A hydrothermal synthesis method for lithium iron manganese phosphate nanoparticles

Through the method of pre-heating outside the kettle and rapid heating of preheating units, the problem of insufficient heat transfer caused by the expansion of the reactor in the hydrothermal method is solved, and the nanoification and spherification of lithium iron manganese phosphate nanoparticles are realized, and the electrical power of the material is improved. Chemical properties and production efficiency.

CN114628660BActive Publication Date: 2024-11-15HENAN VOLUNTE NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210431899.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-22
Publication Date
2024-11-15
Estimated Expiration
2042-04-22

AI Technical Summary

Technical Problem

When the existing hydrothermal method is used to prepare lithium iron manganese phosphate nanoparticles, the expansion of the reactor leads to insufficient heat transfer power, making it difficult to control the particle size and morphology, and low-temperature reactions can easily lead to ion mixing and affect electrochemical performance.

Method used

The raw material mixture slurry is used outside the kettle, and it is quickly heated through the preheating unit and then sent to the reactor. The reaction temperature is controlled at 140-160℃, which shortens the residence time of the low-temperature section, and realizes nanoification and spherification.

Benefits of technology

It improves the uniformity and morphology of product particles, reaches the nanometer level, improves the rate performance and low-temperature performance of the material, has mild operating conditions, small equipment investment, simple and controllable process, and stable product batches.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114628660B_ABST
    Figure CN114628660B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium ion battery positive electrode material preparation, and in particular to a hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles, comprising the following steps: preparing lithium, iron, manganese, and phosphorus source raw material solutions, mixing the raw material solutions to obtain a mixed slurry; conveying the mixed slurry to a preheating unit for preheating, and then conveying the heated mixed slurry to a reactor; carrying out a hydrothermal synthesis reaction in the reactor; filtering, washing, and drying the product to obtain lithium iron manganese phosphate powder; and mixing the lithium iron manganese phosphate powder with a carbon source to obtain carbon-coated lithium iron manganese phosphate. The present invention shortens the residence time of the reaction system in the low temperature section by preheating the mixed slurry of the reaction raw materials outside the reactor and then conveying it to the reactor for continued reaction, thereby fundamentally achieving control of the product morphology and particle size, and the prepared material particles are uniform, the morphology is changed from sheet-like to spherical, and the scale can reach nanometer level, which is conducive to the improvement of the rate performance and low temperature performance of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery positive electrode material preparation, and in particular to a hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles. Background Art

[0002] Lithium iron manganese phosphate has been widely used in the field of electric vehicles because of its high specific capacity, safety, environmental friendliness and long life. However, the low-temperature discharge performance and rate performance of lithium iron manganese phosphate materials still need to be improved. In addition to optimizing the conductive material coating, particle nano-sizing is the most effective way to improve its performance. Many studies have shown that nano-scale positive electrode materials exhibit a specific capacity close to their theoretical capacity. To achieve nano-sizing of materials, it must rely on the preparation process, and the hydrothermal method has unique advantages in the preparation of nanoparticles.

[0003] Generally, the particle morphology and size can be controlled by controlling the hydrothermal synthesis conditions. For example, the patent with publication number CN111777051A uses ethylene glycol as a solvent and a surfactant, the patent with publication number CN104583130A uses glycerol as a solvent, and the patent with publication number CN104918888A uses various alcohols as solvents; using part of the organic solvent to replace water can reduce the pressure of the reaction system and also achieve the purpose of refining particles. However, the solubility of the reaction raw materials in organic solvents is lower than that in water, which further reduces the reaction concentration, which is not high to begin with, and the unit equipment capacity or production efficiency is low. In addition, there are problems with explosion-proof workshops and equipment and organic wastewater treatment.

