A magnetic plasma thruster cathode and a processing method thereof

By designing a multi-stage air-conducting pore structure and using laser 3D printing technology to prepare the cathode, the problems of serious cathode ablation and processing difficulties in the existing technology are solved, and the cathode is quickly started and efficiently operated, which extends the life and improves the thrust efficiency. .

CN114623060BActive Publication Date: 2024-11-05BEIJING INST OF CONTROL ENG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210106583.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-28
Publication Date
2024-11-05
Estimated Expiration
2042-01-28

AI Technical Summary

Technical Problem

The cathode of the existing magnetic plasma powered thrust is severely ablated during the start-up process, and it is difficult to process and is easy to introduce oxidation, resulting in a short life and the inability to quickly enter the stable arc state.

Method used

Design a cathode with a multi-stage air-conducting pore structure, and use laser 3D printing technology to quickly prepare tungsten-tantalum-oxide mixed powder and copper powder in an oxygen-free environment to form a composite structure connecting the main section of the tungsten cathode and copper, thereby improving thermal plasma bombardment Efficiency and conductivity of heat exchange.

Benefits of technology

It shortens the start time of the cathode, reduces ablation, improves the thrust efficiency and life, reduces the generation of microcracks, and ensures efficient operation of the cathode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114623060B_ABST
    Figure CN114623060B_ABST
Patent Text Reader

Abstract

The present invention provides a magnetic plasma power thruster cathode and a processing method thereof, wherein the cathode structure is a composite structure of a tungsten cathode main section and copper connection, wherein the tungsten cathode main section is a mesoporous rod-shaped structure, wherein the mesoporous structure forms an air guide hole of the thruster cathode, and the air guide hole is functionally divided into an airflow buffer chamber, a gas primary ionization chamber, and a gas reionization chamber, wherein the diameter increases step by step from front to back, thereby increasing the degree of restriction of thermal plasma movement step by step; the copper connector is sleeved at the rear end of the cathode, and is a mesoporous truncated cone structure, wherein the front end diameter is consistent with the outer diameter of the tungsten cathode main section, and the diameter gradually increases from the front end to the rear end. In an oxygen-free environment, tungsten-tantalum-oxide powder and copper powder are simultaneously and rapidly prepared into a MPDT composite cathode using laser 3D printing technology. The present invention solves the problems of low efficiency of thermal plasma bombardment of the inner wall of a single-hole cathode, long startup time, and severe ablation, as well as the problems of difficulty in machining of existing MPDT machines and easy oxidation during machining.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of magnetic power technology, and in particular relates to a magnetic plasma power thruster cathode and a processing method thereof. Background Art

[0002] With the proposal of my country's deep space exploration development strategy, future large-scale space missions need to have efficient, large-scale, and rapid orbital maneuverability. Electric propulsion technology has become the most critical link. my country has carried out a variety of electric propulsion technology research and has made great progress. The magnetoplasma propulsion thruster (MPDT) generates a high-temperature arc through a large current to ionize the propellant, injects energy, and uses the Lorentz force of the magnetic field and current to accelerate the plasma and generate thrust. It has the advantages of high specific impulse, large thrust, light weight, and long-term on-orbit operation. However, the life problem of high-power MPDT cathodes limits its widespread application. Therefore, it is urgent to design an MPDT cathode with uniform ablation, long life, and stable arc.

[0003] For this purpose, the inventor has studied the MPDT cathode. The ablation of the MPDT cathode is mainly divided into start-up ablation and arc stabilization ablation. The cathode start-up mode is a cold start mode, that is, under the external input of high-frequency and high-voltage signals, the cathode uses high voltage to achieve working gas breakdown, and the generated hot plasma bombards the inner wall of the cathode, so that the cathode temperature gradually increases, a sheath is formed on the cathode surface, and it turns into an autonomous thermal electron emission mode, accelerating the ionization of plasma, and gradually entering the arc stabilization state. Studies have shown that this start-up mode is accompanied by severe ablation, and the ablation rate is greatly reduced when entering the arc stabilization state. Therefore, it is necessary to shorten the cathode start-up time so that the cathode can enter the arc stabilization state faster.

