Cu-based metal oxide catalyst, preparation method thereof and synthesis method of 2,3-butanediol using the same

The reaction between methanol and 1,2-propanediol was catalyzed by Cu-based metal oxide catalyst, and the safety and cost problems in the production of 2,3-butanediol were solved, achieving high efficiency and low cost 2,3-butanediol Alcohol preparation significantly improves the selectivity and yield of the product.

CN114588904BActive Publication Date: 2024-11-26QINGDAO INST OF BIOENERGY & BIOPROCESS TECH CHINESE ACADEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210220303.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-08
Publication Date
2024-11-26
Estimated Expiration
2042-03-08

AI Technical Summary

Technical Problem

The existing 2,3-butanediol production methods have safety problems and high production costs, and the separation process consumes a lot of energy, resulting in the fact that industrial applications have not yet been scaled.

Method used

Developing Cu-based metal oxide catalyst and its preparation method. By changing the ratio of metal atoms in the oxide, the activity and structure of the catalyst is significantly improved, and used to catalyze the batch high-pressure reaction of methanol and 1,2-propylene glycol, and prepare 2, 3-Butanediol.

Benefits of technology

The selectivity and yield of 2,3-butanediol is significantly improved, the process is simple and the conditions are mild, the catalyst can be reused many times, and the process is free of pollution, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114588904B_ABST
    Figure CN114588904B_ABST
Patent Text Reader

Abstract

The present application discloses a Cu-based metal oxide catalyst, a preparation method thereof, and a synthesis method of 2,3-butanediol using the same. The preparation method includes (1) preparing a mixed aqueous solution of a copper salt, a magnesium salt or a calcium salt, and a first metal A salt; (2) the mixed aqueous solution is added dropwise to a carbonate aqueous solution or an alkaline solution, then an alkaline solution is added dropwise to adjust the pH value of the system, then stirring is continued, standing and aging, then filtering and washing to neutrality, and drying; and (3) the obtained product of step (2) is roasted at a temperature of 500°C to 600°C and in an air atmosphere for 3 to 12 hours to obtain the Cu-based metal oxide catalyst. The preparation method is simple and fast, the process is simple, economical and pollution-free, and easy to operate. The catalyst can not only significantly improve the selectivity and yield of the product. And the synthesis method of the 2,3-butanediol is simple in process, mild in conditions, and significantly improves the selectivity of 2,3-butanediol.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The present application belongs to the field of inorganic catalysts, and specifically, relates to a Cu-based metal oxide catalyst, a preparation method thereof, and a method for synthesizing 2,3-butanediol using the same. Background technology:

[0002] Layered double hydroxides (LDHs), also known as anionic clay compounds, are a general term for natural and synthetic hydrotalcites and hydrotalcite-like compounds. They are a typical class of anionic host-guest layered structure compounds. The most prominent feature is the host layer structure and the exchangeability of interlayer ions. This feature can be used to achieve layer metal ion modulation and functional guest intercalation into interlayer gaps, thereby forming a series of new supramolecular composite functional materials. Most structures of LDHs are close to hydrotalcite, and their molecular formula is Mg 6 Al 2 (OH) 16 CO 3 ·4H 2 O, and naturally exists in fibers. Based on the structural characteristics of hydrotalcite-like compounds, as well as other composite metal oxides MgO-ZrO 2 Alkaline earth metal oxides such as CaO and MgO are often used as catalyst carriers. A series of metal mixed oxides (MMO) are derived and prepared by freely combining Cu, Mg, Al, Zr, and Ca elements. Compared with commonly used heterogeneous catalysts, ternary mixed metal oxides (MMO) have a similar structure to the hydrotalcite system and have the advantages of being regenerable and stable in a wide temperature range.

[0003] 2007 Suárez DR, Zeifert BH, MH et al. reported that copper hydrotalcite compounds: morphology, structure and microstructural characteristics. Hydrotalcite is composed of brucite-like [Mg(OH) 2 ] sheet formation, in which Mg 2+ By trivalent cations (such as Al 3+ ) Partial isomorphous substitution occurs, and the excess positive charge in the layer is compensated by anions that occupy the interlayer space together with water molecules. When the properties of the interlayer cations and interlayer anions are changed, the compound is called a hydrotalcite-like compound (HTLC), which has a wide range of uses in adsorption and catalysis. These compounds are represented by the general formula [M 2+ 1-x M 3+ x (OH) 2 ] x+ (A n- ) x / n ·mH 2O means, where M 2+ and M 3+ are divalent and trivalent cations, x is M 2+ / (M 2+ +M 3+ ) ratio, A n- It is an interlayer anion with a charge number of n. Lee G, Kang JY, Yan N et al. reported on the simple preparation method of Mg-Al hydrotalcite as a base catalyst. The structure of this type of compound is composed of a positively charged brucite-like M 2+ (OH) 2 The layers are composed of exchangeable anions and water molecules, and the exchangeable anions exist in the form of hydrated anions. Kagunya W, Hassan Z, Jones W. Research report on the catalytic properties of layered double hydroxides and their calcined derivatives is introduced. The host and guest of LDHs are connected by weak chemical bonds such as electrostatic attraction, hydrogen bonds or van der Waals forces, and the host and guest are arranged in a very orderly manner. This special structure makes it easy for the layers of the host to be stretched or peeled off by the guest without affecting the layer structure. Therefore, LDHs exhibit intercalation and assembly properties. This type of functional inorganic and organic anion intercalated hydrotalcite has been widely used in the heterogeneity of homogeneous reaction catalysts, catalyst immobilization, and improving the stability of catalysts. Studies have reported that anions of different charges and sizes will cause changes in the position and intensity of a series of characteristic diffraction peaks of intercalated structure LDHs. Miyata and Kumura et al. synthesized a series of terminal straight-chain fatty dicarboxylic acid anions C n H 2n (CO 2 - ) 2 Intercalated ZnAl-LDHs. Changes in the charge density of the LDHs layer will also cause changes in the arrangement of the interlayer guest molecules and thus affect the interlayer spacing. Li Bo et al. used XRD technology to analyze the crystal structure of dodecylsulfonate intercalated MgAl-LDH. Olszówka JE, Karcz R, Bielańska E et al. reported in 2018 new insights into the preferred valence of interlayer anions in hydrotalcite-like compounds: the influence of the Mg / Al ratio. Composite oxide-type solid bases are often prepared by calcining LDHs as precursors, such as hydrotalcite and Mg-Al anionic layered compounds with a hydrotalcite structure. This layered compound is calcined with LDHs as a precursor and is a mesoporous material with strong alkalinity, large specific surface area, high stability, and adjustability of structure and alkalinity.

[0004] 2,3-Butanediol (2,3-butanediol), molecular formula is C 4 H 10 O 2, colorless viscous liquid, crystalline at low temperature. Miscible with water, soluble in alcohol and ether. 2,3-Butanediol is a high value-added compound, widely used in food, chemical, energy and other fields, and is currently mainly produced by bioconversion. 2,3-Butanediol and its derivatives, as important liquid fuels and chemical raw materials, have broad industrial application prospects. Most production methods of 2,3-butanediol have safety issues and high product separation costs. For example, Dai Jianying et al. reviewed the progress of biotechnology production of 2,3-butanediol. At present, the separation process consumes a lot of energy, the production cost of 2,3-butanediol is still relatively high, and its application in various fields has not yet been scaled up (Research Progress of Bio-based Chemical 2,3-Butanediol, Journal of Process Engineering, 2010, 10(1), 200-108). 2,3-Butanediol is widely used in food, chemical, energy and other fields.