[0004] In terms of production technology, the existing hydrothermal method for preparing lithium iron manganese phosphate mainly includes dissolving soluble ferrous salts and manganese salts, phosphoric acid and lithium hydroxide in a certain proportion, mixing them in a reactor, and heating them to 120-374°C (critical temperature of water). Lithium iron manganese phosphate crystals can be obtained in a wide temperature range. Existing technologies focus on the reaction conditions in the preparation process, such as temperature, solvent (water or organic solvent, corresponding to the autogenous pressure of water and solvent), reaction time, pH value of the reaction system, etc. Generally speaking, the higher the reaction temperature, the smaller the particles of the prepared crystals, and the better the electrochemical performance. But in fact, technical solutions such as increasing the reaction temperature and using surfactants or organic solvents have not fundamentally solved the problem of particle size control in the crystallization process. Because, on the surface, the raw materials involved in the hydrothermal reaction are first dissolved and then added to the reactor. The raw materials are molecularly mixed. However, at room temperature or slightly above room temperature, after the reaction raw material solutions are mixed, a new precipitation mixture is immediately formed. The reaction is as follows:

[0005] LiOH+H3PO4+FeSO4→Li3PO4↓+Fe3(PO4)2·nH2O↓+Li2SO4

[0006] As the temperature rises, the Li3PO4 precipitate and the Fe3(PO4)2·nH2O precipitate dissolve successively, releasing Li + , Fe 2+ and PO4 3- , these ions are recombined to form lithium iron phosphate. When part of manganese is used to replace iron, the mechanism is the same, but the dissolution temperature is slightly lower. In such a process, it is difficult to achieve the degree of molecular mixing of raw materials in the actual reaction, and a large number of crystal nuclei cannot be formed in a short time. Therefore, the particle size will be difficult to reduce due to the small number of crystal nuclei.

[0007] It has been reported (Chemical and morphological transformation throughhydrothermal process for LiFePO4 preparation in organic-free system, Electrochimica Acta, (96) 2013: 230-236) that lithium iron phosphate crystals can be formed starting from 120°C, but at low temperatures, iron ions and lithium ions are easily mixed in the crystals, which is not conducive to ion conduction in the crystals. Therefore, the reaction system should be avoided as much as possible from reacting at low temperatures (from 120°C to 140°C). On the other hand, as the reaction volume increases, for example, the reactor volume increases by 100 times, the surface heat transfer area of ​​the reactor theoretically only increases by 21 times (if the internal casing heat transfer is calculated, it will not deviate too much from this value). Therefore, for large-scale industrial production, it is urgent to solve the problem of rapid temperature rise. Patent publication number CN105060266A discloses a hydrothermal synthesis technology that uses high-temperature steam to directly heat a hydrothermal reactor. However, heating with steam will lead to a decrease in the concentration of the reaction system and a decrease in unit production capacity. Moreover, as the volume of a single reactor increases, if the steam transfer rate is increased only by steam, it will cause disturbances to the mass transfer and transmission in the reactor, which is not conducive to production operation control.

[0008] The above problems need to be solved. Summary of the invention

[0009] In order to solve the above problems, the present invention provides a hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles, which preheats the mixture of raw materials outside the reactor and then adds it into the reactor that has been heated to the set value to overcome the problem of insufficient heat transfer power caused by the expansion of the equipment volume, shortens the residence time of the reaction system in the low temperature section, fundamentally realizes the control of product morphology and particle size, and achieves the purpose of nano- and sphericalization.

[0010] The present invention adopts the following technical scheme.

[0011] A hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles comprises the following steps:

[0012] (1) adding a mixture of a lithium source and a phosphorus source into a batching kettle, purging the air in the dead volume of the kettle with an inert gas, and then sealing the batching kettle; opening a feed valve and an exhaust valve of the batching kettle, adding a mixed solution of a pure iron source and a manganese source under stirring, and sealing the batching kettle after the addition is completed, and continuing to stir for 10-30 minutes to obtain a mixed slurry of raw materials;

[0013] (2) The mixed slurry in the batching kettle is transported to a preheating unit for preheating. The outlet slurry temperature of the preheating unit is 140-160° C. The heated mixed slurry is then transported to a reactor preheated to 140-160° C. The air in the dead volume of the reactor has been purged with inert gas in advance. After all the mixed slurries are heated and transported, the reactor is sealed;

