Semiconductor component, plasma processing device and method for forming composite coating
By forming a composite coating on the surface of semiconductor components, the corrosion-resistant coating structure and materials that are alternately arranged, the corrosion and particle pollution problems caused by plasma etching are solved, and the resistance and bonding of components are improved.
Patent Information
- Application Number
- CN202011479293.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-15
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-12-15
AI Technical Summary
In plasma etching process, semiconductor components are susceptible to corrosion and have particle contamination problems, which are difficult to effectively solve in the prior art.
The composite coating is formed on the surface of the semiconductor component, including a first corrosion-resistant coating and a second corrosion-resistant coating alternately arranged, the grain size of the first corrosion-resistant coating is greater than the second corrosion-resistant coating, and the second corrosion-resistant coating is resistant to the second corrosion-resistant coating. The corrosion coating is used to inhibit the grain growth of the first corrosion-resistant coating. The material may be a crystalline composite compound of rare earth elements and oxygen, fluorine, alumina or silicon oxide, etc., and is formed by a physical vapor deposition process or the like.
It improves the resistance of components to plasma corrosion, reduces particle pollution, enhances the bonding force with the component body, and meets process requirements.
Smart Images

Figure CN114639584B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductors, and in particular to a semiconductor component, a plasma processing device and a method for forming a composite coating on the surface of a component body. Background Art
[0002] In the manufacturing process of semiconductor devices, plasma etching is a key process for processing wafers into designed patterns.
[0003] In a typical plasma etching process, process gases (such as CF4, O2, etc.) form plasma under the action of radio frequency (RF). After passing through the electric field (capacitive coupling or inductive coupling) between the upper electrode and the lower electrode, these plasmas physically bombard and chemically react with the wafer surface, thereby etching a wafer with a specific structure.
[0004] However, during the plasma etching process, physical bombardment and chemical reactions will also act on all semiconductor components in contact with the plasma inside the etching chamber, causing corrosion. Therefore, the industry urgently needs to prepare an excellent corrosion-resistant coating on the surface of the component body to resist plasma corrosion and reduce particle contamination problems. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a semiconductor component, a plasma processing device and a composite coating formed on the surface of the component body to improve the ability of plasma corrosion resistance and reduce the problem of particle contamination.
[0006] In order to solve the above technical problems, the present invention provides a semiconductor component, including: a component body; a composite coating, located on the surface of the component body, including a first corrosion-resistant coating and a second corrosion-resistant coating alternately arranged, the grain size of the first corrosion-resistant coating is larger than the grain size of the second corrosion-resistant coating, the outermost layer of the composite coating and the layer in contact with the component body are both the first corrosion-resistant coating, and the second corrosion-resistant coating is used to inhibit the grain growth size of the first corrosion-resistant coating.
[0007] Optionally, the material of the first corrosion-resistant coating is the same as or different from that of the second corrosion-resistant coating.
[0008] Optionally, the first corrosion-resistant coating and the second corrosion-resistant coating are crystalline composite compounds formed by rare earth elements, oxygen and fluorine, and the crystalline composite compounds formed by rare earth elements, oxygen and fluorine include: YOF, Y5O4F7, Y6O5F8, Y7O6F9, Y 17 O 14 F 23, at least one of LaOF, CeOF, CeO6F2, PrOF, NdOF, SmOF, EuOF, Eu3O2F5, Eu5O4F7, GdOF, Gd5O4F7, TbOF, DyOF, HoOF, ErOF, Er3O2F5, Er5O4F7, TmOF, YbOF, Yb5O4F7, Yb6O5F8, LuOF, Lu3O2F5, Lu5O4F7 or Lu7O6F9.