[0005] Therefore, it is necessary to develop a suitable catalyst and a method for synthesizing 2,3-butanediol using the catalyst. Summary of the invention:

[0006] In view of the shortcomings of the above-mentioned prior art, one object of the present application is to provide a Cu-based metal oxide catalyst. The Cu-based metal oxide catalyst is used to catalyze the reaction of synthesizing 2,3-butanediol, which can not only significantly improve the selectivity and yield of the product, but also significantly improve the activity and structure of the catalyst by changing the ratio of metal atoms in the oxide.

[0007] Another object of the present application is to provide a method for preparing the above-mentioned Cu-based metal oxide catalyst. The preparation method is simple and fast, has a simple process, is economical and pollution-free, is easy to operate, and the prepared catalyst can be reused multiple times without a significant decrease in activity.

[0008] Another object of the present application is to provide a method for synthesizing 2,3-butanediol using the Cu-based metal oxide catalyst. The method has simple process, mild conditions, and significantly improves the selectivity of 2,3-butanediol.

[0009] In order to achieve the above objectives, in a first aspect, the present application provides a method for preparing a Cu-based metal oxide catalyst, which comprises the following steps:

[0010] (1) preparing a mixed aqueous solution of a copper salt, a magnesium salt or a calcium salt, and a first metal A salt, wherein the first metal A salt is a salt of a divalent or trivalent metal ion; wherein the molar ratio of Mg or Ca to the first metal A is 1.4 to 6, and the molar amount of Cu is 2% to 60% of the total molar amount of all metal ions;

[0011] (2) adding the mixed aqueous solution of metal salts obtained in step (1) dropwise to a carbonate aqueous solution or an alkaline solution at 60° C. to 70° C., then adding an alkaline solution dropwise to adjust the pH value of the system to 9.5 to 10.5, preferably 10, then stirring at room temperature for 1 to 5 hours, and standing for aging for 18 to 30 hours, preferably 24 hours, then filtering and washing to neutrality, and drying at 100° C. to 120° C. for 12 to 24 hours; and

[0012] (3) calcining the product obtained in step (2) at a temperature of 500° C. to 600° C. in an air atmosphere for 3 to 12 hours to obtain the Cu-based metal oxide catalyst Cu y Mg m A n O x Cu y Ca m A n O x , wherein the ratio of m / n is 1.4 to 6, y / (m+n+y) is 0.02 to 0.6, and x is the chemical oxygen demand of the stoichiometric ratio.

[0013] In combination with the first aspect, in a feasible embodiment, when copper salt and magnesium salt are used in step (1), the first metal A salt is at least one selected from Ca salt, Al salt and Zr salt; when copper salt and calcium salt are used, the first metal A salt is at least one selected from Al salt and Zr salt.

[0014] In combination with the first aspect, in a feasible implementation, the copper salt, magnesium salt, Ca salt and first metal A salt are preferably nitrates.

[0015] In combination with the first aspect, in a feasible implementation manner, the preparation process of step (1) is carried out at 60°C to 70°C.

[0016] In combination with the first aspect, in a feasible embodiment, in step (2), the carbonate in the carbonate aqueous solution is at least one selected from sodium carbonate or potassium carbonate, and preferably sodium carbonate, and the metal salt mixed aqueous solution is added dropwise to the carbonate aqueous solution so that the molar concentration of carbonate in the system is 0.5 to 10 times the total molar concentration of metal ions.

[0017] In combination with the first aspect, in a feasible embodiment, in the step (2), the alkali in the alkali solution is at least one selected from sodium hydroxide or potassium hydroxide, and preferably sodium hydroxide, and the OH in the alkali solution is - The molar concentration of the ions is 1 to 10 times the total molar concentration of the metal ions in the mixed aqueous solution.

[0018] In combination with the first aspect, in a feasible implementation manner, in the step (2), the pH value of the system is preferably adjusted to 10.

[0019] In combination with the first aspect, in a feasible implementation manner, in the step (2), the static aging time is preferably 24 hours.

[0020] In combination with the first aspect, in a feasible embodiment, the preparation method of the Cu-based metal oxide catalyst also includes: in step (3), reducing the calcined product in a hydrogen atmosphere at 300°C to 400°C for 2.5 to 3.5 hours, preferably 3 hours, to obtain the Cu-based metal oxide catalyst.

[0021] In a second aspect, the present application provides a Cu-based metal oxide catalyst prepared by the above-mentioned preparation method of the Cu-based metal oxide catalyst.

[0022] In a third aspect, the present application provides a method for synthesizing 2,3-butanediol using the above-mentioned Cu-based metal oxide catalyst, which comprises:

[0023] In the presence of the Cu-based metal oxide catalyst and in a hydrogen atmosphere, methanol and 1,2-propylene glycol are subjected to an intermittent high-pressure reaction for 3 to 5 hours at a gas pressure of 1 MPa to 3 MPa and a reaction temperature of 190° C. to 210° C. to obtain 2,3-butanediol.

[0024] In conjunction with the third aspect, in a feasible implementation, the weight of 1,2-propylene glycol accounts for 2.5% to 35% of the total weight of the mixture of methanol and 1,2-propylene glycol, and preferably 7.5% to 15%.

[0025] In combination with the third aspect, in a feasible implementation manner, the reaction temperature is preferably 210°C.

[0026] The technical solution provided by this application has at least the following beneficial effects compared with the prior art:

[0027] The present application provides a Cu-based metal oxide catalyst and a preparation method thereof. The Cu-based metal oxide catalyst is used to catalyze the reaction of synthesizing 2,3-butanediol. It has a stable structure, more uniform acid and alkali active sites, and better acid and alkali resistance, and has greater potential in the application of catalyzing the condensation of methanol and 1,2-propylene glycol to prepare 2,3-butanediol. The catalyst can not only significantly improve the selectivity and yield of the product, but also significantly improve the activity and structure of the catalyst by changing the ratio of metal atoms in the oxide. The preparation method is simple and fast, the process is simple, economical and pollution-free, and the operation is convenient, and the obtained catalyst can be reused many times without significantly reducing the activity. In addition, within the specified range of the ratio of each element of the mixed metal oxide, the selectivity of 2,3-butanediol is significantly improved.

[0028] The present application also provides a method for synthesizing 2,3-butanediol by catalyzing the direct condensation of methanol and 1,2-propylene glycol using the above-mentioned Cu-based metal oxide catalyst. The method has a simple reaction process and mild conditions. Description of the drawings:

[0029] Figure 1 These are the two main pathways for the condensation reaction of methanol and 1,2-propylene glycol.

[0030] Figure 2 The invention relates to the reaction steps of synthesizing 2,3-butanediol by reacting methanol and 1,2-propylene glycol.

[0031] Figure 3 The adsorption-desorption curves and pore size distributions of four CuMgAl mixed oxide catalysts prepared according to Examples 1-2 of the present application using aqueous sodium carbonate solutions of different concentrations as precipitants.

[0032] Figure 4 XRD patterns of four CuMgAl mixed oxides prepared using different concentrations of sodium carbonate aqueous solution as precipitant according to Examples 1-2 of the present application

[0033] Figure 5 It is a SEM image of a Cu-based metal oxide catalyst (Gr-CuMgAl) having a molar ratio of Mg:Al:Cu atoms of 12:4:3 prepared according to Examples 1-3 of the present application.

[0034] Figure 6 NH for CuCaZr (Example 10), CuMgCaOx (Example 3-1), CuMgZr (Example 2) and CuMgAl (Example 1-1) catalysts 3 -TPD.

[0035] Figure 7This is the XRD phase analysis of the CuMgCaOx catalyst before and after the reaction prepared by the co-precipitation method described in Example 3-3 of the present application.

[0036] Figure 8 SEM images of Cu-based metal oxide catalysts with a molar ratio of Mg:Ca:Cu atoms of 12:8:3 (upper row) prepared according to Example 3-1 of the present application and a molar ratio of Mg:Ca:Cu atoms of 8:13:3 (lower row) prepared according to Example 3-4.