[0004] The current single-hole cathode gas-conducting hole is in a through-hole state, and the hot plasma is not restricted when passing through. The efficiency of bombarding the inner wall of the cathode is low, the cathode cannot heat up quickly, and it takes a long time to enter the stable arc state, resulting in severe ablation. In addition, in the current conventional processing method, the cathode needs to be immersed in water and oil, and there is an oxidation problem on the surface, which will also cause severe ablation of the cathode. Summary of the invention

[0005] In order to overcome the deficiencies in the prior art, the inventors have conducted intensive research and provided a magnetic plasma thruster cathode and a processing method thereof. By designing an MPDT cathode with a multi-stage air guide hole structure, the problems of low efficiency of thermal plasma bombardment of the inner wall of a single-hole cathode, long startup time, and severe ablation are solved. In view of the problems of difficult machining of existing MPDT machines and easy oxidation during machining, a method for rapidly preparing a MPDT cathode from tungsten-tantalum-oxide mixed powder and copper powder simultaneously in an oxygen-free environment using laser 3D printing technology is proposed, thereby completing the present invention.

[0006] The technical solution provided by the present invention is as follows:

[0007] In a first aspect, a magnetic plasma thruster cathode is a composite structure of a tungsten cathode main section connected with copper, the tungsten cathode main section is a mesoporous rod-shaped structure, the mesoporous structure forms an air guide hole of the thruster cathode, the air guide hole is functionally divided into an airflow buffer chamber, a gas primary ionization chamber, and a gas reionization chamber, and the diameter increases step by step from front to back, thereby gradually increasing the degree of restriction of thermal plasma movement;

[0008] The copper connector is sleeved on the rear end of the cathode and is a frustum structure with a central hole. The front end diameter is consistent with the outer diameter of the tungsten cathode main body, and the diameter increases gradually from the front end to the rear end.

[0009] In a second aspect, a method for processing a cathode of a magnetic plasma thruster comprises the following steps:

[0010] S1, weighing nano-sized tungsten powder, nano-sized tantalum powder, and oxide powder according to a certain proportion, adding anhydrous ethanol, and mixing them evenly by high-energy ball milling to obtain a suspension of tungsten-tantalum-oxide mixed powder and ethanol;

[0011] S2, using a high-speed centrifuge to separate the solid-liquid of the ball-milled tungsten-tantalum-oxide mixed powder and the ethanol suspension, and then performing vacuum drying and desorption and deoxidation treatment;

[0012] S3, respectively loading the processed tungsten-tantalum-oxide mixed powder and copper powder into the powder tank of the 3D printing device, and placing the powder sample to be prepared in an oxygen-free environment; the 3D printing device adopts a coaxial powder feeding system, and is provided with two or more powder transmission channels for simultaneously feeding the tungsten-tantalum-oxide mixed powder and the copper powder; a powder nozzle is provided at the front end of the channel, which can perform three-dimensional movement and plane rotation operations;

[0013] S4, establish a three-dimensional model diagram of the composite structure MPDT cathode, the model diagram is a three-dimensional diagram of the composite structure of the tungsten cathode main segment and the copper connection; slice the model diagram horizontally and vertically to generate the scanning path of the laser and the powder feeder, and set the powder feeding ratio and laser power at different positions and times.

[0014] S5, after the parameters are set, the powder feeder nozzle sprays powder in an inert atmosphere, and the laser beam performs selective sintering to print the designed three-dimensional composite structure MPDT cathode layer by layer;

[0015] S6, vacuum high temperature treatment of the 3D printed MPDT cathode, the vacuum high temperature treatment temperature is 700-850°C, the heating rate is 10-25°C / min, and the heat preservation is 1-2h.

[0016] A magnetic plasma thruster cathode and a processing method thereof provided by the present invention have the following beneficial effects:

[0017] (1) The present invention provides a cathode for a magnetic plasma thruster, wherein the cathode structure has graded air guide holes, which can improve the bombardment efficiency of the thermal plasma on the inner wall of the cathode, shorten the start-up time of the cathode, and reduce the start-up ablation of the cathode.

