviso that any desired chemical element (e.g., C and H required for polyolefins; or Hf required for M=Hf) is not excluded.

[0044] Alternatively, before different embodiments. ASTM means Standardization Organization, ASTM International, West Conshohocken, Pennsylvania, USA. Any comparative examples are for illustrative purposes only and should not be prior art. Containing or lacking means completely absent; alternatively undetectable. ISO is the International Organization for Standardization (Chemin de Blandonnet 8, CP 401-1214 Vernier, Geneva, Switzerland). IUPAC is the International Union of Pure and Applied Chemistry (IUPAC Secretariat, Research Triangle Park, North Carolina, USA). Optionality can be given, but not essential. Operability means functionally capable or effective. Optional (ground) means absence (or exclusion), alternatively presence (or inclusion). PAS is a Publicly Available Specification of the German Institute for Standardization (DIN). Properties can be measured using standard test methods and conditions. Ranges include endpoints, subranges, and integer and / or fractional values ​​contained therein, except for integer ranges that do not include fractional values. Room temperature: 23°C.±1°C.

[0045] Unless otherwise defined, the terms used herein have their IUPAC meanings. See, for example, the Compendium of Chemical Terminology. Gold Book, Version 2.3.3, February 24, 2014.

[0046] The flexural modulus, elongation at break, and tensile strength of the test material can be measured on compression molded plaque samples before and after the sample has been subjected to heat aging according to the Heat Aging Method. The results can be reported as the average of five measurements made on five compression molded plaque samples of the same test material.

[0047] Melt-mixing preparation method for preparing examples of polyolefin formulations of the present invention and examples of comparative formulations: Components (A), (B) and (C) were melt-mixed in a counter-rotating, intermeshing conical twin-screw extruder ("conical TSE") having twin screws each having a diameter of 32 millimeters (mm) and a length of 330.7 mm and a screw speed of 10 revolutions per minute (rpm) under a nitrogen atmosphere. The conical TSE had three consecutive zones, and the melt-mixing used a temperature profile of 180° C. in the first zone, 200° C. in the second zone, and 210° C. in the third zone, and a premix of components (A), (B) and (C) was given in the third zone without components (D) and (E). A stream of the premix from the third zone was extruded through a single-hole die into an underwater Berlyn pelletizer to produce a premix of components (A) to (C) as a uniform pellet.

[0048] Soaking or absorption preparation method: Preheat the pellets of the premix of components (A) to (C) in a glass container at 90°C in an oven under a nitrogen atmosphere for at least 4 hours, and the pellets have been prepared by a melt mixing preparation method. Remove the glass container and contents from the oven and then add to the preheated pellets in the container components (D) and (E). The resulting mixture of components (A) to (E) is shaken briefly, and then the pellets are tumbled at 30 rpm for 10 minutes with (D) and (E) until the pellets have absorbed all of (D) and (E), that is, until (D) and (E) have been soaked or absorbed into the pellets. The resulting soaked pellets are placed in a 90°C oven under a nitrogen atmosphere for at least 10 hours to obtain a polyolefin formulation comprising components (A) to (E) in pellet form. Comparative preparations can be prepared in a similar manner, except that one or two of the components can be omitted from the comparative preparation or one of the components can be used in a non-inventive amount.

[0049] Compression molded plaque sample preparation method: Each compression molded plaque sample of the test material was prepared by compression molding the pellets of the test material in a press at a pressure of 3.5 MPa (500 psi) and at a temperature of 125° C. for 3 minutes, then at a temperature of 125° C. at a pressure of 17 MPa (2500 psi) for 3 minutes, then at a temperature of 200° C. at a pressure of 17 MPa for 12 minutes, then cooling the compression molded plaque sample to 30° C. at a pressure of 17 MPa, and then opening the press to obtain the compression molded plaque sample. Pellets of the test material were prepared according to the soaking or absorption preparation method.

[0050] Density test method: measured according to ASTM D792-13, "Standard Test Methods for Density and Specific Gravity (Relative Density) of Plastics by Displacement, Method B" (used to test solid plastics in liquids other than water, such as in liquid 2-propanol). In grams per cubic centimeter (g / cm 3 ) as the unit to report the results.

[0051] Elongation at break test method: According to ASTM D638-14, "Standard Test Method for Tensile Properties of Plastics", the displacement rate is 5.08 cm / min, and the five results are averaged on five compression molded plate samples prepared from the same test material according to the compression molded plate sample preparation method. The results are reported as elongation at break percentage (%).

