Aramid coated diaphragm and preparation method thereof
Through the wet preparation method, the production process of aramid-coated diaphragm is simplified, the efficiency and tensile strength are improved, the problems of high equipment investment and insufficient safety in the existing process are solved, and efficient and safe aramid coating is achieved Laminate production.
Patent Information
- Application Number
- CN202210268442.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-17
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-03-17
AI Technical Summary
The existing aramid-coated diaphragm preparation process is complicated, resulting in high equipment investment and low production efficiency. The ceramic coating film is easily damaged in high temperature environments and lacks safety.
By using the wet preparation method, the polyolefin composition is melt-extruded, filtered, cooled the casting sheet, bidirectional stretching, and after edge cutting, coated aramid slurry, extracted and dried, and finally lateral stretching is performed to achieve one-time molding. Aramid coated diaphragm production.
The production efficiency of the coating film is improved, the equipment cost is reduced, and the prepared aramid coating has higher tensile strength and thermal stability, improving safety performance.
Smart Images

Figure CN114597587B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and more specifically, relates to a method for preparing an aramid coated diaphragm by a wet process, and the aramid coated diaphragm prepared by the method. Background Art
[0002] With the development of the new energy market, power vehicles are paying more and more attention to indicators such as safety and cruising range. From the perspective of safety, the diaphragm requires higher puncture strength, low closed-cell temperature and high membrane rupture temperature, while the cruising range requires improving the energy density of the power battery, which requires the diaphragm to be thinner and the coating to be lighter.
[0003] At present, the existing separators on the market can meet the conventional performance requirements of lithium-ion batteries, but in high temperature environments, the base film is prone to large-scale thermal shrinkage. Although the ceramic coating film has high thermal stability, once punctured, the hole will expand rapidly, causing a short circuit between the positive and negative electrodes, resulting in safety accidents. In addition, the energy density of domestic power lithium batteries is still relatively low, which restricts the range of new energy vehicles.
[0004] Aramid has gained widespread attention from people in the diaphragm industry because of its excellent high temperature resistance, mechanical properties, flame retardancy, chemical corrosion resistance and light weight. The lithium-ion battery diaphragm obtained using aramid as a coating material has good thermal stability and low surface density, which can effectively solve the safety and energy density problems of power batteries.
[0005] The existing aramid coated diaphragm needs to prepare a microporous base membrane first, and then coat the microporous base membrane with aramid slurry to form a coating layer. The process mainly includes: first feeding polyolefin powder and additives, melt extrusion, casting, stretching, extraction, stretching, winding, and slitting to form a microporous base membrane; before coating the aramid slurry, the microporous base membrane needs to be unwound, pretreated, and then coated, extracted, washed, dried, and heat-set. The preparation process has cumbersome steps, resulting in excessive investment in equipment and low production efficiency of the coated diaphragm. In response to these problems, it is urgent to develop a new preparation process for aramid coated diaphragms. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing an aramid coated diaphragm by a wet process, and an aramid coated diaphragm prepared by the method. The method provided by the present invention can improve the production efficiency of the coated film and reduce equipment investment.
[0007] In a first aspect, the present invention provides a method for preparing an aramid coated diaphragm by a wet process, comprising:
[0008] (1) melt-extruding, filtering, and extrusion-plasticizing a polyolefin composition to obtain a sheet-like substrate; wherein the polyolefin composition comprises a polyolefin resin, a pore-forming agent, and an antioxidant;
[0009] (2) cooling the flaky substrate casting;
[0010] (3) biaxially stretching the cooled substrate and trimming the edges to obtain a thick film;
[0011] (4) coating the aramid slurry on the thick film;
[0012] (5) extracting and drying the coated thick film;
[0013] (6) The dried thick film is stretched transversely.
[0014] In a second aspect, the present invention provides an aramid coated diaphragm prepared by the method described in the first aspect of the present invention.
[0015] Compared with the existing preparation process, the method provided by the present invention has the following advantages:
[0016] 1) Effectively improve coating capacity: directly introduce the coating process into the production process of the base film, and form it in one step; the existing process adopts a two-step method, that is, prepare the microporous base film separately, and then use a coating machine to coat the microporous base film. Compared with the two-step method, the method of the present invention can achieve coating on a wider base film, which is more than several times the effective width of the conventional coating machine;
[0017] 2) Reducing the cost of investment equipment: The method of the present invention effectively combines the base film preparation and the aramid coating process, which can reduce related processes such as base film extraction and base film unwinding, and significantly reduce the cost investment of related equipment.
[0018] In addition, the aramid coating film prepared by the method of the present invention has higher tensile strength than the aramid coating film prepared by the existing two-step method.
[0019] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Exemplary embodiments of the present invention will be described in more detail with reference to the accompanying drawings.
[0021] Figure 1 It is a schematic structural diagram of a coating device according to one embodiment of the present invention.
[0022] Figure 2 The present invention is a process flow chart of wet preparation of aramid coated diaphragm according to one embodiment of the present invention.
[0023] Figure 3 The present invention is a process flow chart of an existing base film production process.
[0024] Figure 4The present invention is a process flow chart of preparing an aramid coated diaphragm by coating a slurry on a base membrane.