[0018] (2) The present invention provides a cathode for a magnetic plasma thruster, the rear end of which is an integrated truncated cone structure of copper and tungsten alloy, and has excellent electrical conductivity and heat exchange capabilities.

[0019] (3) The present invention provides a method for processing a cathode of a magnetic plasma thruster, wherein tantalum powder is added to the powder used, and the laser scanning path between adjacent layers is rotated by a certain angle, which can effectively reduce the tendency of microcracks to be generated during conventional tungsten laser melting and rapid solidification;

[0020] (4) The cathode of a magnetic plasma thruster provided by the present invention has a designed graded air guide hole structure, which can effectively improve the ionization degree of the working fluid gas and increase the thrust efficiency of the thruster. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a cross-sectional view of a cathode of a magnetic plasma thruster of the present invention;

[0022] Among them: 1- copper connector; 2- gas buffer chamber; 3- gas primary ionization chamber; 4- tungsten cathode main section; 5- gas reionization chamber.

[0023] Figure 2 A top view of a cathode of a magnetic plasma thruster according to the present invention;

[0024] Figure 3 The present invention is a flow chart of a method for processing a cathode of a magnetic plasma thruster. DETAILED DESCRIPTION

[0025] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.

[0026] The word "exemplary" is used exclusively herein to mean "serving as an example, embodiment, or illustration." Any embodiment described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other embodiments. Although various aspects of the embodiments are shown in the drawings, the drawings are not necessarily drawn to scale unless otherwise noted.

[0027] According to a first aspect of the present invention, there is provided a cathode of a magnetic plasma thruster, such as Figure 1 and Figure 2As shown, it is a composite structure of a tungsten cathode main section and copper connection. The copper connector 1 is in line with the peripheral thruster structure; the tungsten cathode main section 4 is a mesoporous rod-shaped structure, and the mesoporous structure forms the gas guide hole of the thruster cathode. The gas guide hole is divided into an airflow buffer chamber 2, a gas primary ionization chamber 3, and a gas re-ionization chamber 5 according to the function, and the diameter increases step by step from front to back; the external gas pipe is connected to the end of the gas buffer chamber 2 and is compressed by an elastic gasket. When the working gas enters the chamber, it mainly plays a slow flow role. When the gas moves to the front step wall, the movement is hindered and rebound occurs. Trace ionization can occur in this area, but the temperature is low, and the ionized plasma will recombine into neutral particles; when the working gas enters the gas primary ionization chamber 3, part of the hot plasma generated by ionization directly collides with the chamber wall, and heat transfer occurs, while the hot plasma that does not directly collide is hindered when it moves to the front step of the chamber. , rebounds, moves back to the gas primary ionization chamber 3, and continues to collide with the chamber wall. The residence time of the hot plasma in the chamber increases, the collision efficiency increases, the temperature of the tungsten cathode main section 4 increases, and hot electrons are emitted, so that the working gas that has not been ionized in the chamber is ionized, and the hot plasma is partially re-ionized. At this time, the heat carried is higher and the movement speed is faster, but the ion gas in the chamber has a probability of recombination into neutral, primary particles, but due to the effect of the terminal pressure, the gas eventually enters the gas re-ionization chamber 5; in the gas re-ionization chamber 5, the high-heat primary ionization and secondary ionization plasma collide with the chamber wall more frequently, so that the cathode temperature further increases, the thermal electron emission efficiency increases, and a large number of electrons are generated, which further excites the plasma to re-ionize, and finally transports it to the front end. After calculation, it is found that compared with the ordinary single-hole cathode, the effective collision area of ​​the hot plasma of this structure increases by 25%, which means that the cathode temperature rises faster and the startup time is shorter. In summary, the cathode of this structure can effectively increase the collision efficiency of hot plasma and greatly improve the ionization efficiency of the working gas.