[0014] (3) Stirring the slurry in the reactor, maintaining the temperature at 140-160° C. for 2-4 hours, then stopping heating and cooling to 70-80° C.;

[0015] (4) opening the discharge valve of the reactor, filtering the product and washing until there is no sulfate ion, obtaining a filter cake and a mother liquor, and drying the filter cake to obtain lithium iron manganese phosphate powder;

[0016] (5) mixing the lithium iron manganese phosphate powder and the carbon source, and calcining at 700° C. for 4 hours under the protection of an inert gas to obtain carbon-coated lithium iron manganese phosphate;

[0017] Wherein, the manganese source accounts for 0-70% of the total molar amount of the iron source and the manganese source.

[0018] Furthermore, the preheating unit is composed of a plurality of tubular preheaters connected in parallel, and the tubular preheaters are heated by a high-temperature oil bath or electric heating. Specifically, the overall feeding speed is controlled by controlling the number of tubular preheaters connected in parallel.

[0019] Furthermore, the inlet slurry temperature of the preheating unit is 20-30°C, the outlet slurry temperature is 140-160°C, and the heating time of the slurry in the preheating unit does not exceed 30 minutes.

[0020] Furthermore, the preheating temperature of the reactor in step (2) is lower than the outlet slurry temperature of the preheating unit.

[0021] Furthermore, the molar ratio of the substances added in step (1) is Li:M(Fe+Mn):P=3.0:(0.99-1.0):1.0; and the combined concentration of iron and manganese elements after the addition is completed is 0.5-0.7 mol / L.

[0022] Furthermore, in step (1), lithium hydroxide is dissolved in water and mixed with phosphoric acid as a lithium source and a phosphorus source; or lithium phosphate recovered from the mother liquor is mixed with a required amount of lithium hydroxide solution and phosphoric acid as a lithium source and a phosphorus source; or lithium phosphate is used alone as a lithium source and a phosphorus source.

[0023] Furthermore, the mother liquor obtained by filtration in step (4) and the primary washing water of the filter cake are combined, evaporated and concentrated, and the lithium phosphate is recovered.

[0024] Furthermore, the iron source is ferrous sulfate crystals or liquid before crystallization, and the manganese source is manganese sulfate. Specifically, the molar ratio of the iron source to the manganese source is preferably Fe:Mn=3:7-7:3.

[0025] Furthermore, in step (5), the lithium iron manganese phosphate powder and the carbon source are mixed at a mass ratio of 100:(10-15). Specifically, the dried lithium iron manganese phosphate powder is mixed with the carbon source to form a slurry with a solid content of 30-60%, and then spray-dried to obtain a mixture of lithium iron phosphate powder and carbon source.

[0026] Furthermore, the carbon source is glucose.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles of the present invention solves the problem of insufficient heat transfer power caused by the expansion of the reactor by preheating the mixed slurry of the reaction raw materials outside the reactor, compared with indirect heating in the reactor or direct heating with water vapor, and does not reduce the concentration of reactants and the production capacity of the unit equipment. At the same time, the slurry is quickly heated by the preheating unit and then sent to the reactor for further reaction, which shortens the residence time of the reaction system in the low temperature section, fundamentally realizes the control of the product morphology and particle size, and the prepared material particles are uniform, the morphology is changed from flake to spherical, and the scale can reach nanometer level, which is conducive to the improvement of the rate performance and low temperature performance of the material.

[0029] (2) The hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles of the present invention has mild operating conditions. By preheating at 140-160°C, the corresponding pressure is relatively small, thus avoiding the adverse effects of excessively high reaction temperatures (corresponding to higher autogenous pressures) on the equipment. In addition, the equipment investment is small, the process is simple and controllable, and the batch stability of the product is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 This is a morphology diagram of lithium manganese iron phosphate prepared in Example 1 of the present invention;

[0032] Figure 2 This is a morphology diagram of lithium manganese iron phosphate prepared in Comparative Example 1 of the present invention;

[0033] Figure 3 The 25°C, 0.2C charge and discharge curves of the batteries prepared in Examples 1-3 of the present invention are shown. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention.

