Polar polymer / sulfonated polyarylether polymer composite, ion exchange membrane and preparation method thereof

Through the composite of polar polymer and sulfonated polyarylether polymer, a hydrogen bond network and a non-covalent bond crosslinking structure are formed, which solves the stability of polyarylether ion exchange membrane under high humidity conditions and Mechanical performance issues have enabled the preparation of high-performance ion exchange membranes and are suitable for a variety of industrial applications.

CN114634682BActive Publication Date: 2024-12-03STATE POWER INVESTMENT CORP HYDROGEN ENERGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210397344.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-15
Publication Date
2024-12-03
Estimated Expiration
2042-04-15

AI Technical Summary

Technical Problem

The existing polyarylether ion exchange membranes have poor dimensional stability, physical and mechanical properties, chemical stability and barrier properties under high humidity conditions, and the crosslinking process is difficult to achieve, which affects its performance in fuel cells and other applications.

Method used

Polar polymer/sulfonated polyarylether polymer composite is used to form a hydrogen bond network to improve ion transport efficiency by introducing polar polymers with low water absorption, and a non-covalent bond crosslinking structure is used to facilitate Recover and prepare high-performance non-crosslinked ion exchange membranes.

Benefits of technology

It effectively reduces the water absorption of the composite, improves mechanical properties and chemical stability, solves the problem of excessive water absorption of sulfonated polyarylether polymers, and realizes the preparation of high-performance ion exchange membranes, suitable for chlor-alkali industry, Hydrogen production in water electrolysis and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114634682B_ABST
    Figure CN114634682B_ABST
Patent Text Reader

Abstract

The present invention provides a polar polymer / sulfonated polyarylether polymer composite, an ion exchange membrane and a preparation method thereof. The polar polymer / sulfonated polyarylether polymer composite comprises a polar polymer and a sulfonated polyarylether polymer, wherein the mass content of the polar polymer is 0.1% to 95%; the water absorption rate of the polar polymer at 25°C is less than 30%, and the polar polymer is insoluble in water. By introducing a polar polymer with low water absorption rate, the present application can effectively reduce the water absorption of the composite, and solves the problem that the water absorption of the sulfonated polyarylether polymer is too high, resulting in high swelling, poor membrane dimensional stability, physical and mechanical properties, chemical stability and barrier properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a polar polymer / sulfonated polyarylether polymer composite, an ion exchange membrane and a preparation method thereof. Background Art

[0002] Ion exchange membranes are widely used in fuel cells, chlor-alkali industry, flow batteries, water electrolysis for hydrogen production, membrane separation technology and protective materials. The good comprehensive properties of perfluorosulfonic acid resin make it the most successful material used in ion exchange membranes. However, fluorine-containing materials are expensive and the production process is not environmentally friendly, so non-fluorine proton exchange membranes have always been a hot topic of research. In past studies, the substrates selected for non-fluorine proton exchange membranes were mainly aromatic polymers containing benzene rings or polymers containing functional groups such as hydroxyl, amine, chloromethyl, and carboxyl. Other polymer matrices, such as oxygenated aliphatic hydrocarbon polymers, polycarbonates and polyolefin materials can also be used to prepare proton exchange membranes, but they have been less studied and their performance is not ideal. Therefore, the current main research direction is still aromatic polymer proton exchange membrane materials, and polyarylether polymers have been studied the most and most deeply.

[0003] Polyarylether polymers include polyarylethersulfone, polyarylethernitrile, polyethersulfone, polyetheretherketone and their derivatives, which have good mechanical properties, anti-oxidation and anti-acid catalytic hydrolysis properties, low manufacturing cost, low hydrocarbon fuel permeability and good film-forming properties. Hydrophilic groups (mainly sulfonic acid groups) are inserted into the polymer main chain to improve its hydrophilic properties, and it can be applied to ion exchange membranes. In addition to using sulfonation reagents such as concentrated sulfuric acid, chlorosulfonic acid and acylsulfonic acid to sulfonate the position of the polyarylether polymer benzene ring, direct polymerization of monomers containing sulfonic acid groups can also obtain sulfonated polyarylether polymers with more clear structures and sulfonation degrees. In order to improve the stability of the sulfonic acid groups on the benzene rings and prevent the occurrence of side reactions and degradation reactions, the improvement method is mainly to graft rigid arylsulfonic acid side chains or alkylsulfonic acid and fluoroalkylsulfonic acid side chains on the main chain benzene rings. Another limitation of the ion exchange membrane performance of polyarylether substrates is that the high sulfonation degree polymer materials have poor dimensional stability, large swelling degree, and are easy to dissolve in water. Cross-linking sulfonated polymers or designing different main chain structures and grafting different types of side chains can better control the hydrophilicity of the membrane, but the cross-linked structure is difficult to achieve in terms of technology, which is not conducive to the recovery of the catalyst, so it is difficult to apply it on a large scale on the production line. At the same time, in the process of preparing membrane electrodes, cross-linked polymers as polyelectrolytes cannot be dispersed in the catalyst slurry, which is not conducive to the preparation of membrane electrodes.