[0028] The copper connector 1 is sleeved on the rear end of the cathode and is a frustum structure with a middle hole. The front diameter is consistent with the outer diameter of the tungsten cathode main body, and the diameter gradually increases from the front to the rear end. The length is 10-20 mm, and the cone angle range is 10-25°. This structure is consistent with the design structure of the peripheral thruster, and mainly plays the role of electrical conduction and heat exchange. The electrical conductivity is 5.5-5.7 (×10 7 )S / m, and the thermal conductivity is 390~401W / (m·K).

[0029] The gas guide holes inside the cathode are designed as a hierarchical structure, divided into a gas buffer chamber 2, a gas primary ionization chamber 3, and a gas reionization chamber 5 according to their functions, and the overall length satisfies: length = gas buffer chamber length + primary ionization chamber length + reionization chamber length, which is 60-80 mm. The outer diameter of the tungsten cathode main section 4 is 30-36 mm.

[0030] The gas buffer cavity 2 has a length of 10-15 mm and a diameter of 15-20 mm, and mainly plays the role of airflow buffering.

[0031] The length of the gas primary ionization chamber 3 is 25-30 mm, and the diameter is 10-14 mm. This design structure mainly serves to improve the ionization rate. When the diameter is higher than 14 mm, the thermal plasma cannot collide effectively, the heat transfer efficiency is slow, and it is not beneficial to the electron emission efficiency of the cathode; when the diameter is lower than 10 mm, the discharge is too concentrated, aggravating the cathode ablation and easily causing the cathode to be cut off in the middle.

[0032] The length of the gas reionization chamber 5 is 25 to 35 mm, and the diameter is 5 to 8 mm. It mainly serves to increase the degree of ionization and is also the area with the most serious ablation. In order to extend the service life of the cathode, the length is longer than the primary ionization chamber. When the diameter is greater than 8 mm, the effective collision area of ​​the primary ionization chamber will be too small, and the ionization efficiency will be reduced, thereby reducing the degree of secondary and tertiary ionization. When the diameter is too small, the discharge is also too concentrated, and the cathode is severely ablated.

[0033] In a preferred embodiment, the cathode rear end uses a copper connector with excellent electrical and thermal conductivity to be integrated with the tungsten cathode main section, while the existing cathode rear end uses a tungsten alloy that is consistent with the main material and has low electrical and thermal conductivity efficiency.

[0034] In a preferred embodiment, the tungsten cathode main body section material is selected from tungsten-tantalum-oxide alloy material, which has low work function and high electron emission efficiency. The tungsten-tantalum-oxide alloy material is made of tungsten powder, tantalum powder and oxide powder, the particle size of the tungsten powder is 50-200nm, and the oxygen content is ≤40ppm; the particle size of the tantalum powder is 50-100nm; the oxide powder is selected from one or more of ZrO2, BaO, and Y2O3, and the particle size is 100-300nm; the mass ratio of the tantalum powder in the tungsten-tantalum-oxide alloy material is not higher than 5%, and the mass ratio of the oxide powder in the tungsten-tantalum-oxide alloy material is not more than 1%.

[0035] In a preferred embodiment, the copper connector is made of oxygen-free copper with a particle size of 30 to 50 nm.

[0036] According to the second aspect of the present invention, a method for processing a cathode of a magnetic plasma thruster is provided, wherein tungsten-tantalum-oxide powder and copper powder are simultaneously and rapidly prepared into a MPDT composite cathode by using laser 3D printing technology in an oxygen-free environment. Figure 3 As shown, the specific steps include:

[0037] S1, weigh nano-scale tungsten powder, nano-scale tantalum powder and oxide powder according to the proportion, mix them evenly by high-energy ball milling, with a ball-to-material ratio of 3:1-8:1, and ball mill for 12-20 hours to ensure the size and distribution uniformity of oxide and metal powders; to prevent powder oxidation, add anhydrous ethanol to the ball milling jar, the amount used is sufficient to exceed the volume of the powder;

[0038] S2, using a high-speed centrifuge to separate the solid and liquid of the ball-milled tungsten-tantalum-oxide mixed powder-ethanol suspension, and then performing vacuum drying and desorption and deoxidation treatment;