[0035] Example 1

[0036] A hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles comprises the following steps:

[0037] Step 1: Prepare a mixed slurry of lithium, iron, manganese and phosphorus raw materials

[0038] (1) Preparation of phosphorus source and lithium source mixed slurry: Dissolve 3 kmol of lithium hydroxide monohydrate in water and add water to make the volume of the solution 1m 3 , add to batching kettle 1, add about 75L of 1kmol phosphoric acid under stirring, after adding, purge the air in the dead volume of the kettle with inert gas, seal batching kettle 1, and obtain slurry A with a volume of about 1.07m 3 ;

[0039] (2) Prepare a mixed solution of iron source and manganese source: Take 0.3 kmol of ferrous sulfate heptahydrate and 0.7 kmol of manganese sulfate dihydrate, add water to a volume of 1 m 3 , stir until completely dissolved, filter through a pipeline precision filter, and transfer to batching kettle 2 to obtain slurry B with a volume of about 1.0m 3 ;

[0040] (3) Mixing slurry A and slurry B: Open the liquid-sealed exhaust valve of batching kettle 1 under room temperature and stirring, and add the solution in batching kettle 2 to batching kettle 1. After the addition is completed, continue stirring for 20-30 minutes to obtain slurry C with a volume of about 2m 3 ;

[0041] The molar ratio of the added substances is Li:M(Fe+Mn):P=3.0:1.0:1.0, wherein Fe:Mn (molar ratio)=3:7. After the addition is completed, the total concentration of iron and manganese elements in the solution is about 0.5 mol / L.

[0042] Step 2: Preheating and conveying of raw material slurry

[0043] (1) The slurry C obtained in the first step is transported into the preheating unit equipment by a high-pressure pump. The inlet slurry temperature of the preheating unit equipment is 25°C, the outlet slurry temperature is 155°C, the slurry stays in the preheating unit for 16 minutes, the heating rate is 8°C / min, and the residence time and outlet temperature of the slurry in the preheating unit are controlled by adjusting the outlet flow rate. The preheating unit equipment is four parallel tubular preheaters;

[0044] (2) At the same time, the air in the dead volume of the autoclave is purged with inert gas, and the autoclave is heated to 150°C. The volume of the autoclave is 3m 3 , after the addition is completed, the filling factor of the reactor is about 0.7;

[0045] (3) The slurry from the preheating unit is directly added to the high-pressure reactor with stirring through a pipeline. After all the slurry has been added, the reactor is sealed;

[0046] Step 3: Hydrothermal synthesis reaction

[0047] The reaction vessel was heated by its own jacket and casing (220°C oil bath), the reaction temperature was maintained at 150°C, and the reaction was carried out for 2 hours;

[0048] Step 4: Filtration, washing and drying of the product

[0049] After the above reaction is completed, the reactor is cooled to 80°C with cooling oil through a coil, the vent valve and the discharge valve are opened, the product is filtered to obtain a filter cake and a mother liquor, and then the filter cake is washed three times with water of the same volume as the mother liquor to obtain LiFe 0.3 Mn 0.7 PO4 white powder; the powder is mixed with 12% glucose in terms of solid content to form a slurry with a solid content of about 40%, and then spray-dried; the mother liquor and the first wash water are put into a recovery tank, and sodium phosphate is added after evaporation and concentration to recover lithium phosphate;

[0050] Step 5: Carbon coating

[0051] The spray-dried powder obtained in the fourth step was calcined at 700°C under nitrogen protection for 4 hours to obtain carbon-coated lithium iron phosphate (LiFe 0.3 Mn 0.7 PO4 / C) products.

[0052] The lithium iron manganese phosphate / carbon prepared above was used as the positive electrode material of the battery to test its charge and discharge performance. Specifically: the lithium iron manganese phosphate / carbon, acetylene black, and 60% polytetrafluoroethylene emulsion obtained above were mixed in a mass ratio of 7:2:1, rolled into a sheet with a thickness of 0.10-0.15 mm, and pressed together with aluminum foil, and vacuum dried at 120°C for 12 hours to obtain the positive electrode of the battery. A button cell was assembled with a metal lithium sheet negative electrode, a 1M LiPF6 solution as an electrolyte, and cell gard 2300 as a diaphragm, and the above positive electrode was used to charge and discharge at 0.2C and 1C rates at 25°C, and then discharged at 0.2C at -20°C. The charge and discharge voltage range was 4.5-2.3V.