[0037] Fig. 9 The figure is a TEM image of the Cu-based metal oxide catalyst of CuMgCaOx (the molar ratio of Mg:Ca:Cu atoms is 12:8:3) prepared according to Example 3-1 of the present application. Specific implementation method:

[0038] In order to enable those skilled in the art to more clearly understand the application, the application will be described in detail below in conjunction with examples.Before describing, it should be understood that the terms used in this specification and the attached claims should not be interpreted as being limited to the general meaning and dictionary meaning, but should be interpreted according to the meaning and concept corresponding to the technical aspects of the application on the basis of the principle of allowing the inventor to appropriately define the terms for the best interpretation.Therefore, the description proposed here is only for the preferred example for the purpose of illustration, and it is not intended to limit the scope of the application, so that it should be understood that, without departing from the spirit and scope of the application, other equivalents or improved methods can be obtained therefrom, and the scope of the application for protection should be based on the scope defined by the claims.Unless otherwise specified, the reagents and instruments used in the following examples are commercially available products.

[0039] The present application first provides a Cu-based metal oxide catalyst and a preparation method thereof. The preparation method uses LDHs as a carrier and performs modification, and prepares a Cu-based LDHs-type catalyst by coprecipitation-calcination. The calcined Mg-metal hydrotalcite has an L acid-base pair, which is very beneficial to the cross-condensation reaction. Combined with the strong hydrogenation effect of copper, a Cu-based metal oxide catalyst is developed to be applied to the cross-condensation reaction of diols and monools, such as catalyzing the condensation of methanol and 1,2-propylene glycol to prepare 2,3-butanediol.

[0040] In addition, the present application also provides a method for catalytically synthesizing 2,3-butanediol using the Cu-based metal oxide catalyst. The method mainly obtains the target product through an alcohol coupling reaction, and synthesizes two stereoisomers of 2,3-butanediol and 1,2-butanediol, wherein the selectivity for 2,3-butanediol is higher. The raw materials of the process are cheap and easy to obtain, the operating equipment and process are simple, and the environmental pollution is small.

[0041] Specifically, the present application is implemented through the following technical solutions:

[0042] In a first aspect, the present application provides a method for preparing a Cu-based metal oxide catalyst, which comprises the following steps:

[0043] (1) preparing a mixed aqueous solution of a copper salt, a magnesium salt or a calcium salt, and a first metal A salt, wherein the first metal A salt is a salt of a divalent or trivalent metal ion, wherein the molar ratio of Mg or Ca to the first metal A is 1.4 to 6, and the molar content of Cu is 2% to 60% of the total molar amount of all metal ions; and

[0044] (2) adding the mixed aqueous solution obtained in step (1) dropwise to a carbonate aqueous solution or an alkaline solution at 60° C. to 70° C., then adding an alkaline solution dropwise to adjust the pH value of the system to 9.5 to 10.5, then continuing to stir at room temperature for 1 to 5 hours, and standing for aging for 18 to 30 hours, then filtering and washing to neutrality, and drying at 100° C. to 120° C. for 12 to 24 hours;

[0045] (3) calcining the product obtained in step (2) at a temperature of 500° C. to 600° C. in an air atmosphere for 3 to 12 hours to obtain the Cu-based metal oxide catalyst Cu y Mg m A n O x Cu y Ca m A n O x , wherein the ratio of m / n is 1.4 to 6, y / (m+n+y) is 0.02 to 0.6, and x is the chemical oxygen demand of the stoichiometric ratio.

[0046] The preparation method of the Cu-based metal oxide catalyst according to the present application is simple and fast, has a simple process, is economical and pollution-free, is easy to operate, and the prepared catalyst can be reused multiple times without a significant decrease in activity.

[0047] In combination with the first aspect, in a feasible embodiment, when copper salt and magnesium salt are used in step (1), the first metal A salt is at least one selected from Ca salt, Al salt and Zr salt; when copper salt and calcium salt are used, the first metal A salt is at least one selected from Al salt and Zr salt.

[0048] In the present application, a series of Cu-based metal oxide catalysts can be synthesized by the above catalyst preparation method, including CuMgAl oxide catalyst, CuMgZr oxide catalyst, CuMgCaOx oxide catalyst and CuCaZr oxide catalyst, etc. Among them, CuMgAl oxide catalyst and CuMgCaOx oxide catalyst have higher activity and are more preferred.

[0049] In the step (1), in the mixed aqueous solution, the molar ratio of Mg or Ca to A is 1.4 to 6, for example, 1.4, 1.6, 1.8, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5 or 6, or other values ​​within the range. And the molar content of Cu is 2% to 60% of the total molar amount of all metal ions, for example, 2%, 3%, 10%, 20%, 50% or 60%, or other values ​​within the range. Within the range of the molar ratio (molar fraction), a Cu-based metal oxide catalyst with excellent performance can be obtained.

[0050] In combination with the first aspect, in a feasible embodiment, the copper salt, the magnesium salt and the first metal A salt are preferably nitrates. Nitrates are generally water-soluble, which is conducive to preparing a solution to obtain a precipitated product by a coprecipitation method, and the remaining nitrate is also easy to remove by water washing.

[0051] In combination with the first aspect, in a feasible implementation, the preparation process of step (1) is carried out at 60° C. to 70° C. By preparing the solution at a higher temperature, it is beneficial to improve the solubility of the copper salt, the magnesium salt and the first metal A salt, so as to facilitate the subsequent acquisition of more precipitation products.

[0052] In combination with the first aspect, in a feasible embodiment, in the step (2), the carbonate in the carbonate aqueous solution is selected from at least one of sodium carbonate or potassium carbonate, and preferably sodium carbonate, and the metal salt mixed aqueous solution is added dropwise to the carbonate aqueous solution so that the molar concentration of carbonate in the system is 0.5 to 10 times the total molar concentration of metal ions, for example, it can be 0.5 times, 1 times, 1.5 times, 2 times, 2.5 times, 3 times, 3.5 times, 4 times, 4.5 times, 5 times, 5.5 times, 6 times, 6.5 times, 7 times, 7.5 times, 8 times, 8.5 times, 9 times, 9.5 times or 10 times, or other values ​​within the range. By using a carbonate precipitant, it is convenient to prepare layered composite metal hydroxides (LDHs).

[0053] In combination with the first aspect, in a feasible embodiment, the alkali in the alkaline solution is at least one selected from sodium hydroxide or potassium hydroxide, and preferably sodium hydroxide, and the OH in the alkaline solution is - The molar concentration of the ions is 1 to 10 times the total molar concentration of the metal ions in the mixed aqueous solution, for example, 1 times, 1.5 times, 2 times, 2.5 times, 3 times, 3.5 times, 4 times, 4.5 times, 5 times, 5.5 times, 6 times, 6.5 times, 7 times, 7.5 times, 8 times, 8.5 times, 9 times, 9.5 times or 10 times, or other values ​​within the range.

[0054] In combination with the first aspect, in a feasible implementation, in the step (2), the pH value of the system is preferably adjusted to 10. By controlling the pH value of the system to 9.5 to 10.5, preferably 10, the formation of precipitation can be effectively promoted.

[0055] In conjunction with the first aspect, in a feasible implementation, in the step (2), the standing and aging time is 18 to 30 hours, for example, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, 25 hours, 26 hours, 27 hours, 28 hours, 29 hours or 30 hours, or other values ​​within the range. And, the standing and aging time is preferably 24 hours. By fully standing and aging, it is easy to obtain the desired precipitated product.