[0039] S3, respectively loading the treated tungsten-tantalum-oxide mixed powder and copper powder into the powder tank of the 3D printing device, drawing a vacuum, then filling with argon or helium for cleaning, and drawing a vacuum again, and repeating this process, so that the powder sample to be prepared is in an oxygen-free environment; the 3D printing device adopts a coaxial powder feeding system, and is provided with two or more powder transmission channels for simultaneously feeding the tungsten-tantalum-oxide mixed powder and the copper powder; a powder nozzle is provided at the front end of the channel, which can perform three-dimensional movement and plane rotation operations;

[0040] S4, establish a three-dimensional model diagram of the composite structure MPDT cathode, the model diagram is a three-dimensional diagram of the composite structure of the tungsten cathode main segment and the copper connection; slice the model diagram horizontally and vertically to generate the scanning path of the laser and the powder feeder, and rotate the laser scanning path 60 to 90 degrees between adjacent layers to reduce the generation of micropores and cracks during printing, and set the powder feeding ratio and laser power at different positions and different times;

[0041] S5, after the parameters are set, the powder feeder nozzle sprays the powder, the laser beam performs selective sintering, and the designed three-dimensional composite structure MPDT cathode is printed layer by layer. In this process, in order to ensure an oxygen-free environment, a protective atmosphere such as argon or helium is filled in the printing chamber;

[0042] S6, vacuum high temperature treatment of 3D printed MPDT cathode, vacuum high temperature treatment temperature of 700 ~ 850 ℃, heating rate of 10 ~ 25 ℃ / min, heat preservation of 1 ~ 2h, under this condition, the residual stress of the cathode can be eliminated and the cathode density can be improved.

[0043] In step S1, the selected tantalum powder can effectively reduce the tendency of micro cracks to be generated during the current tungsten laser melting and rapid solidification process.

[0044] In step S2, the vacuum drying and desorption deoxidation treatment method is: in a vacuum environment, while drying, an iron oxygen absorber is placed under the tungsten-tantalum-oxide mixture powder, and the two are separated by a diaphragm. Both treatments are carried out in one chamber at a temperature of 120-150°C and a time of 10-12 hours.

[0045] In step S4, the step of slicing the model image horizontally and vertically includes: slicing the model image into a vertically arranged two-dimensional computer plane with a thickness of 50 to 80 microns, and then slicing the two-dimensional plane horizontally with a width of 50 to 200 microns, thereby generating a scanning path for the laser and the powder feeder. Since tungsten powder and tantalum powder are both refractory metals, when the slice thickness is too large, the laser cannot effectively melt the metal, the cathode density is reduced, and the performance is reduced. When it is too thin, it affects the printing efficiency, and the time and cost required are higher.

[0046] In step S4, the laser printing speed is 0.05-0.15 m / s, and the powder injection speed is 0.05-1 mm 3 / s to ensure uniformity of laser sintering. The power of the laser is set between 200 and 800W. The power is selected according to the material composition of the plane slice. When printing copper connectors, the power is 200 to 300W. When printing the main section of the tungsten cathode, the power is 500 to 800W to ensure that the powder material is fully melted and sintered.

[0047] Example

[0048] Example 1

[0049] Magnetoplasma thruster cathode, such as Figure 1 and Figure 2 As shown in the figure, it is a composite structure of a tungsten cathode main section and copper connection. The tungsten cathode main section is a mesoporous rod-shaped structure with an outer diameter of 30 mm and an overall length of 80 mm. The mesoporous structure forms the gas guide hole of the thruster cathode, which is divided into an airflow buffer chamber, a gas primary ionization chamber and a gas reionization chamber according to its function. The diameter of the airflow buffer chamber is 20 mm and the length is 15 mm. The diameter of the gas primary ionization chamber is 14 mm and the length is 25 mm. The diameter of the gas reionization chamber is 6 mm and the length is 35 mm. The copper connector is sleeved at the rear end of the cathode and is a mesoporous truncated cone structure with a front diameter of 30 mm, a rear diameter of 40 mm, a length of 15 mm, a cone angle of 25°, and a conductivity of 5.7×10 7 S / m, and the thermal conductivity is 401W / (m·K).