[0053] The scanning electron microscope image of the material is as follows Figure 1 As shown in Table 1, the particles of the material are uniform, spherical in shape, and the size can reach the nanometer level. The electrochemical performance test results are shown in Table 1 and Figure 3 As shown, as a positive electrode active material, the prepared lithium-ion battery has good rate performance and low temperature performance.

[0054] Example 2

[0055] The lithium source and phosphorus source in the slurry A in Example 1 are replaced by lithium phosphate recovered from a portion of the mother liquor, and the insufficient part is supplemented by lithium phosphate obtained by the neutralization reaction of lithium hydroxide and phosphoric acid.

[0056] Specifically, a hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles comprises the following steps:

[0057] Step 1: Prepare a mixed slurry of lithium, iron, manganese and phosphorus raw materials

[0058] (1) Preparation of phosphorus source and lithium source mixed slurry: 0.6 kmol (on a dry basis) of wet lithium phosphate crystals obtained by recovering the mother liquor is directly added to batching kettle 1, and then 1.2 kmol of lithium hydroxide monohydrate is added to batching kettle 1, and water is added to dissolve the solution to make the volume of the solution 1m 3 , add 0.4 kmol phosphoric acid (about 30 L) under stirring. After the addition, purge the air in the dead volume of the kettle with inert gas, seal the batching kettle 1, and obtain slurry A with a volume of about 1.0 m 3 ;

[0059] (2) Prepare a mixed solution of iron source and manganese source: Take 0.3 kmol of ferrous sulfate heptahydrate and 0.7 kmol of manganese sulfate dihydrate, add water to a volume of 1 m 3, stir until completely dissolved, filter through a pipeline precision filter, and transfer to batching kettle 2 to obtain slurry B with a volume of about 1.0m 3 ;

[0060] (3) Mixing slurry A and slurry B: Open the liquid-sealed exhaust valve of batching kettle 1 under room temperature and stirring, and add the solution in batching kettle 2 to batching kettle 1. After the addition is completed, continue stirring for 20-30 minutes to obtain slurry C with a volume of about 2m 3 ;

[0061] The molar ratio of the added substances is Li:M(Fe+Mn):P=3.0:1.0:1.0, wherein Fe:Mn (molar ratio)=3:7. After the addition is completed, the total concentration of iron and manganese elements in the solution is about 0.5 mol / L.

[0062] The other preparation steps and testing methods are the same as those in Example 1.

[0063] The electrochemical performance test results are shown in Table 1 and Figure 3 As shown. It can be seen that the product prepared in Example 2 exhibits almost the same electrochemical performance as that in Example 1; this shows that using the relatively coarse lithium phosphate recovered to replace the newly prepared lithium phosphate on site and using the preheating method of the present invention to prepare lithium iron manganese phosphate does not affect the performance of the product.

[0064] Example 3

[0065] The hydrothermal synthesis reaction temperature in Example 1 was set to 160° C. to increase the concentration of reactants.

[0066] Specifically, a hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles comprises the following steps:

[0067] Step 1: Prepare a mixed slurry of lithium, iron, manganese and phosphorus raw materials

[0068] (1) Preparation of phosphorus source and lithium source mixed slurry: Add 1.584 kmol of lithium hydroxide monohydrate into the batching kettle 1, add 0.56 m of water 3 Dissolve, add 0.528 kmol phosphoric acid (about 30 L) under stirring; then add 0.792 kmol (on a dry basis) of lithium phosphate wet crystals obtained by recovering the mother liquor directly into batching kettle 1. After the addition is completed, the air in the dead volume in the kettle is purged with inert gas, and then the batching kettle 1 is sealed to obtain slurry A with a volume of about 0.64 m 3 ;