[0052] Flexural modulus test method: at 23 ° C, according to ASTM D790-15e2, "Standard Test Methods for Flexural Properties of Unreinforced and Reinforced Plastics and Electrical Insulating Materials", measured at 0.05 inches / minute (0.127 cm / minute) on a compression molded plaque specimen with a thickness of 3.18 mm (125 mils) in a crosshead position, and expressed in pounds per square inch (psi) or equivalent megapascals (MPa).

[0053] Heat Aging Method: The test material or compression molded plaque specimens were maintained in a Type II ASTM D5423-93 testing machine convection oven set at 135°C in an air atmosphere for 10 days to give heat aged test material or heat aged plaque specimens, respectively.

[0054] Melt Index (I2) Test Method: For polyethylene polymers, according to ASTM D1238-04, Standard Test Method for Melt Flow Rates of Thermoplastics by Extrusion Platometer, using 190°C / 2.16 kilograms (kg) conditions (formerly known as "Condition E") to measure. The results are reported in grams eluted per 10 minutes (g / 10min) or equivalently in decigrams per 1.0 minute (dg / 1min). 10.0dg=1.00g. The melt index is inversely proportional to the weight average molecular weight of the polyethylene, although the inverse proportionality is not linear. Therefore, the higher the molecular weight, the lower the melt index.

[0055] Melt Flow Rate (MFR) Test Method: For polypropylene polymers, measured according to ASTM D-1238 using conditions of 230°C or 260°C and 2.16 kg.

[0056] Tensile Strength Test Method: (Breaking Stress) Measured according to ASTM D638-14 using a displacement rate of 5.08 cm / min on five compression molded plaque specimens made from the same test material according to the Compression Molded Plaque Specimen Preparation Method, and then average the five results. Report the results in megapascals (MPa).

[0057] Examples

[0058] Component Example (A)-1: having 0.90 g / cm 3 Up to 0.92g / cm 3 A polypropylene homopolymer having a density of 1000 Å and a melt flow rate (MFR) of 3 g / 10 min measured at 230° C., 2.16 kg. Available from Braskem as product FF030F2.

[0059] Component Example (B)-1: Density 0.87 g / cm 3 and a poly(ethylene-co-1-butene) copolymer having a melt index (I2) of less than 0.5 g / 10 min (e.g., 0.4 g / 10 min). Available from The Dow Chemical Company as the product ENGAGE TM HM 7387 obtained.

[0060] Component Example (C)-1: Ethylene / propylene diblock copolymer having a melt flow rate (MFR) of 6.5 g / 10 min measured at 260° C., 2.16 kg. Available from The Dow Chemical Company as INTUNE TM D5535 obtained.

[0061] Component Example (D)-1: Dibenzyltoluene available from Sasol Germany GmbH as Marlotherm SH.

[0062] Component Example (E)-1: 4,6-bis(octylthiomethyl)-o-cresol, available as Irgastab Cable KV10 from BASF.

[0063] Examples 1 to 4 (IE1 to IE4) of the present invention: Unaged polyolefin formulations were prepared according to the immersion or absorption preparation method, and had the compositions shown in Table 1 and the mechanical properties shown in Tables 2 and 3. The polyolefin formulations of IE1 to IE4 were heat aged according to the heat aging method to obtain heat aged polyolefin products of IE1 to IE4, respectively, which had the mechanical properties shown in Tables 2 and 3.

[0064] Comparative Examples 1 to 4 (CE1 to CE4): Unaged comparative formulations were prepared according to the soaking or absorption preparation method and had the compositions shown in Table 1 and the mechanical properties shown in Tables 2 and 3. The comparative formulations of CE1 to CE4 were heat aged according to the heat aging method to obtain heat aged comparative products of CE1 to CE4, respectively, having the mechanical properties shown in Tables 2-3.

[0065] Table 1. Composition of IE1 to IE4 and CE1 to CE4.

[0066] Instance Number (A)-1(wt%) (B)-1 (wt%) (C)-1(wt%) (D)-1(wt%) (E)-1(wt%) Total (wt%) IE1 16.4 72.6 4.7 6.0 0.3 100.0 IE2 35.1 53.9 4.7 6.0 0.3 100.0 IE3 44.5 44.5 4.7 6.0 0.3 100.0 IE4 53.9 35.1 4.7 6.0 0.3 100.0 CE1 46.85 46.85 0 6.0 0.3 100.0 CE2 47.5 47.5 5.0 0 0 100.0 CE3 46.85 0 46.85 6.0 0.3 100.0 CE4 72.6 16.4 4.7 6.0 0.3 100.0

[0067] As can be seen in Table 1, the unaged inventive polyolefin formulations IE1 to IE4 contain components (A) to (E) in the claimed amounts. The unaged comparative formulations CE1 to CE4 lack one of components (A) to (E) (CE1 and CE3), lack two of components (A) to (E) (CE2), or contain each of components (A) to (E), but not in the claimed amounts (CE4).