[0050] The tungsten cathode main section material is made of tungsten powder, tantalum powder and ZrO2 powder, wherein the mass of tantalum powder accounts for 5% of the total mass and the mass of ZrO2 powder accounts for 0.8%.

[0051] Example 2

[0052] Preparation of the MPDT cathode in Example 1:

[0053] (1) Mix tungsten powder with a particle size of 50-200 nm and an oxygen content of ≤40 ppm, tantalum powder with a particle size of 50-100 nm, and ZrO2 powder with a particle size of 100-300 nm, with the mass of tantalum powder accounting for 5% of the total mass and the mass of ZrO2 powder accounting for 0.8%. Put the mixed powder into a high-energy ball mill, add anhydrous ethanol, isolate the air, and the ball-to-material ratio is 3:1. Ball mill for 12 hours to prepare a tungsten-tantalum-oxide mixed powder;

[0054] (2) The ball-milled powder is vacuum dried and desorbed for deoxidation using an iron oxygen absorber at a temperature of 120° C. for 12 h.

[0055] (3) The powder was loaded into a 3D printing powder tank, the tank was vacuumed, and then filled with argon gas for cleaning, and this process was repeated three times.

[0056] (4) Use CAD to build a three-dimensional model of the MPDT cathode and import it into the 3D printing system. Cut the three-dimensional model horizontally and vertically, with a cutting width and thickness of 50 μm. Rotate the laser scanning path 90° between adjacent layers. Set the laser scanning path and laser power. When sintering copper powder, use 200 W power. When sintering tungsten-tantalum mixed powder, use 500 W power. After the parameters are set, start the machine for sintering printing.

[0057] (5) After printing, cool it for half an hour, and then immediately transfer the formed MPDT cathode to a vacuum furnace. Set the temperature to 750°C, increase the heating rate to 10°C / min, and keep it at this temperature for 1 hour before cooling it in the furnace.

[0058] (6) The prepared MPDT cathode was subjected to an ignition test, and the test conditions were working current: 450A, external magnetic field current: 60A, and argon gas flow rate: 50mg / s. Optical measurement of the temperature distribution of the working cathode revealed that the temperature distribution on the cathode surface was uniform, without any local high temperature area, and the end surface temperature was stable at around 2000℃. The temperature from the re-ionization chamber to the primary ionization chamber decreased in sequence from 1100 to 1900℃. After 150h of ignition test, there was no local severe ablation, melting, or fracture of the cathode. The average ablation loss rate was 25.6mg / h, and the converted life could reach more than 11000h.

[0059] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

[0060] The contents not described in detail in the specification of the present invention belong to the common knowledge of those skilled in the art.

Claims

1. A method for processing a cathode of a magnetic plasma thruster, characterized in that: The cathode is a composite structure of a tungsten cathode main section and a copper connection. The tungsten cathode main section (4) is a mesoporous rod-shaped structure. The mesoporous structure forms a gas guide hole of the thruster cathode. The gas guide hole is functionally divided into a gas buffer chamber (2), a gas primary ionization chamber (3) and a gas reionization chamber (5). The diameter increases step by step from front to back, thereby increasing the degree of restriction of thermal plasma movement step by step. The copper connection piece (1) is sleeved on the rear end of the cathode and is a mesoporous truncated cone structure. The front end diameter is consistent with the outer diameter of the tungsten cathode main section, and the diameter gradually increases from the front end to the rear end. The processing method comprises the following steps: S1, weighing nano-sized tungsten powder, nano-sized tantalum powder, and oxide powder according to a certain proportion, adding anhydrous ethanol, and mixing them evenly by high-energy ball milling to obtain a suspension of tungsten-tantalum-oxide mixed powder and ethanol; S2, using a high-speed centrifuge to separate the solid-liquid of the ball-milled tungsten-tantalum-oxide mixed powder and the ethanol suspension, and then performing vacuum drying and desorption and deoxidation treatment; S3, respectively loading the processed tungsten-tantalum-oxide mixed powder and copper powder into the powder tank of the 3D printing device, and placing the powder sample to be prepared in an oxygen-free environment; the 3D printing device adopts a coaxial powder feeding system, and is provided with two or more powder transmission channels for simultaneously feeding the tungsten-tantalum-oxide mixed powder and the copper powder; a powder nozzle is provided at the front end of the channel, which can perform three-dimensional movement and plane rotation operations; S4, establishing a three-dimensional model diagram of the composite structure MPDT cathode, the model diagram is a three-dimensional diagram of the composite structure of the tungsten cathode main segment and the copper connection; slicing the model diagram horizontally and vertically, generating scanning paths of the laser and the powder feeder, and setting the powder feeding ratio and the laser power at different positions and different times; S5, after the parameters are set, the powder feeder nozzle sprays powder in an inert atmosphere, and the laser beam performs selective sintering to print the designed three-dimensional composite structure MPDT cathode layer by layer; S6, vacuum high temperature treatment of the 3D printed MPDT cathode, the vacuum high temperature treatment temperature is 700-850°C, the heating rate is 10-25°C / min, and the heat preservation is 1-2h.