[0069] (2) Prepare a mixed solution of iron source and manganese source: Take 0.528 kmol of ferrous sulfate heptahydrate and 0.792 kmol of manganese sulfate dihydrate, add water to a volume of 1.32 m 3, stir until completely dissolved, filter through a pipeline precision filter, and transfer to batching kettle 2 to obtain slurry B with a volume of about 1.32m 3 ;

[0070] (3) Mixing slurry A and slurry B: Open the liquid-sealed exhaust valve of batching kettle 1 under room temperature and stirring, and add the solution in batching kettle 2 to batching kettle 1. After the addition is completed, continue stirring for 20-30 minutes to obtain slurry C with a volume of about 1.96m 3 ;

[0071] The molar ratio of the added substances is Li:M(Fe+Mn):P=3.0:1.0:1.0, wherein Fe:Mn (molar ratio)=4:6. After the addition is completed, the total concentration of iron and manganese elements in the solution is about 0.67 mol / L.

[0072] Step 2: Preheating and conveying of raw material slurry

[0073] (1) The slurry C obtained in the first step is transported into the preheating unit equipment by a high-pressure pump. The inlet slurry temperature of the preheating unit equipment is 25°C, the outlet slurry temperature is 160°C, the slurry stays in the preheating unit for 17 minutes, the heating rate is 8°C / min, and the residence time and outlet temperature of the slurry in the preheating unit are controlled by adjusting the outlet flow rate. The preheating unit equipment is four parallel tubular preheaters;

[0074] (2) At the same time, the air in the dead volume of the autoclave is purged with inert gas, and the autoclave is heated to 155°C. The volume of the autoclave is 3m 3 , after the addition is completed, the filling factor of the reactor is about 0.7;

[0075] (3) The slurry from the preheating unit is directly added to the high-pressure reactor with stirring through a pipeline. After all the slurry has been added, the reactor is sealed;

[0076] Step 3: Hydrothermal synthesis reaction

[0077] The reactor was heated to 160°C by the reactor jacket and casing (220°C oil bath) and maintained for 2 hours;

[0078] The other steps are the same as those in Example 1, and the performance testing method is the same as that in Example 1.

[0079] The electrochemical performance test results are shown in Table 1 and Figure 3As shown. It can be seen that the product obtained in Example 3 exhibits almost the same electrochemical performance as that of Example 1; this shows that the performance of the product is not affected by using the relatively coarse lithium phosphate recovered to replace the newly prepared lithium phosphate on site and using the preheating method of the present invention to prepare lithium iron manganese phosphate. At the same time, the concentration of the reactants can be increased, which can not only improve the production efficiency of a single kettle, but also reduce water consumption and energy consumption.

[0080] Comparative Example 1

[0081] The hydrothermal synthesis was carried out according to conventional feeding technology.

[0082] Specifically, a hydrothermal synthesis method of lithium iron manganese phosphate comprises the following steps:

[0083] The first step: same as in Example 1.

[0084] Step 2: Use a high-pressure pump to transport the slurry C obtained in the first step into a 3m 3 In the high-pressure reactor, the reactor is heated by jacket electric heating. Due to the limitation of heating power (heat exchange area, oil temperature, equipment wall thickness, etc.), it took 70 minutes for the temperature of the reactor to rise from 20°C to 150°C, which is equivalent to a heating rate of 1.86°C / min.

[0085] Step 3: Hydrothermal synthesis reaction

[0086] The reaction vessel was heated by its own jacket and casing (220°C oil bath), the reaction temperature was maintained at 150°C, and the reaction was carried out for 2 hours;

[0087] The other steps are the same as those in Example 1, and the performance testing method is the same as that in Example 1.

[0088] The scanning electron microscope image of the material is as follows Figure 2 As shown, it can be seen that the lithium iron manganese phosphate particles prepared by the conventional hydrothermal synthesis method are coarse and cannot reach the nanometer level, and the particle uniformity is poor. The electrochemical performance test results are shown in Table 1, and its electrochemical performance is significantly reduced.