[0025] Description of Reference Numerals
[0026] 1: thick film; 2: first transmission guide roller; 3: second transmission guide roller; 4: third transmission guide roller; 5: de-oiling pressure roller; 6: backing roller; 7: narrow slit die head; 8: feed pipe. DETAILED DESCRIPTION
[0027] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0028] In a first aspect, the present invention provides a method for preparing an aramid coated diaphragm by a wet process, comprising:
[0029] (1) melt-extruding, filtering, and extrusion-plasticizing a polyolefin composition to obtain a sheet-like substrate; wherein the polyolefin composition comprises a polyolefin resin, a pore-forming agent, and an antioxidant;
[0030] (2) cooling the flaky substrate casting;
[0031] (3) biaxially stretching the cooled substrate and trimming the edges to obtain a thick film;
[0032] (4) coating the aramid slurry on the thick film;
[0033] (5) extracting and drying the coated thick film;
[0034] (6) The dried thick film is stretched transversely.
[0035] In the present invention, the polyolefin composition comprises a polyolefin resin, a pore former and an antioxidant.
[0036] The polyolefin resin may be selected from polyethylene and polypropylene. Preferably, the polyolefin resin is ultra high molecular weight polyethylene (UHMWPE).
[0037] The pore-forming agent can be selected from liquid or solid hydrocarbons that can form a homogeneous mixture with the polyolefin resin above the melting point, such as white oil, paraffin oil, etc. Preferably, the pore-forming agent is paraffin oil. The viscosity of the paraffin oil can be 30-70 mm 2 / s.
[0038] The antioxidant can improve the thermal stability of the polyolefin resin. The antioxidant can be selected from pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1010) and tris(2,4-di-tert-butylphenyl) phosphite (antioxidant 168), preferably antioxidant 1010.
[0039] In one embodiment, the mass ratio of the polyolefin resin to the pore-forming agent is 1:(2-5), and the content of the antioxidant is 0.1-0.5 wt % based on the total weight of the polyolefin resin and the pore-forming agent.
[0040] The method provided by the present invention belongs to a process for wet-process production of aramid coated diaphragms. Unless otherwise specified (such as degreasing device), the present invention can be implemented on an existing wet-process stretching production line. The production line generally includes: a feeding and batching unit, an extrusion mixing unit, a casting cooling unit, a biaxial stretching unit, a winding unit, and a slitting unit. The specific configuration is well known in the art. The supporting equipment of the wet-process diaphragm production line can be purchased from Isotope of France, Toshiba of Japan, Japan Steel Works, Bruckner of Germany, and Sino-Science Hualian of China.
[0041] According to one embodiment, the feeding and batching unit includes a metering system, a twin-screw extruder with multiple refueling ports, a gear pump, a filtering device and a mold. Step (1) includes: adding a polyolefin resin (powder) and an antioxidant into a twin-screw extruder, adding a pore-forming agent into the twin-screw extruder from a refueling port set on the twin-screw extruder, melt-extruding to a gear pump, extruding to a filtering device; and then extruding to a mold to form a sheet substrate. The melt extrusion can fully mix the components in the polyolefin composition, which can improve the stability of the subsequent extrusion process. Preferably, the conditions for the melt extrusion include: a temperature of 160-200°C and a rotation speed of 40-70rpm. The gear pump can reduce the shear and residence time of the material in the extruder, and the rotation speed of the gear pump can be 70-100rpm. The filtering device can remove impurities in the melt and improve the uniformity of the melt. According to a preferred embodiment, the conditions for extruding to the filtering device include: a pressure of 3-7MPa and a temperature of 200-230°C. The conditions for extrusion to the die include: a pressure of 2-5 MPa and a temperature of 220-240°C.
[0042] According to the present invention, in step (2), the polyolefin composition melt can be quenched by cooling the casting sheet, so that the pore former and the polyolefin undergo thermotropic phase separation, and most of the pore former is locked in the thick sheet. Preferably, the sheet substrate is cooled to 8-15°C by using a cooling casting machine.
[0043] According to the present invention, step (3) comprises: the cooled sheet substrate enters a biaxial stretching unit, and is sequentially preheated, biaxially stretched, shaped, cooled, and then trimmed by a traction machine. Biaxial stretching can orient the molecular chains of the polyolefin in both the longitudinal and transverse directions, and the pore-forming agent is evenly distributed in the polyolefin. In a preferred embodiment, the transverse stretching ratio is 5-9, and the longitudinal stretching ratio is 5-9 (such as the transverse and longitudinal stretching ratios are both 7); the preheating temperature is 100-130°C (such as 122°C), and the wind speed is 15-30m / s (such as 25m / s); the stretching temperature is 100-130°C (such as 119°C), and the wind speed is 15-30m / s (such as 28m / s); the shaping temperature is 110-130°C (such as 117°C), and the wind speed is 15-30m / s (such as 22m / s); the cooling temperature is 15-40°C (such as 30°C), and the wind speed is 15-30m / s (such as 25m / s).