[0004] In the prior art, the ion transport capacity of random copolymerized sulfonated poly(aryletherketone) ion exchange membranes depends on the increase of the sulfonic acid group content, but as the degree of sulfonation and IEC increase, the water absorption of the ion exchange membrane increases sharply, resulting in a sharp decrease in the membrane's dimensional stability, physical and mechanical properties, chemical stability, and barrier properties. This defect limits the application of sulfonated poly(aryletherketone) in high-humidity conditions such as fuel cell proton exchange membranes, electrodialysis membranes, and water electrolysis membranes. The preparation of sulfonated poly(aryletherketone) ion exchange membranes by covalent cross-linking effectively overcomes a series of problems caused by excessive water absorption, but the cross-linking structure process is difficult to achieve, which is not conducive to recovery, and cross-linked polymers are difficult to use as polyelectrolytes for catalyst slurries. Summary of the invention

[0005] The main purpose of the present invention is to provide a polar polymer / sulfonated polyarylether polymer composite, an ion exchange membrane and a preparation method thereof, so as to solve the problems of poor membrane dimensional stability, physical and mechanical properties, chemical stability and barrier properties in the polyarylether ion exchange membrane in the prior art.

[0006] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a polar polymer / sulfonated polyarylether polymer complex is provided, wherein the polar polymer / sulfonated polyarylether polymer complex comprises a polar polymer and a sulfonated polyarylether polymer, wherein the mass content of the polar polymer is 0.1% to 95%; the water absorption rate of the polar polymer at 25°C is less than 30%, and the polar polymer is insoluble in water.

[0007] Furthermore, the polar group of the polar polymer is selected from any one or more of a nitrile group, a phenolic hydroxyl group, an alcoholic hydroxyl group, a phosphate group, a phosphite group or an imide ring, and preferably the polar polymer includes any one or more of polyphosphate, polyphosphate block copolymer, polyurethane, polyaminophosphoester, aminophosphite polymer, ethylene-vinyl alcohol copolymer, and polyimide.

[0008] Furthermore, the polyphosphate block copolymer includes a diblock copolymer or a triblock copolymer formed by a phosphate and at least one of ethylene glycol, ethylene glycol monomethyl ether, caprolactone or propylene; preferably, the ethylene molar content of the ethylene-vinyl alcohol copolymer is 25% to 60%, and the degree of alcoholysis is not less than 95%; preferably, the melt index of the ethylene-vinyl alcohol copolymer is 2.2 to 15.2 g / 10min, preferably 2.7 to 14.7 g / 10min, and more preferably 2.9 to 13.9 g / 10min; preferably, the polyimide is a soluble polyimide.

[0009] Furthermore, the sulfonated polyarylether polymer has a structure shown in Formula I: Wherein m is 1 to 20, n is 1 to 10;

[0010] Ar1 represents One or more of;

[0011] Ar2 represents One or more of;

[0012] Ar3 represents One or more of .

[0013] Further, the sulfonated polyarylether polymer is

[0014] One or more of .

[0015] Furthermore, the polar polymer is selected from One or more of, wherein a ranges from 1 to 30, b ranges from 5 to 25, x ranges from 1 to 20, y ranges from 3 to 22, z ranges from 20 to 35, p ranges from 15 to 20, f ranges from 1 to 10, g ranges from 1 to 15, h ranges from 4 to 28, and c ranges from 8 to 21.

[0016] Furthermore, in the polar polymer / sulfonated polyarylether polymer composite, the mass content of the polar polymer is 1% to 90%, preferably 1.5 to 85%.

[0017] In order to achieve the above object, according to one aspect of the present invention, an ion exchange membrane is provided. The ion exchange membrane comprises the above polar polymer / sulfonated polyarylether polymer composite.

[0018] According to another aspect of the present invention, a method for preparing the above-mentioned ion exchange membrane is provided, which comprises: dissolving and dispersing a polar polymer / sulfonated polyarylether polymer complex in an organic medium to obtain a complex dispersion; making the complex dispersion into a wet film and then drying it to obtain an ion exchange membrane.

[0019] Furthermore, the organic medium is selected from at least one of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone.

[0020] Furthermore, the drying temperature is 70 to 90° C., and the drying time is 24 to 36 hours.

[0021] By applying the technical solution of the present invention, the present application can effectively reduce the water absorption of the composite by introducing a polar polymer with low water absorption, and solves the problem that the high water absorption of sulfonated polyarylether polymers leads to high swelling, decreased membrane dimensional stability, physical and mechanical properties, chemical stability and barrier properties. If the content of polar polymer is too high, it will affect the conductivity and water absorption; if the content of polar polymer is too low, it will reduce the physical and chemical stability of the membrane. Therefore, it is necessary to adjust the ratio between polar polymer and sulfonated polyarylether polymer to effectively regulate the hydrophilicity of the composite and design a suitable water absorption rate as needed. At the same time, the polar groups in the polar polymer and the sulfonic acid groups in the sulfonated polyarylether polymer have hydrogen bonding, and the three-dimensional hydrogen bonding network formed is conducive to the transmission of ions, so that the ion transmission efficiency is improved without increasing the degree of sulfonation, thereby achieving the improvement of the mechanical properties, chemical stability and barrier properties of the material by controlling the degree of sulfonation. At the same time, under the above-mentioned hydrogen bonding, the polar polymer and the sulfonated polyarylether polymer can be evenly mixed, which is conducive to the preparation of polymer membranes. The polar polymer / sulfonated polyarylether polymer composite of the present application is a non-covalent cross-linked structure, which enables the composite to be easily dissolved and dispersed by solvents. This solubility is conducive to the recovery of the composite itself and its products, and is conducive to the preparation of catalyst slurry and membrane electrode. The polar polymer / sulfonated polyarylether polymer composite of the present application solves the problem of excessively high water absorption of sulfonated polyarylether polymers, while overcoming the problem that the cross-linking process of covalently cross-linked sulfonated polyarylether compounds is difficult to implement, and can be used to prepare high-performance non-cross-linked ion exchange membranes. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0023] Figure 1 The conductivity of the ion exchange membranes in Examples 7-9 of the present invention at different temperatures at 95% RH is shown;