[0089] Comparative Example 2

[0090] The raw material ratio is the same as that in Example 2, that is, recycled lithium phosphate is used, and the preparation method is the same as that in Comparative Example 1.

[0091] Specifically, a hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles comprises the following steps:

[0092] Step 1: Prepare a mixed slurry of lithium, iron, manganese and phosphorus raw materials

[0093] (1) Preparation of phosphorus source and lithium source mixed slurry: 0.6 kmol (on a dry basis) of wet lithium phosphate crystals obtained by recovering the mother liquor is directly added to batching kettle 1, and then 1.2 kmol of lithium hydroxide monohydrate is added to batching kettle 1, and water is added to dissolve the solution to make the volume of the solution 1m 3 , add 0.4 kmol phosphoric acid (about 30 L) under stirring. After the addition, purge the air in the dead volume of the kettle with inert gas, seal the batching kettle 1, and obtain slurry A with a volume of about 1.0 m 3 ;

[0094] (2) Prepare a mixed solution of iron source and manganese source: Take 0.3 kmol of ferrous sulfate heptahydrate and 0.7 kmol of manganese sulfate dihydrate, add water to a volume of 1 m 3 , stir until completely dissolved, filter through a pipeline precision filter, and transfer to batching kettle 2 to obtain slurry B with a volume of about 1.0m 3 ;

[0095] (3) Mixing slurry A and slurry B: Open the liquid-sealed exhaust valve of batching kettle 1 under room temperature and stirring, and add the solution in batching kettle 2 to batching kettle 1. After the addition is completed, continue stirring for 20-30 minutes to obtain slurry C with a volume of about 2m 3 ;

[0096] The molar ratio of the added substances is Li:M(Fe+Mn):P=3.0:1.0:1.0, wherein Fe:Mn (molar ratio)=3:7. After the addition is completed, the total concentration of iron and manganese elements in the solution is about 0.5 mol / L.

[0097] Step 2: Use a high-pressure pump to transport the slurry C obtained in the first step into a 3m 3 In the high-pressure reactor, the reactor is heated by jacket electric heating. Due to the limitation of heating power (heat exchange area, oil temperature, equipment wall thickness, etc.), it took 70 minutes for the temperature of the reactor to rise from 20°C to 150°C, which is equivalent to a heating rate of 1.86°C / min.

[0098] Step 3: Hydrothermal synthesis reaction

[0099] The reaction vessel was heated by its own jacket and casing (220°C oil bath), the reaction temperature was maintained at 150°C, and the reaction was carried out for 2 hours;

[0100] The other steps are the same as those in Example 1, and the performance testing method is the same as that in Example 1.

[0101] In this comparative example, the obtained lithium iron manganese phosphate particles are coarse, and the slurry is separated immediately after the third step of discharging. The electrochemical performance of the obtained product is worse than that of Comparative Example 1, and the specific test results are shown in Table 1. This shows that when the lithium iron manganese phosphate is prepared at a lower heating rate by using the relatively coarse lithium phosphate recovered instead of the newly prepared lithium phosphate on site, the particle size of the raw material lithium phosphate also has an adverse effect on the performance of the final product.

[0102] Table 1 Electrochemical performance test results

[0103] <![CDATA[0.2 C specific capacity / mAh g -1 > <![CDATA[Specific capacity at 0.2C at -20℃ / mAh g -1 > Example 1 149.9 120.2 Example 2 149.4 119.5 Example 3 153.6 124.5 Comparative Example 1 118.4 -- Comparative Example 2 112.2 --

[0104] From the above data, it can be seen that compared with the in-kettle heating method of the traditional technology, the preheating unit in the present invention has fast heat transfer. At the same time, compared with direct steam heating, it not only does not reduce the concentration of reactants, but also overcomes the adverse effects of the large lithium phosphate particles obtained by mother liquor recovery, and can increase the concentration of reactants, thereby increasing the production capacity of unit equipment. The prepared material has uniform particles, the morphology changes from flake to spherical, the scale can reach nanometer level, and the rate performance and low temperature performance of the material are good and stable. By controlling the heating link, the problem of product particle size, morphology and crystal structure of iron-lithium ion misalignment is fundamentally solved, avoiding the excessively high pressure resistance requirements for equipment caused by blindly increasing the reaction temperature. The reaction conditions of the present invention are relatively mild, the process is simple and controllable, and the batch stability of the product is good, which provides technical guarantee for large-scale industrial production.