[0056] In combination with the first aspect, in a feasible embodiment, the method for preparing the Cu-based metal oxide catalyst further comprises: in step (3), reducing the calcined product in a hydrogen atmosphere at 300° C. to 400° C. for 2.5 to 3.5 hours, preferably 3 hours, to obtain the Cu-based metal oxide catalyst. When the first metal A salt is, for example, an Al salt, calcining in a hydrogen atmosphere can further improve the reaction activity.

[0057] In a second aspect, the present application provides a Cu-based metal oxide catalyst prepared by the above-mentioned preparation method of the Cu-based metal oxide catalyst.

[0058] The Cu-based metal oxide catalyst according to the present application is used to catalyze the reaction of synthesizing 2,3-butanediol. The catalyst can not only significantly improve the selectivity and yield of the product, but also significantly improve the activity and structure of the catalyst by changing the ratio of metal atoms in the oxide.

[0059] In a third aspect, the present application provides a method for synthesizing 2,3-butanediol using the above-mentioned Cu-based metal oxide catalyst, which comprises:

[0060] In the presence of the Cu-based metal oxide catalyst and in a hydrogen atmosphere, methanol and 1,2-propylene glycol are subjected to an intermittent high-pressure reaction at a gas pressure of 1 to 3 MPa and a reaction temperature of 190° C. to 210° C. for 3 to 5 hours to obtain 2,3-butanediol.

[0061] According to the method for synthesizing 2,3-butanediol using the Cu-based metal oxide catalyst described above, the process is simple, the conditions are mild, and the selectivity of 2,3-butanediol is significantly improved.

[0062] Furthermore, the gas pressure of the reaction may be 1-3 MPa, for example, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa or 3 MPa, or other values ​​within the range. By carrying out the reaction under such gas pressure, the formation of 2,3-butanediol is facilitated.

[0063] Further, the reaction time can be 3 to 5 hours, for example, 3 hours, 3.5 hours, 4 hours, 4.5 hours or 5 hours, or other values ​​within the range. Within this reaction time range, the yield of 2,3-butanediol will reach a maximum.

[0064] In addition, the intermittent high-pressure reaction may be performed in an intermittent high-pressure reactor, but the present application is not limited thereto.

[0065] For the condensation reaction of methanol and 1,2-propylene glycol, there are two carbon chain growth reaction pathways of 1,2-propylene glycol in the methanol system, namely, CC bonding at both ends of 1,2-propylene glycol. The main reaction pathways are as follows: Figure 1 The reaction belongs to the Guerbet reaction, also known as alcohol coupling. This reaction is a dehydration process with high atomic utilization. It is an important way for the carbon chain growth reaction of alcohol compounds. The process mainly includes four reaction steps. The carbon chain growth reaction process of 1,2-propylene glycol in the methanol system mainly includes the following steps: Figure 2 Several processes are shown (dehydrogenation, aldol condensation, dehydration and hydrogenation).

[0066] In conjunction with the third aspect, in a feasible embodiment, the weight of 1,2-propylene glycol accounts for 2.5% to 35% of the total weight of the mixture of methanol and 1,2-propylene glycol, for example, it can be 2.5%, 2.6%, 2.7%, 7.5%, 7.6%, 7.7%, 8.0%, 8.5%, 10.1%, 11.1%, 12.5%, 13.5%, 14.9%, 20.5%, 21.5%, 25.5%, 27.5%, 29.5% or 35%, or other values ​​within the range. Within this molar ratio range, it is helpful to convert methanol and 1,2-propylene glycol and generate 2,3-butanediol.

[0067] In conjunction with the third aspect, in a feasible embodiment, the reaction temperature may be 190°C to 210°C, for example, 190°C, 195°C, 200°C, 205°C or 210°C, or other values ​​within the range. Moreover, the reaction temperature is preferably 210°C. By carrying out the reaction within this temperature range, it is also helpful to promote the production of 2,3-butanediol.

[0068] The present application provides a Cu-based metal oxide catalyst and a preparation method thereof. The Cu-based metal oxide catalyst is used to catalyze the reaction of synthesizing 2,3-butanediol. It has a stable structure, more uniform acid and alkali active sites, and better acid and alkali resistance, and has greater potential in the application of catalyzing the condensation of methanol and 1,2-propylene glycol to prepare 2,3-butanediol. The catalyst can not only significantly improve the selectivity and yield of the product, but also significantly improve the activity and structure of the catalyst by changing the ratio of metal atoms in the oxide. The preparation method is simple and fast, the process is simple, economical and pollution-free, and the operation is convenient, and the obtained catalyst can be reused many times without significantly reducing the activity. In addition, within the specified range of the ratio of each element of the mixed metal oxide, the selectivity of 2,3-butanediol is significantly improved.

[0069] The present application also provides a method for synthesizing 2,3-butanediol by catalyzing the direct condensation of methanol and 1,2-propylene glycol using the above-mentioned Cu-based metal oxide catalyst. The method has a simple reaction process and mild conditions.

[0070] Example

[0071] Example 1-1

[0072] The following preparation method is used to prepare the Cu-based metal oxide catalyst according to the present application:

[0073] (1) preparing a mixed aqueous solution of magnesium nitrate, aluminum nitrate and copper nitrate in a molar ratio of 12:5:3 (volume of the mixed solution is about 150 mL);

[0074] (2) adding the mixed aqueous solution obtained in step (1) dropwise to a sodium carbonate aqueous solution at 65° C. to obtain a molar concentration of carbonate ion of 0.133 mol / L, such as 2.63 g Na 2 CO 3 A solution formed by dissolving in 187 mL of water, a molar concentration of magnesium of 0.06 mol / L, a molar concentration of aluminum of 0.025 mol / L and a molar concentration of copper of 0.015 mol / L, adding dropwise while stirring, then adding a sodium hydroxide solution (1 mol / L) to adjust the pH value of the system to 10, then continuing to stir at room temperature for 1 hour, and standing for aging for 24 hours, then filtering, washing the precipitate to neutrality, and then drying the precipitate at 100° C. for 24 hours; and

[0075] (3) The product obtained in step (2) was heated to 500°C in a tube furnace and calcined in an air atmosphere for 7 hours to obtain a black solid. The solid was then reduced in a hydrogen atmosphere at 350°C for 3 hours to obtain a CuMgAl oxide catalyst.

[0076] The above catalyst is used to synthesize 2,3-butanediol:

[0077] Methanol (analytical grade) and 1,2-propylene glycol (analytical grade) are mixed to form a solution of a certain concentration, which is then put into a reactor, and the catalyst prepared by the above method is added, and the reactor is sealed. Then, the air in the intermittent high-pressure reactor is replaced with nitrogen or hydrogen (multiple times), and the reactor is placed in a thermocouple heating jacket for heating, and the reaction time is set to 3 to 5 hours. After the reaction is completed, it is cooled to room temperature, filtered through a 0.22μm filter membrane, and a sample is prepared. Since 2,3-butanediol has three stereoisomers, including one meso isomer, two peaks will appear through gas chromatography (GC-MS), and the product conversion rate and yield are calculated. The experimental conditions and results are shown in Table 1 below:

[0078] Table 1 Catalytic conditions and catalytic effects of CuMgAl catalyst (reactant concentration refers to the concentration of 1,2-propylene glycol in the total amount of the mixture of methanol and 1,2-propylene glycol, wt.%)

[0079]

[0080] From the results in Table 1, it can be concluded that the catalyst exhibits high activity for low concentration of propylene glycol, and the selectivity is basically the same as that under high concentration of propylene glycol. High temperature is conducive to the conversion of the reaction, but at the same time, the side reactions increase. Therefore, the CuMgAl catalyst shown in Table 1 can significantly improve the conversion rate and selectivity of the reaction.