[0044] According to the present invention, step (4) is preferably carried out in a coating device. The coating device comprises: a tension-breaking mechanism, an oil removal mechanism and a coating mechanism. Figure 1 As shown, the tension-breaking mechanism comprises a first transmission guide roller 2 and a second transmission guide roller 3; the coating mechanism comprises a backing roller 6, a narrow slot die head 7 and a feed pipe 8; wherein the second transmission guide roller 3 is arranged above the first transmission guide roller 2, and the narrow slot die head 7 is arranged above the backing roller 6. The thick film 1 is transferred to the second transmission guide roller 3 along the first transmission guide roller 2, and is transferred successively through the degreasing mechanism and the backing roller 6. During the transfer process, after part of the pore-forming agent is removed by the degreasing mechanism, the feed pipe 8 injects the aramid slurry into the narrow slot die head 7, so that the aramid slurry is coated on the thick film 1. According to a preferred embodiment, the degreasing mechanism comprises a third transmission guide roller 4 and a degreasing pressure roller 5, wherein the third transmission guide roller 4 is located below the degreasing pressure roller 5, and the tops of the second transmission guide roller 3, the third transmission guide roller 4 and the backing roller 6 are located on the same horizontal line. In this embodiment, the thick film 1 is transferred along the first transmission guide roller 2 to the second transmission guide roller 3, and is transferred in sequence through the third transmission guide roller 4 and the back roller 6. During the transfer process, the de-oiling pressure roller 5 applies pressure (e.g., 1-100N) to remove part of the pore-forming agent. After the aramid slurry is injected into the narrow slit die 7 through the feed pipe 8, the aramid slurry is coated on the thick film 1 through the die lip of the narrow slit die 7, and then transferred to the extraction and washing unit through the back roller 6. The de-oiling pressure roller 5 is provided with a cylinder to provide contact extrusion force. The de-oiling pressure roller 5 removes excess pore-forming agent in the thick film 1 (oil film) under the joint action of the third transmission guide roller 4, so as to avoid the aramid coating being directly coated on the pore-forming agent due to the adhesion of the pore-forming agent. According to another embodiment, the de-oiling mechanism includes two vacuum adsorption rollers, and the two vacuum adsorption rollers are respectively replaced. Figure 1The third transmission guide roller 4 and the oil removal pressure roller 5 shown absorb the pore former on the membrane through negative pressure.
[0045] According to one embodiment, the aramid slurry comprises an aramid stock solution and ceramic powder. Preferably, the aramid stock solution is a para-aromatic polyamide stock solution, and the para-aromatic polyamide content in the stock solution is 1-5% by weight. The median particle size (D50) of the ceramic powder is 100-500nm. The solvent in the aramid stock solution can be selected from at least one of N-methylpyrrolidone (NMP), dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide (DMAC), tetramethylurea and acetone, preferably selected from N-methylpyrrolidone or N,N-dimethylacetamide.
[0046] Preferably, based on the total weight of the aramid slurry, the content of the para-aromatic polyamide is 0.9-5% by weight, and the content of the ceramic powder is 1-10% by weight.
[0047] According to the present invention, the extraction in step (5) is carried out in an extraction device. The extractant can be an oily solvent, for example, one or more selected from dichloromethane, chloroform, 1,1,1-trichloroethane, hydrofluoroether, hydrofluorocarbon, pentane, hexane, heptane, methanol, ethanol, isopropanol, tripropylene glycol, acetone, methyl ethyl ketone, N-methylpyrrolidone, ether, tetrahydrofuran, 1,4-dioxane, N,N-dimethylformamide, N,N-dimethylacetamide, toluene and xylene; preferably dichloromethane, or a combination of dichloromethane and the above-mentioned other oily solvents (such as NMP or DMAC). Compared with the existing aramid coating film extraction with water, dichloromethane is more easily volatilized by heat, which can reduce the drying temperature and save energy consumption. Dichloromethane can be used as an extractant for the base film (a film formed by a polyolefin composition). Using the base film extractant, mixed extraction can be directly carried out without introducing other substances.
[0048] According to a preferred embodiment, the extraction device comprises 3-9 extraction tanks (eg, 5, 7 or 8). The extractant in each extraction tank is dichloromethane.
[0049] According to another preferred embodiment, the extraction device comprises 3-9 extraction tanks (e.g., 5, 7 or 8). According to the transmission direction of the thick film, the first two extraction tanks comprise an extractant with a concentration gradient, and the extractant in the remaining extraction tanks is dichloromethane. The extractant with a concentration gradient is selected from dichloromethane and NMP. More preferably, the volume concentration of NMP in the first extraction tank is 35-80%, and the volume concentration of NMP in the second extraction tank is 40-60% of the volume concentration of NMP in the first extraction tank.
[0050] According to one embodiment, the extraction tank device also includes an injection pump and an overflow drainage pump. The extraction tank can adopt an overflow liquid addition method. According to the flow direction of the thick film, the injection and liquid replenishment ports are arranged in the last extraction tank, and an overflow tank is arranged in the first extraction tank. Both are provided with liquid level control. The injection pump or the overflow drainage pump is controlled to start and stop according to the overflow liquid level height of the last extraction tank and the first extraction tank.
[0051] In step (5), the drying temperature may be 40-60° C. Through extraction and drying, coating micropores are formed.
[0052] Optionally, the method of the present invention further comprises: sending the extraction mixed liquid obtained after the extraction in step (5) to a recovery collection tank for recovery.
[0053] According to the present invention, step (6) includes: the dried thick film enters the transverse stretching heat treatment unit, undergoes preheating, transverse stretching, shrinkage, first shaping (transverse expansion), and then transverse and longitudinal shrinkage and second shaping (micro-shrinkage). Preferably, in the transverse expansion, the transverse stretching ratio is 1.1-2 times; the preheating temperature is 110-140°C (such as 127°C), and the wind speed is 15-30m / s (such as 25m / s); the stretching temperature is 110-140°C (such as 125°C), and the wind speed is 15-30m / s (such as 28m / s); the shrinking temperature is 110-140°C (such as 128°C), and the wind speed is 15-30m / s (such as 28m / s); the first shaping temperature is 110-140°C (such as 135°C), and the wind speed is 15-30m / s (such as 22m / s). In the micro-shrinkage, the shrinkage rate in the transverse direction (TD) is 1-10%, the shrinkage rate in the longitudinal direction (MD) is 1-10%, and the second setting temperature is 110-140° C. (such as 130° C.).