[0068] Table 2. Flexural modulus and elongation at break of IE1 to IE4 and CE1 to CE4.

[0069]

[0070] The properties reported in Table 2 were measured on unaged polyolefin formulations or unaged comparative formulations, unless "heat aged" indicates that the property was measured on heat aged polyolefin products or heat aged comparative products prepared therefrom. In Table 2, * indicates an estimated value.

[0071] As shown in Table 2, the unaged polyolefin formulation advantageously has a flexural modulus of less than 300 megapascals (MPa) measured according to ASTM D790-15e2. The heat aged polyolefin products of the present invention prepared therefrom by heat aging advantageously have an elongation at break greater than 350% measured according to ASTM D638-14.

[0072] Table 3: Mechanical properties of IE1 to IE4 and CE1 to CE4.

[0073] Instance Number Tensile strength (MPa) Thermal aging tensile strength (MPa) IE1 18.58 18.2 to 18.9* IE2 20.30 19.92 IE3 21.64 21.72 IE4 24.87 24.26 CE1 18.59 12.25 CE2 19.04 17.42 CE3 12.74 14.75 CE4 21.20 21.52

[0074] The properties reported in Table 3 were measured on unaged polyolefin formulations or unaged comparative formulations, unless "heat aged" indicates that the property was measured on heat aged polyolefin products or heat aged comparative products prepared therefrom. In Table 3, * indicates an estimated value.

[0075] As shown in Table 3, the unaged polyolefin formulations of IE1 to IE4 of the present invention and the heat-aged polyolefin products of IE1 to IE4 of the present invention prepared therefrom advantageously have a tensile strength greater than 8.5 MPa measured according to ASTM D638-14.

[0076] IE3 was a repeat of previous preparation and testing experiments by different individuals. The previous experiments produced samples with a flexural modulus of 211 MPa, an elongation at break of 647%, an elongation at break after heat aging of 477%, a tensile strength of 20.8 MPa, and a tensile strength after heat aging of 15.3 MPa.

[0077] As shown in the examples, the unaged polyolefin formulations of the present invention have improved (increased) flexibility and improved (increased) resistance to the flexibility-reducing effects of heat aging (collectively referred to as the "initial invention benefits"). The improved (increased) flexibility is indicated by a flexural modulus of less than 300 MPa and optionally a lower flexural modulus relative to the flexural modulus of the comparative formulation. The improved (increased) resistance to the effects of heat aging is indicated by the resulting heat-aged polyolefin product having an elongation at break of 350% or more. The improved (increased) resistance to the effects of heat aging is indicated by the resulting heat-aged polyolefin product having a tensile strength of greater than 8.5 MPa after heat aging. Therefore, the unaged polyolefin formulations of the present invention and the heat-aged polyolefin products of the present invention prepared therefrom by heat aging are more useful in industrial applications that benefit from flexibility and resistance to heat aging, such as, for example, as a coating (e.g., insulation layer) of a medium voltage (MV), high voltage (HV) or extra-high voltage (EHV) power cable. Advantageously, the polyolefin formulation is not cross-linked and therefore does not have to be cross-linked in order to be used as a coating in such power cables, and therefore the materials and coatings of the invention are advantageously recyclable. The polyolefin formulation and heat aged polyolefin product may have additional benefits and may be used in other industries such as aerospace, automotive and medical applications.

[0078] The following claims are incorporated herein by reference.

Claims

1. A polyolefin formulation comprising the following amounts of components (A) to (E): 15.0 to 55.0 weight percent (wt%) of (A) a polypropylene homopolymer; 77.9 to 30.0 wt% of (B) a poly(ethylene-co-1-olefin) copolymer; 3.0 to 6.5 wt% of (C) an ethylene / propylene diblock copolymer; 4.0 to 8.0 wt% of (D) a saturated aromatic (C 14 -C 60 ) hydrocarbon; and 0.1wt% to 1.5wt% of (E) an antioxidant; wherein, The wt% of (B) divided by the wt% of (A) is in a mass ratio of 5.0:1.0 to 0.50:1.0; and wherein the total amount of components (A), (B) and (C) is 88.0 wt% to 95.9 wt% of the polyolefin formulation; and wherein the total amount of components (A) to (E) is 92.1 wt% to 100.0 wt% of the polyolefin formulation.