[0009] Optionally, the first corrosion-resistant coating and the second corrosion-resistant coating are crystalline composite compounds formed by rare earth elements and aluminum oxide, and the crystalline composite compounds formed by rare earth elements and aluminum oxide include: Y4Al2O9, YAlO3, Y3Al5O 12 ,LaAlO3,CeAlO3,Ce6AlO3,Pr4Al2O9,PrAlO3,PrAl 11 O 18 ,Nd4Al2O9,NdAlO3,NdAl 11 O 18 ,Sm4Al2O9,SmAlO3,Eu4Al2O9,EuAlO3,Eu3Al5O 12 ,Gd4Al2O9,GdAlO3,Gd3Al5O 12 ,Tb4Al2O9,TbAlO3,Tb3Al5O 12 ,Dy4Al2O9,DyAlO3,Dy3Al5O 12 ,Ho4Al2O9,HoAlO3,Ho3Al5O 12 ,Er4Al2O9,ErAlO3,Er3Al5O 12 ,Tm4Al2O9,TmAlO3,Tm3Al5O 12 ,Yb4Al2O9,Yb6Al 10 O 24 ,Lu4Al2O9,LuAlO3 or Lu3Al5O 12 At least one of .
[0010] Optionally, the first corrosion-resistant coating and the second corrosion-resistant coating are crystalline composite compounds formed by rare earth elements and silicon oxide, and the crystalline composite compounds formed by rare earth elements and silicon oxide include: Y2SiO5, Y2Si2O7, La2SiO5, La2Si2O7, Ce2SiO5, Pr2SiO5, Pr2Si2O7, Nd2SiO5, Nd4Si3O 12 ,Nd2Si2O7,Sm2SiO5,Sm4Si3O 12,Sm2Si2O7,Eu2SiO5,EuSiO3,Eu2Si2O7,Gd2SiO5,Gd4Si3O 12 ,Gd2Si2O7,Tb2SiO5,Tb2Si2O7,Dy2SiO5,Dy4Si3O 12 ,Dy2Si2O7,Ho2SiO5,Er2Si2O7,Er2SiO5,Er4Si3O 12 ,Er2Si2O7,Tm2SiO5,Tm2Si2O7,Yb2SiO5,Yb4Si3O 12 ,Yb2Si2O7,Lu2SiO5,Lu4Si3O 12 Or at least one of Lu2Si2O7.
[0011] Optionally, the first corrosion-resistant coating and the second corrosion-resistant coating are crystalline oxides of rare earth metals, and the crystalline oxides of rare earth metals include LaO, La2O3, CeO, Ce2O3, CeO2, PrO, Pr2O3, Pr6O 11 , at least one of PrO2, NdO, Nd2O3, SmO, Sm2O3, EuO, Eu2O3, Gd2O3, Tb2O3, Tb4O7, TbO2, Dy2O3, Ho2O3, Er2O3, Tm2O3, YbO, Yb2O3 or Lu2O3.
[0012] Optionally, the first corrosion-resistant coating and the second corrosion-resistant coating are crystalline fluorides of rare earth metals, and the crystalline fluorides of rare earth metals include at least one of YF3, LaF3, CeF3, CeF4, PrCl3, PrCl4, NdF3, SmF2, SmF3, EuF2, EuF3, GdF3, TbF3, TbF4, DyF3, HoF3, ErF3, TmF2, TmF3, YbF3 or LuF3.
[0013] Optionally, the grains of the first corrosion-resistant coating are columnar grains; and the grains of the second corrosion-resistant coating are finely divided grains.
[0014] Optionally, the grain size of the first corrosion-resistant coating is greater than 100 nanometers in the width direction; and the grain size of the second corrosion-resistant coating is less than 100 nanometers in the width direction.
[0015] Optionally, the thickness of the first corrosion-resistant coating is 10 nanometers to 5000 nanometers; the thickness of the second corrosion-resistant coating is 1 nanometer to 100 nanometers.
[0016] Optionally, the first corrosion-resistant coating and the second corrosion-resistant coating are crystalline structures or amorphous structures.