[0024] Figure 2 The conductivity of the ion exchange membranes in Examples 13-18 of the present invention at different temperatures at 95% RH is shown;

[0025] Figure 3 The polarization curves of the ion exchange membranes in Examples 13 and 18 of the present invention at 80° C. and 95% RH are shown;

[0026] Figure 4 The polarization curve of the ion exchange membrane in Comparative Example 5 of the present invention is shown. DETAILED DESCRIPTION

[0027] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0028] As analyzed in the background technology of this application, the prior art has the problems of poor membrane dimensional stability, physical and mechanical properties, chemical stability and barrier properties in polyarylether ion exchange membranes. In order to solve these problems, this application provides a polar polymer / sulfonated polyarylether polymer composite, an ion exchange membrane and a preparation method thereof.

[0029] In a typical embodiment of the present application, a polar polymer / sulfonated polyarylether polymer complex is provided, wherein the polar polymer / sulfonated polyarylether polymer complex comprises a polar polymer and a sulfonated polyarylether polymer, wherein the mass content of the polar polymer is 0.1% to 95%; the water absorption rate of the polar polymer at 25°C is less than 30%, and the polar polymer is insoluble in water.

[0030] The present application can effectively reduce the water absorption of the composite by introducing a polar polymer with low water absorption, and solves the problem that the high water absorption of sulfonated polyarylether polymers leads to high swelling, membrane dimensional stability, physical and mechanical properties, chemical stability and barrier properties. If the content of polar polymer is too high, it will affect the conductivity and water absorption; if the content of polar polymer is too low, it will reduce the physical and chemical stability of the membrane. Therefore, it is necessary to adjust the ratio between polar polymer and sulfonated polyarylether polymer to effectively regulate the hydrophilicity of the composite and design a suitable water absorption rate as needed. At the same time, the polar groups in the polar polymer and the sulfonic acid groups in the sulfonated polyarylether polymer have hydrogen bonding, and the three-dimensional hydrogen bonding network formed is conducive to the transmission of ions, so the ion transmission efficiency is improved without increasing the degree of sulfonation, thereby achieving the improvement of the mechanical properties, chemical stability and barrier properties of the material by controlling the degree of sulfonation. At the same time, under the above-mentioned hydrogen bonding, the polar polymer and the sulfonated polyarylether polymer can be evenly mixed, which is conducive to the preparation of polymer membranes. The polar polymer / sulfonated polyarylether polymer composite of the present application is a non-covalent cross-linked structure, which enables the composite to be easily dissolved and dispersed by solvents. This solubility is conducive to the recovery of the composite itself and its products, and is conducive to the preparation of catalyst slurry and membrane electrode. The polar polymer / sulfonated polyarylether polymer composite of the present application solves the problem of excessively high water absorption of sulfonated polyarylether polymers, while overcoming the problem that the cross-linking process of covalently cross-linked sulfonated polyarylether compounds is difficult to implement, and can be used to prepare high-performance non-cross-linked ion exchange membranes.

[0031] Since the composite has improved water absorption and mechanical properties under high humidity conditions, it can be applied to chlor-alkali industrial diaphragms, polyelectrolyte membranes for water electrolysis and hydrogen production, separation membranes, membrane reactors and humidity sensors.

[0032] In order to make the composite have a suitable water absorption rate, the water absorption rate of the polar polymer should not be too high; at the same time, in order to form a more stable hydrogen bond with the sulfonic acid group of the sulfonated polyarylether polymer, in some embodiments, the polar group of the polar polymer is preferably selected from any one or more of nitrile group, phenolic hydroxyl group, alcoholic hydroxyl group, phosphate group, phosphite group or imide ring. There are many polar polymers that can achieve the above functions and have the above polar groups. In order to improve the synergistic composite effect of the polar polymer and the sulfonated polyarylether polymer and better meet the functional requirements of the ion exchange membrane, the polar polymer preferably includes any one or more of polyphosphate, polyphosphate block copolymer, polyurethane, polyamino phosphate, amino phosphite polymer, ethylene-vinyl alcohol copolymer, and polyimide. Preferably, the polyphosphate block copolymer is a diblock copolymer or a triblock copolymer formed by a phosphate and at least one of ethylene glycol, ethylene glycol monomethyl ether, caprolactone or propylene; the ethylene-vinyl alcohol copolymer can be an ethylene-vinyl alcohol copolymer commonly used in the prior art. According to the degree of saponification and alcoholysis, the ethylene molar content of the ethylene-vinyl alcohol copolymer is preferably 25% to 60%, and the alcoholysis degree is not less than 95%. The melt index of the ethylene-vinyl alcohol copolymer is preferably 2.2 to 15.2 g / 10 min, preferably 2.7 ~14.7g / 10min, more preferably 2.9~13.9g / 10min; The above-mentioned polyimide is a soluble polyimide. The present application can improve the solubility by introducing flexible groups such as ether bonds, siloxy bonds, carbonyl groups, sulfone groups, isopropylidene and alkyl groups into the main chain of the polyimide, and / or introducing large side groups such as tert-butyl groups, benzene rings, trifluoromethyl groups into the main chain, and / or introducing fluorine-containing groups into the main chain. Preferably, the polyimide has fluorine-containing groups in the main chain, and / or the main chain contains ether bonds, and or the main chain introduces trifluoromethyl groups. For example The value of c ranges from 8 to 15, preferably c=15, 12 or 8.