[0054] According to a more specific implementation, Figure 2 As shown, the method of the present invention comprises the following process:
[0055] S1: Feeding and extrusion
[0056] The polyethylene powder and the antioxidant are added into the twin-screw extruder through the metering system, the pore-forming agent is added into the twin-screw extruder through the metering pump from the multiple refueling ports set on the twin-screw extruder at the set temperature, and is melted and extruded to the gear pump at the set temperature and speed; extruded to the filtering device at a certain pressure and temperature; and extruded to the mold to form a sheet substrate at a certain pressure and temperature.
[0057] S2: Casting, double drawing
[0058] The sheet substrate is cooled by a cooling casting machine, and the cooled sheet enters a bidirectional synchronous stretching unit, and is made into a thick film of required thickness and width under set temperature and wind speed conditions through preheating, stretching, shaping, cooling and other steps.
[0059] S3: Coating
[0060] The thick film enters after being cut by the traction machine Figure 1 In the coating device shown in the figure, specifically, the thick film 1 is firstly driven in an "S" shape by the first transmission guide roller 2 and the second transmission guide roller 3 to cut off the tension, and then the excess pore-forming agent on the surface of the thick film is removed by the third transmission guide roller 4 and the oil removal pressure roller 5, and the feed conduit 8 injects the aramid slurry into the narrow slit die head 7, and the aramid slurry is coated on the thick film 1 through the die lip, and then transmitted to the extraction and washing unit through the backing roller 6.
[0061] S4: Extraction
[0062] The coated thick film enters the extraction tank filled with extractant to extract the pore-forming agent in the oil film and the solvent in the slurry. The extraction tank device adopts a modular type, including n (n is an integer selected from 3-9) extraction tanks, which are recorded as 1# to n# extraction tanks according to the transmission direction of the thick film. The n#→1# extraction tank adopts an overflow liquid addition method, and the injection and replenishment ports are set in the n# tank to add the extractant; an overflow tank is set in the 1# tank, and each extraction tank is equipped with a liquid level control. The injection pump or the overflow drainage pump is controlled to start and stop according to the overflow liquid level height of the n# tank and the 1# tank, and the overflow drainage is sent to the subsequent liquid phase recovery device (including the recovery collection tank) for treatment. The flow rate of the circulation pump of each tank is set to 30-50m 3 / h, the oil film in the extraction tank is continuously cleaned through a "W"-shaped path, the extraction mixture flows out through the 1# tank to the recovery collection tank, and the thick film after extraction is dried.
[0063] S5: Horizontal pull
[0064] The dried thick film enters the transverse stretching heat treatment unit and undergoes preheating, stretching, shrinking, shaping and other steps. It undergoes a slight transverse expansion under the set temperature and wind speed conditions, and then undergoes a slight transverse and longitudinal shrinkage and shaping to obtain a microporous membrane (thin film).
[0065] S6: Winding and slitting
[0066] The film is trimmed by a traction machine and then rolled up at low tension, and then slit by a slitting machine.
[0067] Unless otherwise stated, Figure 2 The process shown is carried out on the lithium battery separator production line in Iseop, France.
[0068] In a second aspect, the present invention provides an aramid coated diaphragm prepared by the method of the first aspect of the present invention. In the method of the present invention, the aramid is stretched twice together with the thick film, so that the orientation of the aramid fiber after stretching is more consistent, and the aramid coated diaphragm has higher tensile strength.
[0069] The present invention will be further described below in conjunction with embodiments, but the scope of the present invention is not limited to these embodiments.
[0070] In the following embodiments and comparative examples, the polyethylene powder is ultra-high molecular weight polyethylene (UHMWPE), purchased from Celanese with the brand name GUR2122; the paraffin oil is No. 45, purchased from Zhejiang Zhengxin; the antioxidant is antioxidant 1010, purchased from BASF; the aramid stock solution is purchased from Zhonglan Chenguang Chemical Design Institute Co., Ltd. with the brand name T3 (para-aromatic polyamide stock solution, polymer content is 3% by weight, solvent is NMP); the ceramic powder (D50=400nm) is purchased from Suzhou Jinyi New Material Technology Co., Ltd.
[0071] The preparation method of the aramid slurry is as follows: ceramic powder (5 parts by weight) is added into aramid stock solution (95 parts by weight) for high-speed dispersion, and the dispersed mixed solution is filtered (400# filter screen) to obtain the aramid slurry.
[0072] Comparative Example 1
[0073] (1) Base film production process
[0074] Reference Figure 3 The process shown produces the base film.
[0075] 1) Feeding and extrusion
[0076] Polyethylene powder (25 parts by weight) and antioxidant (0.3 parts by weight) are added into a twin-screw extruder through a metering system, paraffin oil (75 parts by weight) is simultaneously added into the twin-screw extruder through a metering pump at a set temperature (110° C.) from a plurality of oil filling ports set on the twin-screw extruder (70% at the first oil filling port, 20% at the second oil filling port, and 10% at the third oil filling port), and melt-extruded to a gear pump at a set temperature and rotation speed (180° C., 60 rpm), with the gear pump rotating speed (85 rpm); extruded to a filtering device at a pressure of 5.5 MPa and a temperature of 215° C., and then extruded to a mold at a pressure of 4 MPa and a temperature of 225° C. to form a sheet substrate.