[0081] Example 1-2

[0082] The Cu-based metal oxide catalyst according to the present application was prepared in the same manner as in Example 1-1 above, except that sodium carbonate aqueous solution of different concentrations was used as the precipitant. Figure 3 As shown, the adsorption-desorption curves and pore size distribution of the prepared CuMgAl (12:4:3) oxide catalyst under different carbonate concentrations as precipitants are shown. During the experiment, for the catalysts prepared with different concentrations of precipitants, L-CuMgAl represents a low concentration precipitant (the molar concentration of carbonate in the system is 0.1 mol / L), calcined at a normal temperature of 550°C, and not reduced. Lr-CuMgAl represents a catalyst that is reduced and calcined at 350°C with hydrogen on the basis of L-CuMgAl treatment. G-CuMgAl represents a higher concentration precipitant (the molar concentration of carbonate in the system is 0.5 mol / L), calcined at a normal temperature of 550°C. The Gr-CuMgAl catalyst is reduced and calcined at 350°C with hydrogen on the basis of G-CuMgAl treatment.

[0083] Figure 3 Medium and high concentrations of Na 2 CO3 The pore size of the CuMgAl catalyst prepared by using the solution as a precipitant is obviously larger than that of the low concentration one, and is mainly composed of mesopores (2nm to 50nm). In addition, the adsorption-desorption isotherms of the four catalysts show an "adsorption-desorption loop", that is, a desorption hysteresis phenomenon, which further proves that the catalyst has capillary pores of different sizes and shapes. 2 CO 3 The catalyst prepared by using the solution as a precipitant When the pressure approaches 1, the adsorption amount increases sharply and capillary condensation occurs. 0 When , the adsorption line becomes steeper and the desorption line drops sharply, which is the characteristic of typical layered mesoporous materials.

[0084] like Figure 4 As shown, it shows the XRD phase analysis of the Cu-based metal oxide catalyst with a molar ratio of Mg:Al:Cu atoms of 12:4:3. Figure 4 The catalyst spectrum shows obvious characteristics: the peak is obviously wider, which can be judged as a crystalline substance; there are multiple independent narrow peaks (2Theta = 0.1° to 0.2°). The crystal particles in the sample should be microcrystals with a size of less than 300nm.

[0085] Figure 4 In a, four catalysts with the same ratio (the molar ratio of Mg:Al:Cu atoms is 12:4:3) were prepared with four different carbonate concentrations as precipitants. Through XRD comparison of the four catalysts, the peak of Gr-CuMgAl catalyst becomes sharper, indicating that the crystal form of the catalyst is relatively good. Figure 4 The physical phase of the Gr-CuMgAl catalyst in Figure b is mainly hydrated basic carbonate, indicating that the main form of metallic copper in the catalyst is Cu 2+ .

[0086] like Figure 5 As shown, it shows the SEM image of a Cu-based metal oxide catalyst (Gr-CuMgAl) with a molar ratio of Mg:Al:Cu atoms of 12:4:3. Under the scanning electron microscope, a lamellar structure is presented, similar to "cotton wool".

[0087] Table 2 Reaction of Gr-CuMgAl in methanol and 1,2-propylene glycol, where 7.5% and 15% represent the concentration of 1,2-propylene glycol in the total mixture of methanol and 1,2-propylene glycol (wt.%)

[0088]

[0089] From the results in Table 2, it can be concluded that the catalyst exhibits high activity for low and high concentrations of 1,2-propylene glycol. When other conditions remain unchanged, a hydrogen atmosphere of appropriate pressure is beneficial to the conversion of the reaction. A hydrogen atmosphere is beneficial to the formation of 1,2-butanediol, but the selectivity of 2,3-butanediol remains basically unchanged.

[0090] Example 2

[0091] The following preparation method is used to prepare the Cu-based metal oxide catalyst according to the present application:

[0092] (1) magnesium nitrate, zirconium oxynitrate and copper nitrate were prepared into a mixed aqueous solution according to a molar ratio of 12:5:3, and the molar concentrations thereof were 0.06 mol / L, 0.025 mol / L and 0.015 mol / L, respectively (the volume of the mixed solution was 150 mL);

[0093] (2) adding the mixed aqueous solution obtained in step (1) dropwise to a sodium carbonate aqueous solution (molar concentration of 0.133 mol / L) at 65° C., stirring while adding dropwise, then adding sodium hydroxide solution (1 mol / L) to adjust the pH value of the system to 10, then continuing to stir at room temperature for 1 hour, and standing for aging for 24 hours, then filtering, washing the precipitate to neutrality, and then drying the precipitate at 100° C. for 24 hours; and

[0094] (3) The product obtained in step (2) was heated to 500°C in a tube furnace and calcined in an air atmosphere for 7 hours to obtain a black solid. The solid was then reduced in a hydrogen atmosphere at 350°C for 3 hours to obtain a CuMgZr oxide catalyst.

[0095] The above catalyst is used to synthesize 2,3-butanediol:

[0096] Methanol (analytical grade) and 1,2-propylene glycol (analytical grade) are mixed to form a solution of a certain concentration, which is then put into a reactor, and the catalyst prepared by the above method is added, and the reactor is sealed. Then, the air in the intermittent high-pressure reactor is replaced with nitrogen or hydrogen (multiple times), and the reactor is placed in a thermocouple heating jacket for heating, and the reaction time is set to 3 to 5 hours. After the reaction is completed, it is cooled to room temperature, filtered through a 0.22μm filter membrane, and a sample is prepared. Since 2,3-butanediol has three stereoisomers, including one meso isomer, two peaks will appear through gas chromatography (GC-MS), and the product conversion rate and yield are calculated. The experimental conditions and results are shown in Table 2 below:

[0097] Table 3 Comparison of catalytic conditions and catalytic effects of CuMgZr catalyst with other catalysts

[0098]

[0099] like Figure 6 As shown, it shows the NH3-TPD of CuCaZr (Example 10), CuMgCaOx (Example 3-1), CuMgZr (Example 2) and CuMgAl (Example 1-1) catalysts prepared according to Example 2 of the present application. Among them, CuMgZr has a more obvious desorption peak below 200°C, indicating that there are weaker acid sites, CuMgZr and CuMgAl have wider desorption peaks at 350°C to 500°C, and CuMgCaOx has a smaller desorption peak at 200°C to 350°C, indicating the presence of medium-strong acid sites. In short, these four mixed metal oxides are acidic mesoporous solid catalysts.

[0100] Example 3-1

[0101] The following preparation method is used to prepare the Cu-based metal oxide catalyst according to the present application:

[0102] (1) preparing a mixed aqueous solution of magnesium nitrate, calcium nitrate and copper nitrate in a molar ratio of 12:8:3, with molar concentrations of 0.06 mol / L, 0.040 mol / L and 0.015 mol / L, respectively (the volume of the mixed solution is about 150 mL);

[0103] (2) adding the mixed aqueous solution obtained in step (1) dropwise to a sodium carbonate aqueous solution (molar concentration of 0.133 mol / L) at 65° C., stirring while adding dropwise, then adding sodium hydroxide solution (1 mol / L) to adjust the pH value of the system to 10, then continuing to stir at room temperature for 1 hour, and standing for aging for 24 hours, then filtering, washing the precipitate to neutrality, and then drying the precipitate at 100° C. for 24 hours; and

[0104] (3) The product obtained in step (2) was heated to 650°C in a tube furnace and calcined in an air atmosphere for 6 hours to obtain a black solid, and then reduced at 350°C in a hydrogen atmosphere for 3 hours to obtain CuMgCaO X Oxide catalysts.

