A method for preparing cesium hafnium chloride scintillation crystal
By using a cooling crystallization method to prepare Cs2HfCl6 scintillator in an acidic solution, the problems of harsh preparation conditions and complex processes in the existing technology are solved, efficient and low-cost crystal preparation is achieved, and high-quality and high-purity scintillation crystals are obtained.
Patent Information
- Application Number
- CN202210076428.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-01-24
AI Technical Summary
The method for preparing Cs2HfCl6 scintillator in the prior art has harsh conditions, complex and single processes, making it difficult to achieve high-efficiency and low-cost preparation.
Using the cooling crystallization method, CsCl and HfCl4 powders are heated and dissolved in an acidic solution, and then cooled and grown step by step. The concentration and temperature of the solution are controlled to avoid supersaturation and the appearance of impurities. Dilute hydrochloric acid is used as the solvent to improve solubility and control. sex.
The high-quality preparation of Cs2HfCl6 crystals is achieved, the preparation cost is reduced, the operation process is simplified, the utilization rate of raw materials is improved, and high-purity scintillation crystals are obtained through air gun cleaning.
Smart Images

Figure CN114606570B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of scintillation crystal materials, and in particular to a method for preparing a cesium hafnium chloride scintillation crystal. Background Art
[0002] Scintillator crystal is a kind of energy conversion material. After absorbing high-energy rays or particles, it converts energy into ultraviolet light or visible light. The scintillation counter with it as the core component can detect high-energy rays or high-energy particles such as X-rays, gamma rays, and neutrons, and is widely used in medical imaging, high-energy physics, industrial detection and other fields.
[0003] Cs 2 HfCl 6 Scintillator is a new type of inorganic halide scintillator that can detect gamma rays. Due to its characteristics such as high light output and high energy resolution in an undoped state, it is expected to become a cost-effective scintillator for gamma-ray detectors.
[0004] Inorganic halide scintillators have a low melting point and are traditionally prepared by the Bridgman method. 2 HfCl 6 Crystals can currently only be obtained through the Bridgman method, which is a very simple preparation method. 2 HfCl 6 CsCl powder and HfCl in the raw materials of crystal 4 The powders are difficult to dissolve in common organic solvents such as DMSO, GBL, DMF, etc., and the preparation conditions are harsh and the process is complicated. Summary of the invention
[0005] Therefore, the technical problem to be solved by the present invention is to overcome the problems of harsh preparation conditions, complex processes and very single preparation methods in the prior art.
[0006] In order to solve the above technical problems, the present invention provides a method for preparing cesium hafnium chloride scintillation crystal. 2 HfCl 6 The crystal growth method is the cooling crystallization method. This growth method is to mix the powder and solvent to prepare a high-concentration clear solution, heat it to dissolve, stir it and filter it, and then cool it down to grow Cs crystals with regular shapes. 2 HfCl 6 Crystal.
[0007] The first object of the present invention is to provide a Cs 2 HfCl 6 A method for preparing a scintillation crystal comprises the following steps:
[0008] S1, CsCl and HfCl 4Add to an acidic solution, stir and heat to 75-85°C to obtain a precursor solution; the acidic solution is a hydrochloric acid solution;
[0009] S2, heating the precursor solution in step S1, and then cooling and growing in steps to obtain the Cs 2 HfCl 6 Scintillation crystal; the step cooling is divided into two times, the first cooling is to cool to 35-45°C at a rate of 4-6°C / h; the second cooling is to cool to 25-30°C at a rate of 0.1-2°C / h.
[0010] In one embodiment of the present invention, in order to inhibit HfCl 4 The hydrolysis reaction of HfCl 4 To effectively participate in the crystal nucleation and growth process, the solution needs to be in an acidic environment under specific conditions. Dilute hydrochloric acid can easily dissolve CsCl and HfCl because the solvent concentration is controllable. 4 , and no impurities are introduced, so dilute hydrochloric acid solvent is used.