[0077] 2) Casting, double drawing
[0078] The sheet substrate was cooled to 12°C by a cooling casting machine. The cooled sheet (thickness 1300μm, width 650mm) entered the biaxial synchronous stretching unit (biaxial stretching ratio was 7 times), and was preheated, biaxially stretched, shaped, and cooled (preheated at 122°C, wind speed 25m / s; stretched at 119°C, wind speed 28m / s; shaped at 117°C, wind speed 22m / s; cooled at 30°C, wind speed 25m / s) to form a thick film with a thickness of 30μm and a width of 4550mm.
[0079] 3) Extraction
[0080] The thick film is trimmed by a traction machine (thickness 30μrn, width 4300mm), and then enters an extraction tank filled with dichloromethane (including 8 extraction tanks from 1# to 8#) to extract the paraffin oil in the film. The 8# to 1# extraction tank adopts overflow liquid addition, and the injection and replenishment ports are set in the 8# tank. The overflow tank is set in the 1# tank. Both are equipped with liquid level control. The injection pump or overflow drainage pump is controlled to start and stop according to the overflow liquid level height of the 8# tank and the 1# tank. The overflow drainage is treated by the subsequent liquid phase recovery device. The flow rate of the circulation pump of each tank is set to 35m 3 / h, the oil film in the extraction tank is continuously cleaned through a "W"-shaped path, the extraction mixture flows out through the 1# tank to the recovery collection tank, and the film is dried at 45°C.
[0081] 4) Horizontal pull
[0082] The dried film (thickness 12μm, width 3150mm) enters the transverse stretching heat treatment unit and undergoes preheating, stretching, shrinking, first shaping and other steps. Under the set temperature and wind speed conditions (preheating 127℃, wind speed 25m / s; stretching 125℃, wind speed 28m / s; shrinking 128℃, wind speed 28m / s; first shaping 135℃, wind speed 22m / s), a slight transverse expansion (stretching ratio 1.5 times) is carried out, and then a slight transverse and longitudinal shrinkage (TD direction, shrinkage 10%; MD direction, shrinkage 10%) and a second shaping (temperature 130℃) are carried out to obtain a thin film (microporous membrane).
[0083] 5) Rolling and slitting
[0084] The microporous membrane is trimmed by a traction machine and then rolled up at a low tension (rolling tension 8N / m), and then cut into the required width by a slitting machine and rolled up (the width after cutting is 840mm).
[0085] (2) Aramid coating process
[0086] Reference Figure 4 Coating was performed according to the process shown.
[0087] 1) Unwinding and coating
[0088] The slit base film is rewound and enters the diaphragm coating unit, where the aramid slurry is coated on one side of the base film using a T-shaped narrow-slit coating mechanism;
[0089] 2) Extraction and drying
[0090] The obtained coating film is pre-coagulated in a concentration gradient coagulation bath (the coagulation bath is composed of NMP and water, and the volume concentration of NMP is 40% and 20% respectively), and the aramid in the coating gradually precipitates into a three-dimensional network structure, and the NMP in the coating is dissolved in the coagulation bath and slowly replaced. The coating film pre-coagulated in the coagulation bath enters the remaining 6 water tanks, and the residual NMP is fully eluted and then enters the oven to be dried at 85°C. After drying, the aramid coated diaphragm enters the heat treatment process and is heat-set at 120°C.
[0091] 3) Rolling and slitting
[0092] The heat-set coated film is collected into rolls and slit.
[0093] The following embodiments are combined Figure 1 and Figure 2 The wet process for preparing the aramid coated diaphragm of the present invention is described.
[0094] Example 1
[0095] Polyethylene powder (25 parts by weight) and antioxidant (0.3 parts by weight) are added into a twin-screw extruder through a metering system, and paraffin oil (75 parts by weight) is simultaneously added into the twin-screw extruder through a metering pump at a set temperature (110° C.) from multiple oil filling ports set on the twin-screw extruder (70% at the first oil filling port, 20% at the second oil filling port, and 10% at the third oil filling port). The extruder is melt-extruded to a gear pump at a set temperature and rotation speed (180° C., 60 rpm), and the gear pump rotates at a speed of (85 rpm); the extruder is extruded to a filter device at a pressure of 5.5 MPa and a temperature of 215° C., and then extruded to a mold at a pressure of 4 MPa and a temperature of 225° C. to form a sheet substrate.
[0096] The sheet substrate was cooled to 12°C by a cooling casting machine. The cooled sheet (thickness 1300μm, width 650mm) entered the bidirectional synchronous stretching unit (bidirectional stretching ratio was 7 times), and after preheating, stretching, shaping, cooling and other steps, a thick film with a thickness of 30μm and a width of 4550mm was made under the set temperature and wind speed conditions (preheating 122°C, wind speed 25m / s; stretching 119°C, wind speed 28m / s; shaping 117°C, wind speed 22m / s; cooling 30°C, wind speed 25m / s) was made.
[0097] The thick film is cut by the traction machine (thickness 30μm, width 4300mm) and enters Figure 1The coating device shown controls the pressure of the oil removal pressure roller to 25N to remove excess paraffin oil, and coats the aramid slurry on the thick film (oil film).