[0105] The above catalyst is used to synthesize 2,3-butanediol:

[0106] Methanol (analytical grade) and 1,2-propylene glycol (analytical grade) are mixed to form a solution of a certain concentration, which is then put into a reactor, and the catalyst prepared by the above method is added, and the reactor is sealed. Then, the air in the intermittent high-pressure reactor is replaced with nitrogen or hydrogen (multiple times), and the reactor is placed in a thermocouple heating jacket for heating, and the reaction time is set to 3 to 5 hours. After the reaction is completed, it is cooled to room temperature, and a sample is taken through a 0.22μm filter membrane to prepare a sample. Since 2,3-butanediol has three stereoisomers, including one meso isomer, two peaks will appear through gas chromatography (GC-MS), and the product conversion rate and yield are calculated. The experimental conditions and results are shown in Table 4 below:

[0107] Table 4 Catalytic conditions and catalytic effects of CuMgCaOx catalyst

[0108]

[0109] From the results in Table 4, it can be seen that the CuMgCaOx catalyst has good activity in the reaction, especially in a hydrogen atmosphere, the selectivity is significantly improved, but the conversion rate is reduced. The concentration of the reactants, the reaction atmosphere and the pressure also have an effect on the reaction.

[0110] In addition, if Figure 8 As shown, it shows the SEM image of the Cu-based metal oxide catalyst with a molar ratio of Mg:Ca:Cu atoms of 12:8:3. Observing its morphology, it can be seen that it has "worm-like" channels, the channels are adhered, and the overall structure is a hollow lamellar structure.

[0111] Example 3-2

[0112] The Cu-based metal oxide catalyst according to the present application was prepared in the same manner as in Example 3-1 above, except that the molar ratio of Mg:Ca:Cu atoms was 3:1:1. The catalyst was used to synthesize 2,3-butanediol, and the experimental conditions and results are shown in Table 5 below:

[0113] Table 5 Catalytic effect of changing other CuMgCaOx catalytic conditions at the same raw material liquid concentration of 15% (wt.%)

[0114]

[0115] Table 6 Catalytic effect of changing other conditions of CuMgCaOx catalysis under the same raw material liquid concentration (7.5%wt.)

[0116]

[0117] It can be seen from the results in Tables 5 and 6 that, under the premise that the Mg content is higher than that of Cu and Ca, changing the catalyst ratio has little effect on its activity. The combination of catalyst properties and reaction conditions can effectively improve the activity of the catalyst.

[0118] Example 3-3

[0119] The Cu-based metal oxide catalyst according to the present application was prepared in the same manner as in Example 3-1 above, except that the molar ratio of Mg:Ca:Cu atoms was 12:8:3.

[0120] like Figure 7 As shown, it shows the XRD phase analysis of Cu-based metal oxide catalysts with a Mg:Ca:Cu molar ratio of 12:8:3. x The XRD phase diagram of the catalyst before use, and the three figures b, c, and d are XRD phase diagrams after 5h, 10h, and 20h of reaction, respectively. From the perspective of phase analysis, there are changes before and after the reaction, and the phase of the catalyst remains basically constant after 10h and 20h of reaction. The above shows that it is more appropriate to keep the reaction time at about 5h. After the reaction, the copper element of the catalyst mainly changes from the original oxidation state to the free state, which can be inferred that the valence state of the Cu element changes during the reaction.

[0121] Embodiment 3-4

[0122] The Cu-based metal oxide catalyst according to the present application was prepared in the same manner as in Example 3-1 above, except that the molar ratio of Mg:Ca:Cu atoms was 8:13:3. Figure 8 , which shows SEM images of the Cu-based metal oxide catalyst with a molar ratio of Mg:Ca:Cu atoms of 12:8:3 (upper row) prepared in Example 3-1 and a molar ratio of Mg:Ca:Cu atoms of 8:13:3 (lower row) prepared in this example. Fig. 9 CuMgCaO x TEM images (the molar ratio of Mg:Ca:Cu atoms is 12:8:3). The four images a, b, c, and d are the morphologies within different fields of view. The overall structure is relatively regular.

[0123] Table 7 Catalyst CuMgCaOx (Mg:Ca:Cu atomic molar ratio is 8:13:3)

[0124]

[0125] As can be seen from Table 7, the reaction data can determine that an important condition in the preparation process of this type of mixed metal oxide is that the Mg content must be greater than the Ca content, otherwise the conversion rate of the reaction raw materials will be affected.

[0126] By changing the Mg / Ca ratio, excessive Ca content affects the structure of the catalyst, while an appropriate content of Ca can, to a certain extent, help form a more regular structure.

[0127] Example 4

[0128] The following preparation method is used to prepare the Cu-based metal oxide catalyst according to the present application:

[0129] (1) magnesium nitrate, aluminum nitrate and copper nitrate were prepared into a mixed aqueous solution according to a molar ratio of 12:5:3, and the molar concentrations thereof were 0.06 mol / L, 0.025 mol / L and 0.015 mol / L, respectively (the volume of the mixed solution was about 150 mL);

[0130] (2) adding the mixed aqueous solution obtained in step (1) dropwise to a sodium carbonate aqueous solution (molar concentration of 0.40 mol / L, mass of 7.95 g, solution volume of about 187 mL) at 65° C., stirring while adding dropwise, then adding sodium hydroxide solution (1 mol / L) to adjust the pH value of the system to 10, then continuing to stir at room temperature for 1 hour, and standing for 24 hours, then filtering, washing the precipitate to neutrality, and then drying the precipitate at 100° C. for 24 hours; and

[0131] (3) The product obtained in step (2) was heated to 600° C. in a tube furnace and calcined in an air atmosphere for 6 hours to obtain a CuMgAl oxide catalyst.

[0132] The above catalyst is used to synthesize 2,3-butanediol:

[0133] 2 mL of 1,2-propylene glycol and 15 mL of methanol were added to an intermittent autoclave, and 0.2 g of the catalyst prepared by the above method was added, and the autoclave was sealed. Then, the air in the intermittent autoclave was replaced with hydrogen (multiple times), and then the reaction was carried out at a hydrogen pressure of 2 MPa and a temperature of 210° C. for 3 h. After the reaction was completed, the mixture was cooled to room temperature and filtered through a 0.22 μm filter membrane to prepare a sample. Since 2,3-butanediol has three stereoisomers, including one meso isomer, a qualitative analysis was performed by gas chromatography (GC-MS), and it was calculated that the conversion rate of 1,2-propylene glycol was close to 50.9%, and the selectivity of 2,3-butanediol was 54.9%.

[0134] Example 5

[0135] The following preparation method is used to prepare the Cu-based metal oxide catalyst according to the present application:

[0136] (1) magnesium nitrate, aluminum nitrate and copper nitrate are prepared into a mixed aqueous solution according to a molar ratio of 12:5:3, and the molar concentrations thereof are 0.06 mol / L, 0.025 mol / L and 0.015 mol / L, respectively (the volume of the mixed solution is about 150 mL);

[0137] (2) adding the sodium hydroxide solution (1 mol / L) obtained in step (1) dropwise to the mixed aqueous solution at 65° C., stirring while adding dropwise, and adjusting the pH value of the system to 10, then continuing to stir at room temperature for 1 hour, and standing for 24 hours, then filtering, washing the precipitate to neutrality, and then drying the precipitate at 100° C. for 24 hours; and

[0138] (3) The product obtained in step (2) was heated to 500° C. in a tube furnace and calcined in an air atmosphere for 6 hours to obtain a dark brown solid. The solid was then reduced in a hydrogen atmosphere at 400° C. for 3 hours to obtain a CuMgAl oxide catalyst.