[0033] In order to make the composite have good mechanical properties and obtain good film-forming properties, a sulfonated polyarylether compound with a high degree of sulfonation is selected. In some embodiments, the sulfonated polyarylether polymer has a structure shown in Formula I: wherein m is 1 to 20, n is 1 to 10, and the degree of sulfonation is ensured to be 70% to 100%;

[0034] Ar1 represents

[0035] Ar2 represents

[0036] Ar3 represents

[0037] In some embodiments, the sulfonated polyarylether polymer is:

[0038] One or more of .

[0039] The ion transport capacity of the polar polymer itself is negligible, but the hydrogen bonding between the polar groups of these polar polymers and the sulfonic acid groups can effectively improve the material properties. In some embodiments, the polar polymer is selected from

[0040]

[0041] One or more of, wherein a ranges from 1 to 30, b ranges from 5 to 25, x ranges from 1 to 20, y ranges from 3 to 22, z ranges from 20 to 35, p ranges from 15 to 20, f ranges from 1 to 10, g ranges from 1 to 15, h ranges from 4 to 28, and c ranges from 8 to 21.

[0042] The polar polymer and the sulfonated polyarylether polymer in the present application can be blended in any proportion to obtain a composite, and the water absorption rate of the composite can be regulated by changing the mass content of the polar polymer in the composite, thereby regulating the hydrophilicity of the composite. In some embodiments, in the polar polymer / sulfonated polyarylether polymer composite, the mass content of the polar polymer is 1% to 90%, preferably 1.5 to 85%. The mass content of the polar polymer is controlled within this range to maintain relatively stable physical and chemical properties and high conductivity.

[0043] In another typical embodiment of the present application, an ion exchange membrane is provided. The ion exchange membrane includes the above-mentioned polar polymer / sulfonated polyarylether polymer composite.

[0044] The ion exchange membrane having the above-mentioned polar polymer / sulfonated polyarylether polymer composite can reduce water absorption and ion exchange capacity (IEC), but the physical cross-linking structure between molecules improves the proton transmission ability, so that the ion exchange membrane has a higher proton conductivity, thereby solving the problem of high swelling caused by high water absorption, decreased membrane dimensional stability, physical and mechanical properties, chemical stability and barrier properties.

[0045] In another typical embodiment of the present application, a method for preparing the above-mentioned ion exchange membrane is provided, which comprises: dissolving and dispersing the polar polymer / sulfonated polyarylether polymer complex in an organic medium to obtain a complex dispersion; making the complex dispersion into a wet film and then drying it to obtain an ion exchange membrane.

[0046] Due to the solubility of the polar polymer / sulfonated polyarylether polymer complex, the complex can be dissolved and dispersed in an organic medium to obtain a complex dispersion, and then the dispersion is used to prepare an ion exchange membrane. The reaction conditions of the present application are mild, the method is simple, and it is easy to implement. The ion exchange membrane with the above-mentioned polar polymer / sulfonated polyarylether polymer complex can reduce water absorption and ion exchange capacity (IEC), but the physical cross-linking structure between molecules improves the proton transmission capacity, so that the ion exchange membrane has a higher proton conductivity, thereby solving the problem of high swelling caused by high water absorption, membrane dimensional stability, physical and mechanical properties, chemical stability and reduced barrier properties.

[0047] All methods of preparing wet film from composite dispersion in the prior art can be applied to the present application. In some embodiments, wet film can be prepared by casting, coating or pouring.

[0048] In order to enable the composite to be completely dissolved and dispersed in the organic medium, the mass ratio of the composite to the organic medium is controlled to be 50:1 to 4:1.

[0049] The present application has no particular restrictions on the type of organic medium, and any organic medium commonly used in the art can be applied to the present application. In some embodiments, the organic medium is selected from at least one of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, or N-methylpyrrolidone.

[0050] In order to evaporate and remove the organic medium without damaging the structure of the ion exchange membrane, in some embodiments, the drying temperature is 70 to 90° C. and the drying time is 24 to 36 hours.

[0051] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0052] The phosphate copolymer in the present application is prepared in the laboratory. The preparation method of the copolymer is as follows: using styrene-terminated polypropylene as a starting material, polypropylene terminated with benzyl bromide groups is obtained by Markovnikov addition reaction, and 4-vinylbenzylphosphonic acid diethyl is polymerized by atom transfer radical polymerization to synthesize the phosphate copolymer.

[0053] The polyphosphate diblock copolymer used in the examples of the present application has the structural formula

[0054] Among them, a=1200, b=300.

[0055] It should be noted that the polar groups in this application may be weakly acidic or weakly alkaline, but except for some phosphates and phosphites, others do not have ion exchange capacity like carboxylic acid, sulfonic acid, phosphoric acid, quaternary ammonium, nitrogen onium and other groups. The reason why some phosphates and phosphites have IEC is that there may be a P-OH bond and POC coexisting in the functional group. At this time, the P-OH bond in the functional group is no different from the P-OH bond in phosphoric acid, so it has ion exchange capacity and can characterize the IEC value.