[0098] The coated thick film enters the extraction tank filled with dichloromethane and NMP to extract the paraffin oil in the oil film and the NMP in the slurry. The extraction tank device adopts a combined type (including 8 extraction tanks from 1# to 8#). The 8#→1# extraction tank adopts the overflow liquid addition method. The injection and replenishment ports are set in the 8# tank. Dichloromethane is added. An overflow tank is set in the 1# tank. Both are equipped with liquid level control. The NMP volume concentration of the 1# tank is set at 40%, and the NMP volume concentration of the 2# tank is set at 20%. The remaining tanks are dichloromethane. According to the overflow liquid level height of the 8# tank and the 1# tank, the injection pump or the overflow drainage pump is controlled to start and stop respectively. The overflow drainage is collected and processed in the subsequent liquid recovery tank. The flow rate of the circulation pump of each tank is set to 35m 3 / h, the oil film in the extraction tank is continuously cleaned through a "W"-shaped path, the extraction mixture flows out through the 1# tank to the recovery collection tank, and the film is dried at 45°C.
[0099] The dried thick film (thickness 16μm, width 3200mm) enters the transverse stretching heat treatment unit and undergoes preheating, transverse stretching, shrinking, and the first shaping step. At the set temperature and wind speed (preheating 127°C, wind speed 25m / s; stretching 125°C, wind speed 28m / s; shrinking 128°C, wind speed 28m / s; first shaping 135°C, wind speed 22m / s), a slight transverse expansion (stretching ratio 1.5 times) is carried out, and then a slight transverse and longitudinal shrinkage (TD direction, shrinkage 10%; MD direction, shrinkage 10%) and a second shaping (temperature 130°C) are carried out to obtain a microporous coated film, which is finally rolled and slit.
[0100] Example 2
[0101] Polyethylene powder (25 parts by weight) and antioxidant (0.3 parts by weight) are added into a twin-screw extruder through a metering system, and paraffin oil (75 parts by weight) is simultaneously added into the twin-screw extruder through a metering pump at a set temperature (110° C.) from multiple oil filling ports set on the twin-screw extruder (70% at the first oil filling port, 20% at the second oil filling port, and 10% at the third oil filling port). The extruder is melt-extruded into a gear pump at a set temperature and speed (180° C., 60 rpm), and the gear pump speed is (85 rpm); the extruder is extruded into a filtering device at a pressure of 5.5 MPa and a temperature of 215° C., and then extruded into a mold at a pressure of 4 MPa and a temperature of 225° C. to form a sheet substrate.
[0102] The sheet substrate was cooled to 12°C by a cooling casting machine. The cooled sheet (thickness 1300μm, width 650mm) entered the bidirectional synchronous stretching unit (bidirectional stretching ratio was 7 times), and after preheating, stretching, shaping, cooling and other steps, a thick film with a thickness of 30μm and a width of 4550mm was made under set temperature and wind speed conditions (preheating 122°C, wind speed 25m / s; stretching 119°C, wind speed 28m / s; shaping 117°C, wind speed 22m / s; cooling 30°C, wind speed 25m / s) was made.
[0103] After the thick film passes through the traction machine and cuts the edge (thickness 30μm, width 4300mm) Figure 1 In the coating device shown, the pressure of the oil removal pressure roller is controlled to 25N to remove excess paraffin oil, and the aramid slurry is coated on the thick film.
[0104] The coated thick film enters the extraction tank filled with dichloromethane and NMP to extract the paraffin oil in the oil film and the NMP in the slurry. The extraction tank device adopts a combined type (including 8 extraction tanks from 1# to 8#). The 8#→1# extraction tank adopts the overflow liquid addition method. The injection and replenishment ports are set in the 8# tank, and pure dichloromethane solution is added. An overflow tank is set in the 1# tank, and both are equipped with liquid level control. The NMP volume concentration of the 1# tank is set at 80%, and the NMP volume concentration of the 2# tank is set at 40%. The remaining tanks are dichloromethane. According to the overflow liquid level height of the 8# tank and the 1# tank, the injection pump or the overflow drainage pump is controlled to start and stop, and the overflow drainage is recycled to the subsequent liquid phase recovery tank. The flow rate of the circulation pump of each tank is set to 35m 3 / h, the oil film in the extraction tank is continuously cleaned through a "W"-shaped path, the extraction mixture flows out through the 1# tank to the recovery collection tank, and the film is dried at 45°C.
[0105] The dried film (thickness 16μm, width 3200mm) enters the transverse stretching heat treatment unit and undergoes preheating, transverse stretching, shrinking, first shaping and other steps. Under the set temperature and wind speed conditions (preheating 127℃, wind speed 25m / s; stretching 125℃, wind speed 28m / s; shrinking 128℃, wind speed 28m / s; first shaping 135℃, wind speed 22m / s), a slight transverse expansion (stretching ratio 1.5 times) is carried out, and then a slight transverse and longitudinal shrinkage (TD direction, shrinkage 10%; MD direction, shrinkage 10%) and a second shaping (temperature 130℃) are carried out to obtain a microporous coated film, which is finally rolled and slit.
[0106] Example 3
[0107] Polyethylene powder (25 parts by weight) and antioxidant (0.3 parts by weight) are added into a twin-screw extruder through a metering system, and paraffin oil (75 parts by weight) is simultaneously added into the twin-screw extruder through a metering pump at a set temperature (110° C.) from multiple oil filling ports set on the twin-screw extruder (70% at the first oil filling port, 20% at the second oil filling port, and 10% at the third oil filling port). The extruder is melt-extruded to a gear pump at a set temperature and rotation speed (180° C., 60 rpm), and the gear pump rotates at a speed of (85 rpm); the extruder is extruded to a filter device at a pressure of 5.5 MPa and a temperature of 215° C., and then extruded to a mold at a pressure of 4 MPa and a temperature of 225° C. to form a sheet substrate.