[0139] The above catalyst is used to synthesize 2,3-butanediol:

[0140] 2 mL of 1,2-propylene glycol and 15 mL of methanol were added to an intermittent autoclave, 0.25 mL of the reaction intermediate hydroxyacetone was added as an initiator, and 0.2 g of the catalyst prepared by the above method was added, and the autoclave was sealed. Then, the air in the intermittent autoclave was replaced with hydrogen (multiple times), and then the reaction was carried out at a hydrogen pressure of 2 MPa and a temperature of 210° C. for 3 h. After the reaction was completed, the reaction was cooled to room temperature, and the sample was filtered through a 0.22 μm filter membrane to prepare a sample. Since 2,3-butanediol has three stereoisomers, including one meso isomer, it was qualitatively analyzed by gas chromatography (GC-MS), and the conversion rate of 1,2-propylene glycol was calculated to be close to 21.43%, and the selectivity of 2,3-butanediol was 75.6%.

[0141] Example 6

[0142] The following preparation method is used to prepare the Cu-based metal oxide catalyst according to the present application:

[0143] (1) preparing a mixed aqueous solution of magnesium nitrate, aluminum nitrate and copper nitrate in a molar ratio of 69:29:2, with molar concentrations of 0.069 mol / L, 0.029 mol / L and 0.02 mol / L, respectively (the volume of the mixed solution is about 150 mL);

[0144] (2) adding the mixed aqueous solution obtained in step (1) dropwise to a sodium carbonate aqueous solution (molar concentration of 0.133 mol / L) at 65° C., stirring while adding dropwise, then adding sodium hydroxide solution (1 mol / L) to adjust the pH value of the system to 10, then continuing to stir at room temperature for 1 hour, and standing for aging for 24 hours, then filtering, washing the precipitate to neutrality, and then drying the precipitate at 100° C. for 24 hours; and

[0145] (3) The product obtained in step (2) was heated to 600° C. in a tube furnace and calcined in an air atmosphere for 6 hours to obtain a dark brown solid. The solid was then reduced in a hydrogen atmosphere at 300° C. for 3 hours to obtain a CuMgAl oxide catalyst.

[0146] The above catalyst is used to synthesize 2,3-butanediol:

[0147] 2 mL of 1,2-propylene glycol and 15 mL of methanol were added to an intermittent autoclave, and 0.2 g of the catalyst prepared by the above method was added, and the autoclave was sealed. Then, the air in the intermittent autoclave was replaced with hydrogen (multiple times), and then the reaction was carried out at a hydrogen pressure of 2 MPa and a temperature of 210° C. for 3 h. After the reaction was completed, the mixture was cooled to room temperature and filtered through a 0.22 μm filter membrane to prepare a sample. Since 2,3-butanediol has three stereoisomers, including one meso isomer, it was qualitatively analyzed by gas chromatography (GC-MS), and the conversion rate of 1,2-propylene glycol was calculated to be close to 58.3%, and the selectivity of 2,3-butanediol was 78.8%.

[0148] Example 7

[0149] The following preparation method is used to prepare the Cu-based metal oxide catalyst according to the present application:

[0150] (1) preparing a mixed aqueous solution of magnesium nitrate, aluminum nitrate and copper nitrate in a molar ratio of 12:4:3, with molar concentrations of 0.06 mol / L, 0.02 mol / L and 0.015 mol / L, respectively (the volume of the mixed solution is about 150 mL);

[0151] (2) adding the mixed aqueous solution obtained in step (1) dropwise to a sodium carbonate aqueous solution (molar concentration of 0.133 mol / L) at 65° C., stirring while adding dropwise, then adding sodium hydroxide solution (1 mol / L) to adjust the pH value of the system to 10, then continuing to stir at room temperature for 1 hour, and standing for aging for 24 hours, then filtering, washing the precipitate to neutrality, and then drying the precipitate at 100° C. for 24 hours; and

[0152] (3) The product obtained in step (2) was heated to 426° C. in a tube furnace and calcined in an air atmosphere for 12 hours to obtain a CuMgAl oxide catalyst.

[0153] The above catalyst is used to synthesize 2,3-butanediol:

[0154] 2 mL of 1,2-propylene glycol and 15 mL of methanol were added to an intermittent autoclave, and 0.2 g of the catalyst prepared by the above method was added, and the autoclave was sealed. Then, the air in the intermittent autoclave was replaced with hydrogen (multiple times), and then the reaction was carried out at a hydrogen pressure of 2 MPa and a temperature of 210° C. for 3 h. After the reaction was completed, the reaction was cooled to room temperature and filtered through a 0.22 μm filter membrane to prepare a sample. 2,3-butanediol has three stereoisomers, including one meso isomer. A qualitative analysis was performed by gas chromatography (GC-MS), and the conversion rate of 1,2-propylene glycol was calculated to be close to 57.74%, and the selectivity of 2,3-butanediol was 70.8%.

[0155] Example 8

[0156] The following preparation method is used to prepare the Cu-based metal oxide catalyst according to the present application:

[0157] (1) preparing a mixed aqueous solution of magnesium nitrate, aluminum nitrate and copper nitrate in a molar ratio of 20:13:5, with molar concentrations of 0.06 mol / L, 0.039 mol / L and 0.015 mol / L, respectively (the volume of the mixed solution is about 150 mL);

[0158] (2) adding the mixed aqueous solution obtained in step (1) dropwise to a sodium carbonate aqueous solution (molar concentration of 0.133 mol / L) at 65° C., stirring while adding dropwise, then adding sodium hydroxide solution (1 mol / L) to adjust the pH value of the system to 10, then continuing to stir at room temperature for 1 hour, and standing for aging for 24 hours, then filtering, washing the precipitate to neutrality, and then drying the precipitate at 100° C. for 24 hours; and

[0159] (3) The product obtained in step (2) was heated to 550° C. in a tube furnace and calcined in an air atmosphere for 6 hours to obtain a dark brown solid. The solid was then reduced in a hydrogen atmosphere at 350° C. for 3 hours to obtain a CuMgAl oxide catalyst.

[0160] The above catalyst is used to synthesize 2,3-butanediol:

[0161] 2 mL of 1,2-propylene glycol and 15 mL of methanol were added to an intermittent autoclave, and 0.2 g of the catalyst prepared by the above method was added, and the autoclave was sealed. Then, the air in the intermittent autoclave was replaced with hydrogen (multiple times), and then the reaction was carried out at a hydrogen pressure of 2 MPa and a temperature of 210° C. for 3 h. After the reaction was completed, the mixture was cooled to room temperature and filtered through a 0.22 μm filter membrane to prepare a sample. Since 2,3-butanediol has three stereoisomers, including one meso isomer, a qualitative analysis was performed by gas chromatography (GC-MS), and the conversion rate of 1,2-propylene glycol was calculated to be close to 42.99%, and the selectivity of 2,3-butanediol was 58.5%.

[0162] Example 9

[0163] The following preparation method is used to prepare the Cu-based metal oxide catalyst according to the present application:

[0164] (1) preparing a mixed aqueous solution of magnesium nitrate, aluminum nitrate and copper nitrate in a molar ratio of 20:13:5, with molar concentrations of 0.06 mol / L, 0.039 mol / L and 0.015 mol / L, respectively (the volume of the mixed solution is about 150 mL);

[0165] (2) adding the mixed aqueous solution obtained in step (1) dropwise to a sodium carbonate aqueous solution (molar concentration of 0.40 mol / L) at 65° C., stirring while adding dropwise, then adding sodium hydroxide solution (1 mol / L) to adjust the pH value of the system to 10, then continuing to stir at room temperature for 1 hour, and standing for 24 hours, then filtering, washing the precipitate to neutrality, and then drying the precipitate at 100° C. for 24 hours; and

[0166] (3) The product obtained in step (2) was heated to 550° C. in a tube furnace and calcined in an air atmosphere for 6 hours to obtain a dark brown solid. The solid was then reduced in a hydrogen atmosphere at 350° C. for 3 hours to obtain a CuMgAl oxide catalyst.