[0056] The above polyphosphate diblock copolymer has only POC bonds and no P-OH bonds, so the copolymer has no IEC.

[0057] The structural formula of the polyphosphate triblock copolymer prepared by ring-opening copolymerization is

[0058] Among them, x=23, y=16, z=15, p=3, and IEC is 0.39 mmol / g.

[0059] Polyaminophosphoric acid ester (PAPE), PAPE is a compound known in the prior art, which can be synthesized according to the method in the prior art or purchased commercially. The structural formula of PAPE is

[0060] Where d = 25. PAPE does not have IEC.

[0061] The structural formula of the aminophosphite polymer synthesized by reacting ethylenediamine with an aqueous solution of hypophosphorous acid under acidic conditions (pH = 1) is:

[0062] Wherein, e=27, and the IEC of the aminophosphite polymer is 2.2 mmol / g.

[0063] The structural formula of ethylene-vinyl alcohol copolymer (EVOH) is

[0064] Wherein, ethylene molar content = f / (f+g+h)*100%; alcoholysis degree = g / (g+h)*100%. Wherein, f accounts for the ethylene molar content, h accounts for the alcoholysis degree (saponification degree), and the melt index of the polymer is 2.2-15.2 g / 10min. The EVOH used in the examples of this application is shown in Table 1.

[0065] Table 1

[0066]

[0067] The structural formula of the soluble polyimide prepared by stepwise polymerization is

[0068] Among them, c=15.

[0069] The structural formula of sulfonated polyetheretherketone (SPAEK-1) is

[0070] The polymer has an IEC of 1.86 mmol / g and is obtained by polymerization of 4,4-difluorobenzophenone, hexafluorobisphenol A and methoxyhydroquinone at 170°C.

[0071] The structural formula of sulfonated polyetheretherketone (SPAEK-2) is

[0072] The IEC of the polymer was 1.91 mmol / g.

[0073] The structural formula of sulfonated polyetheretherketone (SPAEK-3) is

[0074] The IEC of the polymer was 1.85 mmol / g.

[0075] The structural formula of sulfonated polyarylethersulfone (SPAES) is

[0076] The polymer has an IEC of 1.79 mmol / g and is obtained by polymerization of 4,4-difluorodiphenyl sulfone, hexafluorobisphenol A and methoxyhydroquinone at 170°C.

[0077] The structural formula of sulfonated poly(arylether nitrile) (SPAEN) is

[0078] The polymer has an IEC of 1.83 mmol / g and is obtained by polymerization of 2,6-difluorobenzonitrile, hexafluorobisphenol A and methoxyhydroquinone at 170°C.

[0079] The structural formula of sulfonated polyaryletherketone (SPAEK) is

[0080] The IEC of the polymer was 1.82 mmol / g.

[0081] Example 1

[0082] 0.3 parts by mass of a polyphosphoric acid diblock copolymer and 0.7 parts by mass of a sulfonated polyetheretherketone (SPAEK-1) were dissolved and dispersed in 9 parts by mass of N,N-dimethylacetamide (DMAc) to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 24 hours to obtain a non-cross-linked ion exchange membrane (M-1).

[0083] Example 2

[0084] 0.3 parts by mass of polyphosphate triblock copolymer and 0.7 parts by mass of sulfonated polyetheretherketone (SPAEK-1) were dissolved and dispersed in 9 parts by mass of N,N-dimethylacetamide (DMAc) to obtain a composite dispersion; the composite dispersion was cast in an ultra-flat mold and dried at 80°C for 24 hours to obtain a non-cross-linked ion exchange membrane (M-2).

[0085] Example 3

[0086] 0.3 parts by mass of polyaminophosphate (PAPE) and 0.7 parts by mass of sulfonated polyetheretherketone (SPAEK-1) were dissolved and dispersed in 9 parts by mass of N,N-dimethylacetamide (DMAc) to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 24 hours to obtain a non-cross-linked ion exchange membrane (M-3).

[0087] Example 4

[0088] 0.3 parts by mass of aminophosphite polymer and 0.7 parts by mass of sulfonated polyetheretherketone (SPAEK-1) were dissolved and dispersed in 9 parts by mass of N,N-dimethylacetamide (DMAc) to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 24 hours to obtain a non-cross-linked ion exchange membrane (M-4).

[0089] Example 5

[0090] 0.3 parts by mass of ethylene-vinyl alcohol copolymer (EVOH-1) and 0.7 parts by mass of sulfonated polyetheretherketone (SPAEK-1) were dissolved and dispersed in 9 parts by mass of N,N-dimethylacetamide (DMAc) to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 24 hours to obtain a non-cross-linked ion exchange membrane (M-5).

[0091] Example 6

[0092] 0.3 parts by mass of soluble polyimide and 0.7 parts by mass of sulfonated polyetheretherketone (SPAEK-1) were dissolved and dispersed in 9 parts by mass of N,N-dimethylacetamide (DMAc) to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 24 hours to obtain a non-cross-linked ion exchange membrane (M-6).

[0093] The properties of the ion exchange membranes prepared in Examples 1-6 are shown in Table 2, wherein the temperature for the conductivity test is 80° C. and the humidity is 95% RH (relative humidity).