[0011] In one embodiment of the present invention, in order to prevent the solution from being too supersaturated during the cooling process, to avoid precipitation of multiple crystals, and to prevent the growth rate from being too fast which affects the crystallization quality of the crystals, the cooling is performed in steps, where the solution is cooled faster initially and then cooled slowly within the crystal growth temperature range.
[0012] In one embodiment of the present invention, in step S1, the CsCl and HfCl 4 The molar ratio is 2-3:1.
[0013] In one embodiment of the present invention, in step S1, the molar concentration of the acidic solution is 1.06-2.15 mol / L.
[0014] In one embodiment of the present invention, in step S1, the stirring speed is 400-800 r / min; and the stirring time is 4-12 h.
[0015] In one embodiment of the present invention, step S1 further includes a step of filtering the obtained precursor solution, wherein the pore size of the filter used for filtration is 1-5 μm.
[0016] In one embodiment of the present invention, in step S2, the heating is performed at 55-65° C. for 30-90 min.
[0017] In one embodiment of the present invention, in step S2, the growth time is 5-15 days.
[0018] In one embodiment of the present invention, the Cs 2 HfCl 6The scintillation crystals were air-gun cleaned.
[0019] In one embodiment of the present invention, the gas of the air gun is nitrogen.
[0020] The second object of the present invention is to provide a Cs 2 HfCl 6 Scintillator crystal, the Cs 2 HfCl 6 The length and width of the scintillation crystal are 4-10 mm respectively, and the thickness is 2-5 mm.
[0021] The technical solution of the present invention has the following advantages compared with the prior art:
[0022] The cesium hafnium chloride scintillation crystal of the present invention is prepared by a cooling crystallization method using the law that the solubility of the precursor solution in an acidic environment changes with temperature. Compared with the conventional Bridgman growth method, the preparation method has low cost and does not require equipment such as a vacuum quartz crucible, high temperature, simple operation, low raw material cost, high raw material utilization rate, and the solution can be recycled. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:
[0024] Figure 1 This is the growth diagram of the crystal in Example 1 of the present invention.
[0025] Figure 2 This is a crystal diagram of Example 1 of the present invention.
[0026] Figure 3 This is the growth diagram of the crystal of Comparative Example 1 of the present invention.
[0027] Figure 4 This is the growth diagram of the crystal of Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0029] Example 1
[0030] A Cs 2 HfCl 6 The method for preparing a scintillation crystal specifically comprises the following steps:
[0031] (1) Add CsCl powder and HfCl with a purity of 99.9% in a ratio of 2:1. 4The powders weighing 2.70 g and 2.56 g respectively are added into a flat-bottomed transparent glass bottle, and 6 mL of dilute hydrochloric acid with a molar concentration of 1.06 mol / L is added thereto. The mixture is placed on a magnetic stirrer and stirred and heated at a temperature of 80°C and a speed of 600 r / min for 8 hours to completely dissolve it until it is saturated. After dissolution, it is filtered with a filter with a pore size of 2 μm to obtain a precursor solution for growing crystals.
[0032] (2) placing the saturated crystal growth solution in step (1) in an oil bath and slowly cooling it down, the initial temperature of the oil bath being 60° C., cooling it down to 40° C. at a rate of 5° C. / h, and then cooling it down to 28° C. at a rate of 1° C. / h, and precipitating seed crystals from the solution, maintaining the temperature of the oil bath at 28° C. for a growth time of 5 days, and growing an inorganic halide single crystal having a length and width of 4 mm and a thickness of 2 mm, and taking out the Cs 2 HfCl 6 The residual growth solution on the surface was blown away with a nitrogen gun to obtain Cs 2 HfCl 6 Scintillating crystals.
[0033] Figure 1 The growth process of the crystal in Example 1 is shown in the figure. It can be seen from the figure that CsCl powder and HfCl 4 The powder can be stably combined and grown into Cs in a dilute hydrochloric acid solution environment. 2 HfCl 6 Crystal.