[0105] The present invention is further described above with the aid of specific embodiments. However, it should be understood that the specific description here should not be construed as limiting the essence and scope of the present invention. Various modifications made to the above embodiments by ordinary technicians in the field after reading this specification are all within the scope of protection of the present invention.

Claims

1. A hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles, characterized in that: The following steps are involved: (1) adding a mixture of a lithium source and a phosphorus source into a batching kettle, purging the air in the dead volume of the kettle with an inert gas, sealing the batching kettle, opening the feed valve and exhaust valve of the batching kettle, adding a mixed solution of a pure iron source and a manganese source under stirring, sealing the batching kettle after the addition is completed, and continuing to stir for 10-30 minutes to obtain a mixed slurry; (2) The mixed slurry in the batching kettle is transported to a preheating unit for preheating. The outlet slurry temperature of the preheating unit is 140-160° C. The heated mixed slurry is then transported to a reactor preheated to 140-160° C. The air in the dead volume of the reactor has been purged with inert gas in advance. After all the mixed slurries are heated and transported, the reactor is sealed; (3) The reactor is stirred and maintained at 140-160° C. for 2-4 hours, then the heating is stopped and the temperature is cooled to 70-80° C.; (4) opening the discharge valve of the reactor, filtering the product and washing until there is no sulfate ion, obtaining a filter cake and a mother liquor, washing the filter cake, and drying it to obtain lithium iron manganese phosphate powder; (5) mixing the lithium iron manganese phosphate powder and the carbon source, and calcining at 700° C. for 4 hours under the protection of an inert gas to obtain carbon-coated lithium iron manganese phosphate; Wherein, the manganese source accounts for 0-70% of the total molar amount of the iron source and the manganese source; The inlet slurry temperature of the preheating unit is 20-30°C, the outlet slurry temperature is 140-160°C, and the slurry heating time in the preheating unit does not exceed 25 minutes.

2. The hydrothermal synthesis method of lithium manganese iron phosphate nanoparticles according to claim 1, characterized in that: The preheating unit is composed of a plurality of tubular preheaters connected in parallel, and the tubular preheaters are heated by a high-temperature oil bath or electric heating.

3. The hydrothermal synthesis method of lithium manganese iron phosphate nanoparticles according to claim 1, characterized in that: The preheating temperature of the reactor in step (2) is lower than the outlet slurry temperature of the preheating unit.

4. The hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles according to claim 1, characterized in that: The molar ratio of the substances added in step (1) is Li:M(Fe+Mn):P=3.0:(0.99-1.0):1.0; after the addition is completed, the total concentration of iron and manganese elements is 0.5-0.7 mol / L.

5. The hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles according to claim 1, characterized in that: In step (1), lithium hydroxide is dissolved in water and mixed with phosphoric acid as a lithium source and a phosphorus source; or lithium phosphate recovered from the mother liquor is mixed with a required amount of lithium hydroxide solution and phosphoric acid as a lithium source and a phosphorus source; or lithium phosphate is used alone as a lithium source and a phosphorus source.

6. The hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles according to claim 1, characterized in that: The mother liquor obtained by filtration in step (4) and the primary washing water of the filter cake are combined, evaporated and concentrated, and the lithium phosphate is recovered.

7. The hydrothermal synthesis method of lithium manganese iron phosphate nanoparticles according to claim 1, characterized in that: The iron source is ferrous sulfate crystals or liquid before crystallization, and the manganese source is manganese sulfate.

8. The hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles according to claim 1, characterized in that: In step (5), the lithium iron manganese phosphate powder and the carbon source are mixed in a mass ratio of 100:(10-15).

9. The hydrothermal synthesis method of lithium iron manganese phosphate nanoparticles according to claim 1, characterized in that: The carbon source is glucose.