[0108] The sheet substrate was cooled to 12°C by a cooling casting machine. The cooled sheet (thickness 1300μm, width 650mm) entered the bidirectional synchronous stretching unit (bidirectional stretching ratio was 7 times), and after preheating, stretching, shaping, cooling and other steps, a thick film with a thickness of 30μm and a width of 4550mm was made under set temperature and wind speed conditions (preheating 122°C, wind speed 25m / s; stretching 119°C, wind speed 28m / s; shaping 117°C, wind speed 22m / s; cooling 30°C, wind speed 25m / s) was made.
[0109] The thick film is cut by the traction machine (thickness 30μm, width 4300mm) and enters Figure 1 In the coating device shown, the pressure of the oil removal pressure roller is controlled to 25N to remove excess paraffin oil, and the aramid slurry is coated on the thick film.
[0110] The thick film after coating enters the extraction tank filled with dichloromethane to extract the paraffin oil in the oil film and the NMP in the slurry. The extraction tank device adopts a combined type (including 8 extraction tanks from 1# to 8#). The 8#→1# extraction tank adopts the overflow liquid addition method. The injection and replenishment ports are set in the 8# tank, and pure dichloromethane solution is added. The overflow tank is set in the 1# tank, and both are equipped with liquid level control. The injection pump or overflow drainage pump is controlled to start and stop according to the overflow liquid level height of the 8# tank and the 1# tank. The overflow drainage is collected and processed in the subsequent liquid recovery tank. The flow rate of the circulation pump of each tank is set to 35m 3 / h, the oil film in the extraction tank is continuously cleaned through a "W"-shaped path, the extraction mixture flows out through the 1# tank to the recovery collection tank, and the thick film is dried at 45°C.
[0111] The dried film (thickness 16μm, width 3200mm) enters the transverse stretching heat treatment unit and undergoes preheating, stretching, shrinking, first shaping and other steps. At the set temperature and wind speed (preheating 127°C, wind speed 25m / s; stretching 125°C, wind speed 28m / s; shrinking 128°C, wind speed 28m / s; first shaping 135°C, wind speed 22m / s), a slight transverse expansion (stretching 1.5 times) is carried out, and then a slight transverse and longitudinal shrinkage (TD direction, shrinkage 10%; MD direction, shrinkage 10%) and a second shaping (temperature 130°C) are carried out to obtain a microporous coated film, which is finally rolled and slit.
[0112] The coating films prepared in the comparative examples and examples were subjected to the following performance tests.
[0113] 1. Air permeability test method:
[0114] In the test temperature and humidity (temperature 25°C, humidity 40%) and normal pressure environment, the test instrument (Wang Yan type air permeability instrument) applies a pressure of 1.21kPa, and 100mL of air passes through 6.45cm 2 The time required for the diaphragm.
[0115] Cut 3 pieces of membrane from the film roll at 150mm intervals in the longitudinal direction. If the membrane width is ≥100mm, the sample size is 100mm×100mm. If the membrane width is <100mm, the sample size is 100mm (length)×membrane width. Place the membrane in the test instrument for air permeability test, and take the average of the 3 test results as the membrane air permeability.
[0116] 2. Porosity
[0117] The volume of the pores inside the diaphragm is the percentage of the total volume of the diaphragm. The test is carried out using the method specified in GBT36363-2018.
[0118] 3. Heat shrinkage
[0119] The test was carried out according to the method specified in GB / T12027-2004.
[0120] 4. Tensile strength
[0121] The test was conducted in accordance with the requirements of GB / T 1040.3-2006. The specimen was prepared by cutting method and the specimen type was Type 2. The specimen was in the shape of a strip with a length of 200 mm and a width of 25 mm. The distance between the fixtures was (100±5) mm and the test speed was (250±10) mm / min.
[0122] The test results are shown in Table 1.
[0123] Table 1
[0124]
[0125]
[0126] 1:12 means that the thickness of the polyethylene base film is 12 μm, and 4 means that the thickness of the aramid coating is 4 μm.
[0127] By comparing the preparation processes of the embodiment and the comparative example, it can be seen that the method of the embodiment introduces the coating process after biaxial stretching and before extraction and washing, and directly introduces the coating process into the base film production process, which can realize the one-time molding of the coating film. Compared with the method of the comparative example, the cost of investment equipment can be reduced accordingly, such as one less base film unwinding device, coating film drying device, and coating film winding device. Moreover, compared with the production method of the comparative example, the online coating process provided by the embodiment makes the aramid coating film not only have conventional properties such as thermal yield and air permeability comparable to those of the existing coated aramid, but also have higher tensile strength of the coating film. Compared with the original aramid diaphragm manufacturing process, the transverse stretching makes the orientation of the aramid fiber more consistent after stretching.