[0034] Figure 2 For the crystal grown in Example 1, it can be seen from the picture that the prepared Cs 2 HfCl 6 The crystal has a square shape and is transparent inside.
[0035] Example 2
[0036] A Cs 2 HfCl 6 The method for preparing a scintillation crystal specifically comprises the following steps:
[0037] (1) Add CsCl powder and HfCl with a purity of 99.9% in a ratio of 2:1. 4 The powders weighing 2.70 g and 2.56 g respectively are added into a flat-bottomed transparent glass bottle, and 8 mL of dilute hydrochloric acid with a molar concentration of 2.05 mol / L is added thereto. The mixture is placed on a magnetic stirrer and stirred and heated at a temperature of 80°C and a speed of 600 r / min for 8 hours to completely dissolve it until it is saturated. After dissolution, it is filtered with a filter with a pore size of 2 μm to obtain a precursor solution for growing crystals.
[0038] (2) placing the saturated crystal growth solution in step (1) in an oil bath and slowly cooling it down, the initial temperature of the oil bath being 60° C., cooling it down to 40° C. at a rate of 5° C. / h, and then cooling it down to 25° C. at a rate of 1° C. / h, and precipitating seed crystals from the solution, maintaining the temperature of the oil bath at 25° C., and growing it for 5 days, growing an inorganic halide single crystal with a length and width of 6 mm and a thickness of 3 mm, and taking out the Cs 2 HfCl 6 The residual growth solution on the surface was blown away with a nitrogen gun to obtain Cs 2 HfCl 6 Scintillating crystals.
[0039] Example 3
[0040] A Cs 2 HfCl 6 The method for preparing a scintillation crystal specifically comprises the following steps:
[0041] (1) Add CsCl powder and HfCl with a purity of 99.9% in a ratio of 3:1. 4 The powders weighing 4.05 g and 2.56 g respectively are added into a flat-bottomed transparent glass bottle, and 7 mL of dilute hydrochloric acid with a molar concentration of 2.0 mol / L is added thereto. The mixture is placed on a magnetic stirrer and stirred and heated at a temperature of 80°C and a speed of 600 r / min for 8 hours to completely dissolve it until it is saturated. After dissolution, it is filtered with a filter with a pore size of 2 μm to obtain a precursor solution for growing crystals.
[0042] (2) placing the saturated crystal growth solution in step (1) in an oil bath and slowly cooling it down, the initial temperature of the oil bath being 60° C., cooling it down to 40° C. at a rate of 5° C. / h, and then cooling it down to 25° C. at a rate of 1° C. / h, and precipitating seed crystals from the solution, maintaining the temperature of the oil bath at 25° C., and growing it for 5 days, growing an inorganic halide single crystal with a length and width of 6 mm and a thickness of 3 mm, and taking out the Cs 2 HfCl 6 The residual growth solution on the surface was blown away with a nitrogen gun to obtain Cs 2 HfCl 6 Scintillating crystals.
[0043] Comparative Example 1
[0044] The method is basically the same as Example 1, except that the temperature for preparing the precursor solution is 60° C., and specifically includes the following steps:
[0045] (1) Add CsCl powder and HfCl with a purity of 99.9% in a ratio of 2:1. 4The powders weighing 2.70 g and 2.56 g respectively were added into a flat-bottomed transparent glass bottle, and 6 mL of dilute hydrochloric acid with a molar concentration of 1.06 mol / L was added thereto. The mixture was placed on a magnetic stirrer and stirred and heated at a temperature of 60°C and a speed of 600 r / min for 8 hours to completely dissolve it until it was saturated. After dissolution, it was filtered with a filter with a pore size of 2 μm to obtain a precursor solution for growing crystals.
[0046] (2) The saturated crystal growth solution in step (1) is placed in an oil bath and slowly cooled. The initial temperature of the oil bath is 60°C, and the temperature is lowered to 40°C at a rate of 5°C / h, and then lowered to 25°C at a rate of 1°C / h. Seed crystals are precipitated from the solution. The oil bath temperature is maintained at 25°C. The growth time is 5 days, and dendritic crystals are precipitated from the solution.