[0094] Table 2

[0095]

[0096] Example 7

[0097] 0.3 parts by mass of soluble polyimide and 0.7 parts by mass of sulfonated polyarylethersulfone (SPAES) were dissolved and dispersed in 9 parts by mass of DMSO to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 36 hours to obtain a non-cross-linked ion exchange membrane (M-7).

[0098] Example 8

[0099] 0.3 parts by mass of soluble polyimide and 0.7 parts by mass of sulfonated polyarylethernitrile (SPAEN) were dissolved and dispersed in 9 parts by mass of DMSO to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 36 hours to obtain a non-cross-linked ion exchange membrane (M-8).

[0100] Example 9

[0101] 0.3 parts by mass of soluble polyimide and 0.7 parts by mass of sulfonated polyaryletherketone (SPAEK) were dissolved and dispersed in 9 parts by mass of DMSO to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 36 hours to obtain a non-cross-linked ion exchange membrane (M-9).

[0102] The performance of the ion exchange membranes prepared in Examples 7-9 is shown in Table 3. The conductivity data in the table are measured at 80°C and 95% RH. Figure 1 shown.

[0103] Table 3

[0104]

[0105] Example 10

[0106] 0.01 parts by mass of polyaminophosphate (PAPE) and 0.99 parts by mass of sulfonated polyetheretherketone (SPAEK-1) were dissolved and dispersed in 9 parts by mass of N,N-dimethylacetamide (DMAc) to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 24 hours to obtain a non-cross-linked ion exchange membrane (M-10).

[0107] Embodiment 11

[0108] 0.5 parts by mass of polyaminophosphate (PAPE) and 0.5 parts by mass of sulfonated polyetheretherketone (SPAEK-1) were dissolved and dispersed in 9 parts by mass of N,N-dimethylacetamide (DMAc) to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 24 hours to obtain a non-cross-linked ion exchange membrane (M-11).

[0109] Example 12

[0110] 0.95 parts by mass of polyaminophosphate (PAPE) and 0.05 parts by mass of sulfonated polyetheretherketone (SPAEK-1) were dissolved and dispersed in 9 parts by mass of N,N-dimethylacetamide (DMAc) to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 24 hours to obtain a non-cross-linked ion exchange membrane (M-12).

[0111] The properties of the ion exchange membranes prepared in Examples 10-12 are shown in Table 4, wherein the conductivity data are measured at 80° C. and 95% RH.

[0112] Table 4

[0113]

[0114] Because PAPE itself has low strength and high toughness, but after blending with SPAEK-1, PAPE and SPEEK can synergistically enhance toughness, so Example 10 has the best effect. There is less PAPE in Example 10, and less SPAEK-1 in Example 12, and the synergistic effect is poor.

[0115] Example 13

[0116] 0.3 parts by mass of EVOH-2 and 0.7 parts by mass of sulfonated polyetheretherketone (SPAEK-3) were dissolved and dispersed in 9 parts by mass of DMF to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 12 hours to obtain a non-cross-linked ion exchange membrane (M-13).

[0117] Embodiment 14

[0118] 0.3 parts by mass of EVOH-3 and 0.7 parts by mass of sulfonated polyetheretherketone (SPAEK-3) were dissolved and dispersed in 9 parts by mass of DMF to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 12 hours to obtain a non-cross-linked ion exchange membrane (M-14).

[0119] Embodiment 15

[0120] 0.3 parts by mass of EVOH-4 and 0.7 parts by mass of sulfonated polyetheretherketone (SPAEK-3) were dissolved and dispersed in 9 parts by mass of DMF to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 12 hours to obtain a non-cross-linked ion exchange membrane (M-15).

[0121] Example 16

[0122] 0.3 parts by mass of EVOH-5 and 0.7 parts by mass of sulfonated polyetheretherketone (SPAEK-3) were dissolved and dispersed in 9 parts by mass of DMF to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 12 hours to obtain a non-cross-linked ion exchange membrane (M-16).

[0123] Embodiment 17

[0124] 0.3 parts by mass of EVOH-6 and 0.7 parts by mass of sulfonated polyetheretherketone (SPAEK-3) were dissolved and dispersed in 9 parts by mass of DMF to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 12 hours to obtain a non-cross-linked ion exchange membrane (M-17).

[0125] Embodiment 18

[0126] 0.3 parts by mass of EVOH-7 and 0.7 parts by mass of sulfonated polyetheretherketone (SPAEK-3) were dissolved and dispersed in 9 parts by mass of DMF to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80°C for 12 hours to obtain a non-cross-linked ion exchange membrane (M-18).

[0127] The performance of the ion exchange membranes prepared in Examples 13-18 is shown in Table 5. The conductivity data in the table are measured at 80°C and 95% RH. The conductivity of the ion exchange membranes prepared in Examples 13-18 at different temperatures under 95% RH is shown in Table 5. Figure 2 The polarization curves of the ion exchange membranes of Example 13 and Example 18 at 80°C and 95% RH are shown in Figure 3 The hydrogen permeation current density of ion exchange membranes M-13 and M-18 is 1.27 mA / cm 2 and 1.75mA / cm 2 .