2. The method for processing the cathode of a magnetic plasma thruster according to claim 1, characterized in that: In step S2, the vacuum drying and desorption deoxidation treatment method is: under a vacuum environment, while drying, an iron oxygen absorber is placed under the tungsten-tantalum-oxide mixture powder, and the two are separated by a diaphragm. Both treatments are carried out in one chamber at a temperature of 120-150° C. and a time of 10-12 hours.

3. The method for processing the cathode of a magnetic plasma thruster according to claim 1, characterized in that: In step S4, the step of slicing the model image horizontally and vertically includes: slicing the model image into a vertically arranged computer two-dimensional plane with a thickness of 50 to 80 microns, and then dividing the two-dimensional plane horizontally with a width of 50 to 200 microns, thereby generating a scanning path for the laser and the powder feeder, and rotating the laser 60 to 90 degrees between adjacent layers.

4. The method for processing the cathode of a magnetic plasma thruster according to claim 1, characterized in that: In step S4, the laser printing speed is 0.05-0.15 m / s, and the powder injection speed is 0.05-1 mm 3 / s; the setting power of the laser is between 200 and 800 W. When printing copper connectors, a power of 200 to 300 W is selected, and when printing the tungsten cathode main body, a power of 500 to 800 W is selected.

5. The method for processing the cathode of a magnetic plasma thruster according to claim 1, characterized in that: The outer diameter of the tungsten cathode main body section (4) is 30-36 mm, and the overall length is 60-80 mm; the diameter of the gas buffer chamber (2) is 15-20 mm, and the length is 10-15 mm; the diameter of the gas primary ionization chamber (3) is 10-14 mm, and the length is 25-30 mm; the diameter of the gas reionization chamber (5) is 5-8 mm, and the length is 25-35 mm; The length of the copper connector (1) is 10-20 mm, the cone angle range is 10-25°, and the electrical conductivity is 5.5-5.7 (×10 7 )S / m, and the thermal conductivity is 390~401W / (m·K).

6. The method for processing the cathode of a magnetoplasma thruster according to claim 1, characterized in that: The tungsten cathode main section (4) and the copper connecting piece (1) are formed in one piece.

7. The method for processing the cathode of a magnetic plasma thruster according to claim 1, characterized in that: The material of the tungsten cathode main section is a tungsten-tantalum-oxide alloy material, which is made of tungsten powder, tantalum powder and oxide powder. The particle size of the tungsten powder is 50-200nm, and the oxygen content is ≤40ppm; the particle size of the tantalum powder is 50-100nm; the oxide powder is selected from one or more of ZrO2, BaO, and Y2O3, and the particle size is 100-300nm; the mass ratio of the tantalum powder in the tungsten-tantalum-oxide alloy material is not higher than 5%, and the mass ratio of the oxide powder in the tungsten-tantalum-oxide alloy material is not more than 1%.