[0017] Correspondingly, the present invention also provides a plasma processing device, comprising: a reaction chamber, which contains a plasma environment; the above-mentioned semiconductor component is located in the reaction chamber and exposed to the plasma environment.
[0018] Optionally, the plasma environment contains at least one of fluorine, chlorine, oxygen or hydrogen plasma.
[0019] Optionally, the plasma processing device is a plasma etching device or a plasma cleaning device.
[0020] Optionally, when the plasma processing device is an inductively coupled plasma processing device, the components include: at least one of a ceramic plate, an inner sleeve, a gas nozzle, a gas distribution plate, a gas pipe flange, an electrostatic suction cup assembly, a covering ring, a focusing ring, an insulating ring or a plasma confinement device.
[0021] Optionally, when the plasma processing device is a capacitively coupled plasma processing device, the components include: a shower head, an upper grounding ring, a moving ring, a gas distribution plate, a gas buffer plate, an electrostatic suction cup assembly, a lower grounding ring, a covering ring, a focusing ring, an insulating ring or at least one of a plasma confinement device.
[0022] Correspondingly, the present invention also provides a method for forming a composite coating on the surface of a component body, comprising: providing a component body; and forming the composite coating on the surface of the component body.
[0023] Optionally, the formation process of the first corrosion-resistant coating and the second corrosion-resistant coating includes: at least one of a physical vapor deposition process, a chemical vapor deposition process or an atomic layer deposition process.
[0024] Optionally, the melting point of the composite coating is T m When the first corrosion-resistant coating and the second corrosion-resistant coating are formed by a physical vapor deposition process, the temperature range for forming the first corrosion-resistant coating is: 1 / 3T m ~1 / 2T m , the temperature range for forming the second corrosion-resistant coating is less than 1 / 3T m .
[0025] Optionally, when the material of the composite coating is yttrium oxide, the temperature range for forming the first corrosion-resistant coating is 800 degrees Celsius to 1200 degrees Celsius, and the temperature range for forming the second corrosion-resistant coating is less than 800 degrees Celsius.
[0026] Optionally, a rate for forming the first corrosion-resistant coating is a first rate, a rate for forming the second corrosion-resistant coating is a second rate, and the second rate is less than 1 / 2 of the first rate.
[0027] Optionally, when the composite coating is yttrium oxide, the first rate ranges from 0.5 nm / s to 5 nm / s, and the second rate ranges from 0.01 nm / s to 0.3 nm / s.
[0028] Optionally, the process of forming the composite coating further includes: processing with an auxiliary enhancement source; the auxiliary enhancement source also includes: at least one of a plasma source, an ion beam source, a microwave source or a radio frequency source.
[0029] Optionally, under the action of the auxiliary enhancement source, the power for forming the first corrosion-resistant coating is a first power, and the power for forming the second corrosion-resistant coating is a second power, and the second power is less than 1 / 2 of the first power.
[0030] Compared with the prior art, the technical solution of the embodiment of the present invention has the following beneficial effects:
[0031] In the semiconductor component provided by the technical solution of the present invention, the surface of the component body has a composite coating, and the composite coating includes a first corrosion-resistant coating and a second corrosion-resistant coating, the grain size of the first corrosion-resistant coating is larger than the grain size of the second corrosion-resistant coating, and the second corrosion-resistant coating is used to inhibit the grain growth of the first corrosion-resistant coating and prevent the generation of large grains in the first corrosion-resistant coating. In this way, the semiconductor component is exposed to the plasma environment, and it is not easy to diffuse along the edge of the large grains so that the large particles fall off, so it is helpful to reduce particle contamination to better meet the process requirements. In addition, the composite coating in contact with the component body is the first corrosion-resistant coating, the first corrosion-resistant coating has a strong bonding force with the component body, and the outermost layer of the composite coating is the first corrosion-resistant coating, the grain size of the first corrosion-resistant coating is larger than the grain size of the second corrosion-resistant coating, and has a strong corrosion resistance, which can improve the component body from being corroded by plasma. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a structural schematic diagram of a plasma processing device of the present invention;
[0033] Figure 2 It is a structural schematic diagram of another plasma processing device of the present invention;
[0034] Figure 3 It is a structural schematic diagram of a semiconductor component of the present invention;
[0035] Figure 4 It is a process flow chart of forming a composite coating on the surface of a component body of the present invention;
[0036] Figure 5 It is a schematic diagram of the device used for physical vapor deposition process of the present invention. DETAILED DESCRIPTION
[0037] As described in the background technology, it is urgent to prepare a corrosion-resistant coating with excellent performance on the surface of the component body to resist plasma corrosion and reduce particle pollution problems. To this end, the present invention is committed to providing a semiconductor component, a plasma processing device and a method for forming a composite coating on the surface of the component body. The semiconductor component has strong corrosion resistance in a plasma environment and can reduce particle pollution problems. The following is a detailed description:
[0038] Figure 1 The figure is a schematic structural diagram of a plasma processing device according to the present invention.