[0128] Table 5

[0129]

[0130]

[0131] Embodiment 19

[0132] 0.95 parts by mass of polyaminophosphoric acid ester (PAPE) and 0.05 parts by mass of sulfonated polyetheretherketone (SPAEK-2) were dissolved and dispersed in 9 parts by mass of N,N-dimethylacetamide (DMAc) to obtain a composite dispersion; the composite dispersion was cast in an ultra-flat mold and dried at 80°C for 24 hours to obtain a non-crosslinked ion exchange membrane (M-19). The IEC of M-19 is 0.09 mmol / g, the water absorption is 15.0%, the conductivity is 0.006 S / cm, the tensile strength is 41 MPa, and the elongation at break is 73.2%.

[0133] Embodiment 20

[0134] 0.001 parts by mass of polyaminophosphoric acid ester (PAPE) and 0.999 parts by mass of sulfonated polyetheretherketone (SPAEK-1) were dissolved and dispersed in 9 parts by mass of N,N-dimethylacetamide (DMAc) to obtain a composite dispersion; the composite dispersion was cast in an ultra-flat mold and dried at 80°C for 24 hours to obtain a non-crosslinked ion exchange membrane (M-20). The IEC of M-20 is 1.82 mmol / g, the water absorption is 47.0%, the conductivity is 0.147 S / cm, the tensile strength is 50 MPa, and the elongation at break is 34.5%.

[0135] Comparative Example 1

[0136] 1 part by mass of sulfonated polyetheretherketone (SPAEK-1) was dissolved and dispersed in 9 parts by mass of N,N-dimethylacetamide (DMAc) to obtain a polymer dispersion; the polymer dispersion was cast into an ultra-flat mold and dried at 80°C for 24 hours to obtain an ion exchange membrane (DM-1).

[0137] The IEC of DM-1 is 1.69mmol / g, the water absorption is 65.0%, the conductivity is 0.139S / cm, the tensile strength is 48MPa, and the elongation at break is 21.9%. Compared with the ion exchange membranes in Examples 1-3 and Example 5, the introduction of polar polymers improves the conductivity and enhances toughness. The introduction of EVOH in Example 5 can comprehensively improve the performance of the ion exchange membrane; compared with DM-1, the ion exchange membrane of Example 5 has a tensile strength increased by 42.5%, an elongation at break increased by about 477%, and significantly improved mechanical properties, and the conductivity at 80°C increased by about 22%. Compared with Example 6, the introduction of soluble polyimide increases strength and reduces water absorption. This is because the toughness of the soluble polyimide material itself is low.

[0138] Comparative Example 2

[0139] 1 part by mass of sulfonated polyarylethersulfone (SPAES) was dissolved and dispersed in 9 parts by mass of DMSO to obtain a polymer dispersion; the polymer dispersion was cast into an ultra-flat mold and dried at 80° C. for 36 hours to obtain an ion exchange membrane (DM-2).

[0140] Comparative Example 3

[0141] 1 part by mass of sulfonated polyarylethernitrile (SPAEN) was dissolved and dispersed in 9 parts by mass of DMSO to obtain a polymer dispersion; the polymer dispersion was cast into an ultra-flat mold and dried at 80° C. for 36 hours to obtain an ion exchange membrane (DM-3).

[0142] Comparative Example 4

[0143] 1 part by mass of sulfonated polyaryletherketone (SPAEK) was dissolved and dispersed in 9 parts by mass of DMSO to obtain a composite dispersion; the composite dispersion was cast into an ultra-flat mold and dried at 80° C. for 36 hours to obtain an ion exchange membrane (DM-4).

[0144] Compared with the non-crosslinked ion exchange membranes prepared by blending soluble polyimide and sulfonated polyarylether polymer in Comparative Examples 2-4 and Examples 7-9, the tensile strength of the membranes decreased by more than 20%.

[0145] Comparative Example 5

[0146] 1 part by mass of sulfonated polyetheretherketone (SPAEK-3) was dissolved and dispersed in 9 parts by mass of DMF to obtain a polymer dispersion; the polymer dispersion was cast into an ultra-flat mold and dried at 80° C. for 12 hours to obtain an ion exchange membrane (DM-5).

[0147] The IEC of DM-5 is 1.86mmol / g, the water absorption is 58.4%, and the conductivity is 0.169S·cm -1 , tensile strength 55MPa, elongation at break 25.5%, hydrogen permeation current density 2.64mA / cm 2 , the polarization curve is shown in Figure 4 .

[0148] Compared with the non-crosslinked ion exchange membrane prepared by blending EVOH and SPAEK-3 in Examples 13-18, the conductivity decreased by more than 6%, and the elongation at break decreased by more than 50%. Compared with the ion exchange membrane M-14, the conductivity decreased by about 14%.

[0149] The performance of the ion exchange membranes of Comparative Examples 1-5 is shown in Table 6, wherein the conductivity data are measured at 80° C. and 95% RH.

[0150] Table 6

[0151]

[0152] Test Method

[0153] The tensile properties are tested according to GB / T 1040-2006 standard.

[0154] Battery performance: Battery performance includes battery polarization curve and hydrogen permeation current density. Dalian Yuke fuel cell test bench and GAMRY electrochemical workstation are used to test the performance of single-chip batteries. The test method refers to GB / T20042.5-2009 "Proton Exchange Membrane Fuel Cell Part 5: Membrane Electrode Test Method".

[0155] Conductivity: The electrochemical workstation Metrohm Autolab PGSTAT302N was used to measure the AC impedance of the film and calculate the proton conductivity. The AC frequency was 1 to 10 5 Hz, scanning amplitude 10mV. The film was clamped according to the four-electrode method.