2. The polyolefin formulation of claim 1, wherein the polyolefin formulation is an unaged polyolefin formulation that has not been subjected to heat aging and has characteristics (i) and (ii) and optionally characteristic (iii): (i) a flexural modulus of less than 300 megapascals (MPa) measured according to ASTM D790-15e2; and (ii) an elongation at break greater than or equal to 550% measured according to ASTM D638-14; and optionally (iii) a tensile strength greater than 8.5 MPa measured according to ASTM D638-14.

3. The polyolefin formulation of claim 2, wherein subjecting the unaged polyolefin formulation to heat aging at 135 degrees Celsius (° C.) for 10 days produces a heat-aged polyolefin product having characteristic (i) and optionally characteristic (ii): (i) an elongation at break greater than 350% measured according to ASTM D638-14; and optionally (ii) a tensile strength greater than 8.5 MPa measured according to ASTM D638-14.

4. The polyolefin formulation according to any one of claims 1 to 3, wherein the polyolefin formulation has 16.0 wt% to 54.0 wt% of the (A) polypropylene homopolymer; 72.0 wt% to 35.4 wt% of the (B) poly(ethylene-co-1-olefin) copolymer; 4.0 to 6.0 wt% of the (C) ethylene / propylene diblock copolymer; 5.0 wt% to 7.0 wt% of the (D) saturated aromatic (C 14 -C 60 ) hydrocarbon; and 0.1wt% to 1.0wt% of the (E) antioxidant; wherein, The wt% of (B) divided by the wt% of (A) is in a mass ratio of 4.5:1.0 to 0.60:1.0; and wherein the total amount of components (A), (B) and (C) is 88.0 wt% to 94.9 wt% of the polyolefin formulation; and wherein the total amount of components (A) to (E) is 93.0 wt% to 100.0 wt% of the polyolefin formulation.

5. The polyolefin formulation according to any one of claims 1 to 3, having any one of features (i) to (v): (i) the (A) polypropylene homopolymer has a molecular weight of 0.89 g / cm3 to 0.93 g / cm3 (g / cm 3) and a melt flow rate of 1.0 g / 10 min to 10 g / 10 min as measured at 230° C., 2.16 kg in accordance with ASTM D-1238; (ii) wherein the (B) poly(ethylene-co-1-olefin) copolymer has a density of 0.850 g / cm2 as measured in accordance with ASTM D792-13 Method B. 3 Up to 0.890g / cm 3 and a melt index (I2) of 0.1 g / 10 min to 5.0 g / 10 min measured at 190° C., 2.16 kg according to ASTM D-1238; (iii) wherein the (C) ethylene / propylene diblock copolymer has a melt flow rate of 4 g / 10 min to 8 g / 10 min measured at 260° C., 2.16 kg according to ASTM D-1238; (iv) wherein the (D) saturated aromatic (C 14 -C 60 ) hydrocarbons are saturated aromatic (C 19 -C 23 ) hydrocarbons; (v) wherein the antioxidant is a compound containing a sulfur atom.

6. A method for preparing a polyolefin formulation according to any one of claims 1 to 5, comprising melt mixing components (A), (B) and (C) at a temperature of 180 degrees Celsius to 220 degrees Celsius (°C) for an effective mixing period to obtain a premix of components (A), (B) and (C) and not containing components (D) and (E); and soaking or absorbing components (D) and (E) into the premix at a temperature of 80°C to 100°C for an effective absorption period of at least 4 hours to obtain the polyolefin formulation comprising components (A) to (E).

7. A heat aged polyolefin product made by subjecting the polyolefin formulation according to any one of claims 1 to 5 to heat aging conditions comprising a temperature of 50 to 140 degrees Celsius (°C) and a heat aging effective period of 10 days or more and an air atmosphere.

8. An article of manufacture comprising or made from the polyolefin formulation according to any one of claims 1 to 5 or the heat-aged polyolefin product according to claim 7.

9. A coated conductor comprising a conductive core and an insulating layer comprising a polyolefin formulation according to any one of claims 1 to 5 or a heat aged polyolefin product according to claim 7 at least partially covering the conductive core.

10. A method of conducting electricity, the method comprising applying a voltage across the conductive core of the coated conductor of claim 9 so as to produce an electric current through the conductive core.