[0039] Please refer to Figure 1 The plasma reaction device includes: a reaction chamber 100, the reaction chamber 100 is a plasma environment, the semiconductor components and the inner wall of the reaction chamber 100 are exposed to the plasma environment, and the plasma includes at least one of F-containing plasma, Cl-containing plasma, H-containing plasma or O-containing plasma.
[0040] The plasma reaction device further includes: a base 101, an electrostatic chuck 103 is arranged above the base 101, an electrode (not shown in the figure) is arranged inside the electrostatic chuck 103, and the electrode is connected to a direct current power supply DC, and is used to generate electrostatic adsorption to fix the substrate W to be processed, and the plasma is used to process the substrate W to be processed. Since plasma is highly corrosive, in order to prevent the surface of the semiconductor parts exposed to the plasma environment from being corroded by the plasma, a composite coating needs to be coated on the surface of the parts body.
[0041] In this embodiment, the plasma reaction device is a capacitively coupled plasma reaction device, and accordingly, the semiconductor components exposed to the plasma environment include: a shower head 102, an upper grounding ring 104, a moving ring, a gas distribution plate 105, a gas buffer plate, an electrostatic suction cup assembly 103, a lower grounding ring 106, a cover ring 107, a focusing ring 108, an insulating ring, and at least one of a plasma confinement device 109.
[0042] Figure 2 It is a schematic structural diagram of another plasma processing device of the present invention.
[0043] In this embodiment, the plasma reaction device is an inductively coupled plasma reaction device, and accordingly, the semiconductor components exposed to the plasma environment include: a ceramic plate, an inner sleeve 200, a gas nozzle 201, a gas distribution plate, a gas pipe flange, an electrostatic suction cup assembly 202, a cover ring 203, a focusing ring 204, an insulating ring and at least one of a plasma confinement device 205.
[0044] During the plasma etching process, physical bombardment and chemical reactions will also act on all semiconductor components in contact with the plasma inside the reaction chamber, causing corrosion to the semiconductor components. Long-term exposure to the plasma corrosion environment will damage the surface structure of the semiconductor components, causing the precipitation of bulk components, which will separate from the surface to form tiny particles and contaminate the wafer. Advanced semiconductor manufacturing has strict requirements for tiny particle contamination, such as the number of particles larger than 45nm is 0. Therefore, it is necessary to apply a composite coating on the surface of the component body in the plasma reaction device to resist plasma corrosion.
[0045] The following is a detailed description of semiconductor components:
[0046] Figure 3 The figure is a schematic structural diagram of a semiconductor component of the present invention.
[0047] Please refer to Figure 3 The semiconductor component includes: a component body 300; a composite coating 301, located on the surface of the component body 300, including a first corrosion-resistant coating 301a and a second corrosion-resistant coating 301b alternately arranged, the grain size of the first corrosion-resistant coating 301a is larger than the grain size of the second corrosion-resistant coating 301b, the outermost layer of the composite coating 301 and the layer in contact with the component body 300 are both the first corrosion-resistant coating 301a, and the second corrosion-resistant coating 301b is used to inhibit the grain growth size of the first corrosion-resistant coating 301a.