[0156] IEC test: The IEC values ​​of polymers and films were determined using a Titrino plus automatic potentiometric titrator.

[0157] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0158] The present application can effectively reduce the water absorption of the composite by introducing a polar polymer with low water absorption, and solve the problem of high swelling, film dimensional stability, physical and mechanical properties, chemical stability and barrier properties caused by high water absorption. By adjusting the ratio between the polar polymer and the sulfonated polyarylether polymer, the hydrophilicity of the composite can be effectively regulated, and a suitable water absorption can be designed as needed. At the same time, the polar groups in the polar polymer and the sulfonic acid groups in the sulfonated polyarylether polymer have hydrogen bonding, and the three-dimensional hydrogen bonding network formed is conducive to the transmission of ions and improves the mechanical properties of the material. Under the action of hydrogen bonding, the polar polymer and the sulfonated polyarylether polymer can be uniformly mixed, which is conducive to the preparation of polymer membranes. The polar polymer / sulfonated polyarylether polymer composite of the present application is a non-covalent cross-linked structure, which enables the composite to be easily dissolved and dispersed by solvent, and this solubility is conducive to the recovery of the composite itself and its products, and is conducive to the preparation of catalyst slurry and membrane electrode. The polar polymer / sulfonated polyarylether polymer composite of the present application solves the problem of excessively high water absorption of sulfonated polyarylether polymers while overcoming the problem of difficulty in implementing the cross-linking process of covalently cross-linked sulfonated polyarylether compounds, and can be used to prepare high-performance non-cross-linked ion exchange membranes.

[0159] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A polar polymer / sulfonated polyarylether polymer composite, characterized in that: The polar polymer / sulfonated polyarylether polymer composite comprises a polar polymer and a sulfonated polyarylether polymer, wherein the mass content of the polar polymer is 0.1% to 95%; The polar polymer has a water absorption rate of less than 30% at 25°C and is insoluble in water; The polar polymer is selected from any one or more of polyphosphate, polyphosphate block copolymer, polyaminophosphoric acid ester, aminophosphite polymer, ethylene-vinyl alcohol copolymer, and polyimide; The polyphosphate block copolymer is selected from One or more of, wherein a is in the range of 1 to 30, b is in the range of 5 to 25, x is in the range of 1 to 20, y is in the range of 3 to 22, z is in the range of 20 to 35, and p is in the range of 15 to 20; The ethylene-vinyl alcohol copolymer is selected from Among them, the range of f is 1 to 10, the range of g is 1 to 15, and the range of h is 4 to 28; The ethylene-vinyl alcohol copolymer has an ethylene molar content of 25% to 60% and an alcoholysis degree of not less than 95%; The polyimide is a soluble polyimide, and the structural formula of the polyimide is: The range of c value is 8-15.

2. The polar polymer / sulfonated polyarylether polymer composite according to claim 1, characterized in that: The melt index of the ethylene-vinyl alcohol copolymer is 2.2 to 15.2 g / 10 min.

3. The polar polymer / sulfonated polyarylether polymer composite according to claim 1, characterized in that: The ethylene-vinyl alcohol copolymer is 2.9-13.9 g / 10 min.

4. The polar polymer / sulfonated polyarylether polymer composite according to claim 1, characterized in that: The sulfonated polyarylether polymer has a structure shown in Formula I: Wherein m is 1 to 20, n is 1 to 10; Ar1 represents One or more of; Ar2 represents One or more of; Ar3 represents One or more of .

5. The polar polymer / sulfonated polyarylether polymer composite according to claim 1, characterized in that: The sulfonated polyarylether polymer is One or more of .

6. The polar polymer / sulfonated polyarylether polymer composite according to claim 1, characterized in that: In the polar polymer / sulfonated polyarylether polymer composite, the mass content of the polar polymer is 1% to 90%.

7. The polar polymer / sulfonated polyarylether polymer composite according to claim 1, characterized in that: In the polar polymer / sulfonated polyarylether polymer composite, the mass content of the polar polymer is 1.5-85%.

8. An ion exchange membrane, characterized in that: The ion exchange membrane comprises the polar polymer / sulfonated polyarylether polymer composite as claimed in any one of claims 1 to 7.

9. A method for preparing an ion exchange membrane according to claim 8, characterized in that: The preparation method comprises: dissolving and dispersing the polar polymer / sulfonated polyarylether polymer complex in an organic medium to obtain a complex dispersion; The composite dispersion is made into a wet film and then dried to obtain the ion exchange membrane.

10. The preparation method according to claim 9, characterized in that: The organic medium is selected from at least one of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone.

11. The preparation method according to claim 9, characterized in that: The drying temperature is 70 to 90° C., and the drying time is 24 to 36 hours.

Citation Information

Patent Citations

  • Organic-inorganic ternary hybrid sulfonated polyaryletherketone proton exchange membrane and preparation method thereof

    CN102911494A

  • Organic-inorganic hybridized sulfonated polyaryletherketone proton exchange membrane and preparation method thereof

    CN102949943A

  • Polyamide / sulfonated polyether ether ketone composite proton exchanging membrane

    CN106887628A

  • Preparation method of cross-linking sulfonated polyarylether proton exchange membrane

    CN108192119A

  • Phosphorylated polyvinyl alcohol / perfluorosulfonic acid resin compound and ion exchange membrane

    CN113429715A