[0047] Figure 3 This is the result of Comparative Example 1. Since CsCl and HfCl 4 The powder can be completely dissolved in the solvent at a temperature of 50°C. Therefore, in Comparative Example 1, the container is heated to 60°C to prepare the precursor solution before the subsequent growth step. However, dendritic crystals are precipitated from the solution during the growth process. This is because the lower temperature does not allow the solution to react fully.
[0048] Comparative Example 2
[0049] The same as Example 1, except that CsCl powder and HfCl 4 The amount ratio of the powder material is 4:1, and specifically includes the following steps:
[0050] (1) Add CsCl powder and HfCl with a purity of 99.9% in a ratio of 4:1. 4 The powders weighing 5.40 g and 2.56 g respectively are added into a flat-bottomed transparent glass bottle, and 8 mL of dilute hydrochloric acid with a molar concentration of 1.06 mol / L is added thereto. The mixture is placed on a magnetic stirrer and stirred and heated at a temperature of 80°C and a speed of 600 r / min for 8 hours to completely dissolve it until it is saturated. After dissolution, it is filtered with a filter with a pore size of 2 μm to obtain a precursor solution for growing crystals.
[0051] (2) The saturated crystal growth solution in step (1) is placed in an oil bath and slowly cooled. The initial temperature of the oil bath is 60°C, and the temperature is lowered to 40°C at a rate of 5°C / h, and then lowered to 25°C at a rate of 1°C / h. Seed crystals are precipitated from the solution. The oil bath temperature is maintained at 25°C. The growth time is 5 days, and large pieces of translucent crystals are precipitated from the solution.
[0052] Figure 4 The crystal obtained in Comparative Example 2 is 4Effectively participate in the crystal nucleation process to avoid the presence of easily hydrolyzed Hf in the crystal 4+ ions, we tried to equip it with excess CsCl, but the resulting crystals were irregular in shape and had low crystallinity. This was because the excess CsCl participated in the nucleation process alone, resulting in the presence of CsCl components in the grown crystals.
[0053] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A method for preparing Cs2HfCl6 scintillation crystal, characterized in that: The following steps are included: S1. Add CsCl and HfCl4 into an acidic solution, stir and heat to 75-85°C to obtain a precursor solution; the molar concentration of the acidic solution is 1.06-2.15 mol / L; the acidic solution is a hydrochloric acid solution; the molar ratio of CsCl to HfCl4 is 2-3:1; S2. Heat the precursor solution in step S1, and then cool and grow it in steps to obtain the Cs2HfCl6 scintillation crystal; the heating is 55-65°C for 30-90min; the cooling in steps is divided into two times, the first cooling is to cool to 35-45°C at a rate of 4-6°C / h; the second cooling is to cool to 25-30°C at a rate of 0.1-2°C / h.
2. The method for preparing Cs2HfCl6 scintillation crystal according to claim 1, characterized in that: In step S1, the stirring speed is 400-800 r / min; and the stirring time is 4-12 h.
3. The method for preparing Cs2HfCl6 scintillation crystal according to claim 1, characterized in that: In step S1, the step of filtering the obtained precursor solution is also included, and the pore size of the filter used for filtering is 1-5 μm.
4. The method for preparing Cs2HfCl6 scintillation crystal according to claim 1, characterized in that: In step S2, the growth time is 5-15 days.
5. The method for preparing Cs2HfCl6 scintillation crystal according to claim 1, characterized in that: The method also includes air gun cleaning the Cs2HfCl6 scintillation crystal.
6. The method for preparing Cs2HfCl6 scintillation crystal according to claim 5, characterized in that: The gas of the air gun is nitrogen.
7. The Cs2HfCl6 scintillation crystal prepared by the method according to any one of claims 1 to 6, characterized in that: The length and width of the Cs2HfCl6 scintillation crystal are 4-10 mm respectively, and the thickness is 2-5 mm.