[0048] The material of the component body 300 includes at least one of aluminum alloy, silicon carbide, silicon, quartz or ceramic.
[0049] The surface of the component body 300 has a composite coating 301. When the semiconductor component is exposed to a plasma environment, since the composite coating 301 has strong corrosion resistance, the composite coating 301 can protect the component body 300 and prevent the component body 300 from being corroded by the plasma, which is beneficial to improving the service life of the semiconductor component.
[0050] The composite coating 301 includes a first corrosion-resistant coating 301a and a second corrosion-resistant coating 301b. The materials of the first corrosion-resistant coating 301a and the second corrosion-resistant coating 301b are the same or different. When the materials of the first corrosion-resistant coating 301a and the second corrosion-resistant coating 301b are different, after the first corrosion-resistant coating 301a is formed, the material needs to be replaced to form a second corrosion-resistant coating 301b having a material different from that of the first corrosion-resistant coating 301a.
[0051] The first corrosion-resistant coating 301a and the second corrosion-resistant coating 301b are crystalline structures or amorphous structures.
[0052] In one embodiment, the first corrosion-resistant coating 301a and the second corrosion-resistant coating 301b are crystalline composite compounds formed by rare earth elements, oxygen and fluorine, and the crystalline composite compounds formed by rare earth elements, oxygen and fluorine include: YOF, Y5O4F7, Y6O5F8, Y7O6F9, Y 17 O 14 F 23 ,LaOF (lanthanum oxyfluoride), CeOF, CeO6F2, PrOF (praseodymium oxyfluoride), NdOF (neodymium oxyfluoride), SmOF (samarium oxyfluoride), EuOF (europium oxyfluoride), Eu3O2F5, Eu5O4F7, GdOF (gadolinium oxyfluoride), Gd5O4F7, TbOF (terbium oxyfluoride), DyOF (dysprosium oxyfluoride), HoOF (holmium oxyfluoride), ErOF (erbium oxyfluoride), Er3O2F5, Er5O4F7, TmOF (thulium oxyfluoride), YbOF (ytterbium oxyfluoride), Yb5O4F7, Yb6O5F8, LuOF (lutetium oxyfluoride), Lu3O2F5, Lu5O4F7 or Lu7O6F9.
[0053] In another embodiment, the first corrosion-resistant coating 301a and the second corrosion-resistant coating 301b are crystalline composite compounds formed by rare earth elements and aluminum oxide, and the crystalline composite compounds formed by rare earth elements and aluminum oxide include: Y4Al2O9, YAlO3, Y3Al5O 12 ,LaAlO3,CeAlO3(cerium aluminum oxide),Ce6AlO3,Pr4Al2O9(praseodymium aluminum oxide),PrAlO3,PrAl 11 O 18 ,Nd4Al2O9,NdAlO3(neodymium aluminum oxide),NdAl 11 O 18 ,Sm4Al2O9(Samarium Aluminum Oxide),SmAlO3,Eu4Al2O9(Europium Aluminum Oxide),EuAlO3,Eu3Al5O 12 ,Gd4Al2O9(gadolinium aluminum oxide),GdAlO3,Gd3Al5O 12 ,Tb4Al2O9(terbium aluminum oxide), TbAlO3, Tb3Al5O 12 ,Dy4Al2O9(dysprosium aluminum oxide), DyAlO3, Dy3Al5O 12 ,Ho4Al2O9(holmium aluminum oxide), HoAlO3, Ho3Al5O 12 ,Er4Al2O9(erbium aluminum oxide), ErAlO3, Er3Al5O 12,Tm4Al2O9(thulium aluminum oxide), TmAlO3, Tm3Al5O 12 ,Yb4Al2O9(ytterbium aluminum oxide), Yb6Al 10 O 24 ,Lu4Al2O9 (lutetium aluminum oxide), LuAlO3 or Lu3Al5O 12 At least one of .