[0128] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
[0129] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A method for preparing an aramid coated diaphragm by a wet process, characterized in that: The method includes: (1) melt-extruding, filtering, and extrusion-plasticizing a polyolefin composition to obtain a sheet-like substrate; wherein the polyolefin composition comprises a polyolefin resin, a pore-forming agent, and an antioxidant; (2) cooling the flaky substrate casting to 8-15° C.; (3) biaxially stretching the cooled substrate and trimming the edges to obtain a thick film; (4) coating the aramid slurry on the thick film; (5) extracting and drying the coated thick film; (6) stretching the dried thick film transversely; Wherein, the pore-forming agent is paraffin oil; Wherein, step (4) is performed in a coating device, and the coating device comprises: a tension-breaking mechanism, an oil removal mechanism and a coating mechanism; wherein the tension-breaking mechanism comprises a first transmission guide roller and a second transmission guide roller; and the coating mechanism comprises a backing roller, a narrow slit die head and a feed pipe; Wherein, in step (5), the extraction is carried out in an extraction device, and the extraction device includes 3-9 extraction tanks; according to the transmission direction of the thick film, the first two extraction tanks include an extractant with a concentration gradient, and the extractant with the concentration gradient is selected from dichloromethane and N-methylpyrrolidone, the volume concentration of N-methylpyrrolidone in the first extraction tank is 35-80%, the volume concentration of N-methylpyrrolidone in the second extraction tank is 40-60% of the volume concentration of N-methylpyrrolidone in the first extraction tank, and the extractant in the remaining extraction tanks is dichloromethane.
2. The method according to claim 1, characterized in that The polyolefin resin is selected from polyethylene and polypropylene; The antioxidant is selected from pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and tris(2,4-di-tert-butylphenyl) phosphite.
3. The method according to claim 2, characterized in that The polyethylene is ultra-high molecular weight polyethylene.
4. The method according to claim 2, characterized in that: The mass ratio of the polyolefin resin to the pore-forming agent is 1:(2-5), and the content of the antioxidant is 0.1-0.5 wt % based on the total weight of the polyolefin resin and the pore-forming agent.
5. The method according to claim 1, characterized in that The aramid slurry comprises aramid stock solution and ceramic powder.
6. The method according to claim 5, characterized in that The aramid stock solution is a para-aromatic polyamide stock solution, and the content of para-aromatic polyamide in the stock solution is 1-5% by weight; the median particle size of the ceramic powder is 100-500nm.
7. The method according to claim 6, characterized in that Based on the total weight of the aramid slurry, the content of the para-aromatic polyamide is 0.9-5% by weight, and the content of the ceramic powder is 1-10% by weight.
8. The method according to claim 1, characterized in that Step (1) comprises: adding polyolefin resin and antioxidant into a twin-screw extruder, adding a pore-forming agent into the twin-screw extruder from a refueling port set on the twin-screw extruder, melting and extruding to a gear pump, extruding to a filtering device; and then extruding to a mold to form a sheet substrate.
9. The method according to claim 8, characterized in that The conditions for melt extrusion include: temperature of 160-200°C and rotation speed of 40-70rpm; the rotation speed of the gear pump is 70-100rpm; the conditions for extrusion to the filtering device include: pressure of 3-7MPa and temperature of 200-230°C; the conditions for extrusion to the mold include: pressure of 2-5MPa and temperature of 220-240°C.
10. The method according to claim 1, characterized in that Step (3) comprises: the cooled sheet substrate enters into a biaxial stretching unit, and is sequentially preheated, biaxially stretched, shaped, cooled, and then trimmed by a traction machine.
11. The method according to claim 10, characterized in that The transverse stretching ratio is 5-9, and the longitudinal stretching ratio is 5-9; the preheating temperature is 100-130°C, and the wind speed is 15-30m / s; the stretching temperature is 100-130°C, and the wind speed is 15-30m / s; the shaping temperature is 110-130°C, and the wind speed is 15-30m / s; the cooling temperature is 15-40°C, and the wind speed is 15-30m / s.
12. The method according to claim 1, characterized in that The second transmission guide roller is arranged above the first transmission guide roller, and the narrow slit die head is arranged above the backing roller. The thick film is transmitted along the first transmission guide roller to the second transmission guide roller, and is transmitted successively through the deoiling mechanism and the backing roller. During the transmission process, after part of the pore-forming agent is removed by the deoiling mechanism, the feed pipe injects the aramid slurry into the narrow slit die head, so that the aramid slurry is coated on the thick film.
13. The method according to claim 12, characterized in that The oil removal mechanism comprises a third transmission guide roller and an oil removal pressure roller, wherein the third transmission guide roller is located below the oil removal pressure roller, and the second transmission guide roller, the third transmission guide roller and the top of the back roller are located on the same horizontal line.
14. The method according to claim 1, characterized in that Step (6) includes: the dried thick film enters the transverse drawing heat treatment unit, undergoes preheating, transverse stretching, shrinkage, first shaping, and then transverse and longitudinal shrinkage and second shaping.
15. The method according to claim 14, characterized in that The transverse stretching ratio is 1.1-2 times; the preheating temperature is 110-140°C, and the wind speed is 15-30m / s; the stretching temperature is 110-140°C, and the wind speed is 15-30m / s; the shrinking temperature is 110-140°C, and the wind speed is 15-30m / s; the first setting temperature is 110-140°C, and the wind speed is 15-30m / s; the transverse shrinkage rate is 0.1-10%, the longitudinal shrinkage rate is 0.1-10%, and the second setting temperature is 110-140°C.
16. Aramid coated diaphragm obtained by the method according to any one of claims 1 to 15.
Citation Information
Patent Citations
Method for improving surface activity of polyethylene lithium battery diaphragm
CN104821382A
Method for preparing separation membrane for electrochemical device, and separation membrane for electrochemical device prepared thereby
CN105393383A
Separator for electrochemical device
CN105659410A
Lithium battery diaphragm and preparing method thereof
CN109285981A
Novel lithium ion battery aramid diaphragm preparation method
CN109560235A