[0167] The above catalyst is used to synthesize 2,3-butanediol:

[0168] 2 mL of 1,2-propylene glycol and 15 mL of methanol were added to an intermittent autoclave, 0.05 mL of the reaction intermediate formaldehyde was added as an initiator, and 0.2 g of the catalyst prepared by the above method was added, and the autoclave was sealed. Then, the air in the intermittent autoclave was replaced with hydrogen (multiple times), and then the reaction was carried out at a hydrogen pressure of 2 MPa and a temperature of 210° C. for 3 h. After the reaction was completed, the reaction was cooled to room temperature, and the sample was filtered through a 0.22 μm filter membrane to prepare a sample. Since 2,3-butanediol has three stereoisomers, including one meso isomer, it was qualitatively analyzed by gas chromatography (GC-MS), and the conversion rate of 1,2-propylene glycol was calculated to be close to 21.24%, and the selectivity of 2,3-butanediol was 78.19%.

[0169] Example 10

[0170] The following preparation method is used to prepare the Cu-based metal oxide catalyst according to the present application:

[0171] (1) preparing a mixed aqueous solution of calcium nitrate, zirconium oxynitrate and copper nitrate in a molar ratio of 6:2:1, wherein the molar concentrations thereof are 0.06 mol / L, 0.02 mol / L and 0.01 mol / L, respectively (the volume of the mixed solution is about 150 mL);

[0172] (2) adding the mixed aqueous solution obtained in step (1) dropwise to a sodium carbonate aqueous solution at 65° C. to obtain a carbonate molar concentration of 0.53 mol / L (10.6 g Na 2 CO 3 , solution volume is about 187mL), calcium molar concentration is 0.06mol / L, zirconium molar concentration is 0.02mol / L and copper molar concentration is 0.01mol / L, adding dropwise while stirring, then adding sodium hydroxide solution (1mol / L) to adjust the system pH value to 10, then continuing stirring at room temperature for 1 hour, and standing for aging for 24 hours, then filtering, washing the precipitate to neutrality, and then drying the precipitate at 100°C for 24 hours; and

[0173] (3) The product obtained in step (2) was heated to 550° C. in a tube furnace and calcined in an air atmosphere for 6 hours. The obtained solid was then reduced in a hydrogen atmosphere at 350° C. for 3 hours to obtain a CuCaZr oxide catalyst.

[0174] The above catalyst is used to synthesize 2,3-butanediol:

[0175] 2 mL of 1,2-propylene glycol and 15 mL of methanol were added to an intermittent autoclave, 0.02 mL of the reaction intermediate hydroxyacetone was added as an initiator, and 0.2 g of the catalyst prepared by the above method was added, and the autoclave was sealed. Then, the air in the intermittent autoclave was replaced with hydrogen (multiple times), and then the reaction was carried out at a hydrogen pressure of 2 MPa and a temperature of 210° C. for 3 h. After the reaction was completed, the reaction was cooled to room temperature, and the sample was filtered through a 0.22 μm filter membrane to prepare a sample. Since 2,3-butanediol has three stereoisomers, including one meso isomer, it was qualitatively analyzed by gas chromatography (GC-MS), and the conversion rate of 1,2-propylene glycol was calculated to be close to 39.1%, and the selectivity of 2,3-butanediol was 58.16%.

[0176] The above-mentioned specific embodiments of the present application are merely preferred embodiments for explaining the present application, and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications without creative contribution as needed. However, any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.

Claims

1. A Cu-based metal oxide catalyst for catalyzing the condensation of methanol and 1,2-propylene glycol to synthesize 2,3-butanediol, characterized in that: The preparation method of the Cu-based metal oxide catalyst comprises the following steps: (1) preparing a mixed aqueous solution of a copper salt, a magnesium salt or a calcium salt, and a first metal A salt, wherein the first metal A salt is at least one selected from a Ca salt, an Al salt, and a Zr salt; wherein the molar ratio of Mg or Ca to A is 1.4 to 6, and the molar content of Cu is 2% to 60% of the total molar amount of all metal ions, wherein when a copper salt and a magnesium salt are used, the first metal A salt is at least one selected from a Ca salt, an Al salt, and a Zr salt, and when a copper salt and a calcium salt are used, the first metal A salt is at least one selected from an Al salt and a Zr salt; (2) adding the mixed aqueous solution of metal salts prepared in step (1) dropwise to a carbonate aqueous solution or an alkaline solution at 60° C. to 70° C., then adding an alkaline solution dropwise to adjust the pH value of the system to 9.5 to 10.5, then continuing to stir at room temperature for 1 to 5 hours, and standing for aging for 18 to 30 hours, then filtering and washing to neutrality, and drying at 100° C. to 120° C. for 12 to 24 hours, wherein the mixed aqueous solution of metal salts is added dropwise to the carbonate aqueous solution so that the molar concentration of carbonate in the system is 0.5 to 10 times the total molar concentration of metal ions; and (3) calcining the product obtained in step (2) at a temperature of 500° C. to 600° C. in an air atmosphere for 3 to 12 hours to obtain the Cu-based metal oxide catalyst Cu y Mg m A n O x or Cu y Ca m A n O x , where the ratio of m / n is 1.4~6, y / (m+n+y) is 0.02~0.6, and x is the chemical oxygen demand of the stoichiometric ratio.

2. The use according to claim 1, characterized in that In the step (2), the pH value of the system is adjusted to 10.

3. The use according to claim 1, characterized in that In the step (2), the mixture is allowed to stand for 24 hours.

4. The use according to claim 1, characterized in that The copper salt, the magnesium salt or the calcium salt and the first metal A salt are nitrates.

5. The use according to claim 1, characterized in that: The preparation process of step (1) is carried out at 60°C to 70°C.

6. The use according to claim 1, characterized in that: In the step (2), the carbonate in the carbonate aqueous solution is at least one selected from sodium carbonate or potassium carbonate.

7. The use according to claim 6, characterized in that The carbonate in the carbonate aqueous solution is sodium carbonate.

8. The use according to claim 1, characterized in that In the step (2), the alkali in the alkaline solution is at least one selected from sodium hydroxide or potassium hydroxide.

9. The use according to claim 8, characterized in that The alkali in the alkali solution is sodium hydroxide.

10. The use according to claim 1, characterized in that In the step (2), the OH in the alkaline solution - The molar concentration of the ions is 1 to 10 times the total molar concentration of the metal ions in the mixed aqueous solution.

11. The use according to claim 1, characterized in that Also includes: In step (3), the calcined product is reduced in a hydrogen atmosphere at 300° C. to 400° C. for 2.5 to 3.5 hours to obtain the Cu-based metal oxide catalyst.

12. The use according to claim 11, characterized in that In step (3), the calcined product is reduced in a hydrogen atmosphere for 3 hours.

13. The use according to any one of claims 1 to 12, wherein the Cu-based metal oxide catalyst catalyzes the condensation of methanol and 1,2-propylene glycol to synthesize 2,3-butanediol, comprising: In the presence of the Cu-based metal oxide catalyst and in a hydrogen atmosphere, methanol and 1,2-propylene glycol are subjected to an intermittent high-pressure reaction for 3 to 5 hours at a gas pressure of 1 MPa to 3 MPa and a reaction temperature of 190° C. to 210° C. to obtain 2,3-butanediol.

14. The use according to claim 13, characterized in that The weight of 1,2-propylene glycol accounts for 2.5% to 35% of the total weight of the mixture of methanol and 1,2-propylene glycol.

15. The use according to claim 14, characterized in that The weight of 1,2-propylene glycol accounts for 7.5% to 15% of the total weight of the mixture of methanol and 1,2-propylene glycol.

16. The use according to claim 13, characterized in that The reaction temperature is 210°C.