[0054] In another embodiment, the first corrosion-resistant coating 301a and the second corrosion-resistant coating 301b are crystalline composite compounds formed by rare earth elements and silicon oxide, and the crystalline composite compounds formed by rare earth elements and silicon oxide include: Y2SiO5, Y2Si2O7, La2SiO5 (lanthanum silicon oxide), La2Si2O7, Ce2SiO5 (cerium silicon oxide), Pr2SiO5 (praseodymium silicon oxide), Pr2Si2O7, Nd2SiO5 (neodymium silicon oxide), Nd4Si3O 12 ,Nd2Si2O7,Sm2SiO5(Samarium Silicon Oxide),Sm4Si3O 12 ,Sm2Si2O7,Eu2SiO5(europium silicon oxide),EuSiO3,Eu2Si2O7,Gd2SiO5(gadolinium silicon oxide),Gd4Si3O 12 ,Gd2Si2O7,Tb2SiO5(terbium silicon oxide),Tb2Si2O7,Dy2SiO5(dysprosium silicon oxide),Dy4Si3O 12 ,Dy2Si2O7,Ho2SiO5(holmium silicon oxide),Er2Si2O7(erbium silicon oxide),Er2SiO5,Er4Si3O 12 ,Er2Si2O7,Tm2SiO5(Thulium SiO),Tm2Si2O7,Yb2SiO5,Yb4Si3O 12 ,Yb2Si2O7,Lu2SiO5,Lu4Si3O 12 Or at least one of Lu2Si2O7.
[0055] In another embodiment, the first corrosion-resistant coating 301a and the second corrosion-resistant coating 301b are crystalline oxides of rare earth metals, and the crystalline oxides of rare earth metals include LaO, La2O3, CeO, Ce2O3, CeO2, PrO, Pr2O3, Pr6O 11 , at least one of PrO2, NdO, Nd2O3, SmO, Sm2O3, EuO, Eu2O3, Gd2O3, Tb2O3, Tb4O7, TbO2, Dy2O3, Ho2O3, Er2O3, Tm2O3, YbO, Yb2O3 or Lu2O3.
[0056] In other embodiments, the first corrosion-resistant coating and the second corrosion-resistant coating are crystalline fluorides of rare earth metals, and the crystalline fluorides of rare earth metals include at least one of YF3, LaF3, CeF3, CeF4, PrCl3, PrCl4, NdF3, SmF2, SmF3, EuF2, EuF3, GdF3, TbF3, TbF4, DyF3, HoF3, ErF3, TmF2, TmF3, YbF3 or LuF3.
[0057] In the process of forming the first corrosion-resistant coating 301a, due to the cumulative effect of the thermal effect, when the first corrosion-resistant coating 301a is deposited to a certain thickness, the molecular flow breaks through the nucleation energy barrier to form a large number of nuclei, and rapidly agglomerates and grows, which will randomly generate abnormally large grains. In order to prevent the generation of abnormally large grains, in this embodiment, the thickness range of the first corrosion-resistant coating 301a is: 10 nanometers to 5000 nanometers. Within the thickness range of the first corrosion-resistant coating 301a, the first corrosion-resistant coating 301a is not easy to generate large grains, and the grains of the first corrosion-resistant coating 301a are columnar grains. The grain size of the second corrosion-resistant coating 301b is larger than the grain size of the first corrosion-resistant coating 301a, so the second corrosion-resistant coating 301b can be used to suppress the first corrosion-resistant coating 301a from generating large grains. Specifically, the grains of the second corrosion-resistant coating 301b are finely divided grains, and the thickness of the second corrosion-resistant coating 301b is 1 nanometer to 100 nanometers.
[0058] The significance of selecting the thickness of the second corrosion-resistant coating 301b is that if the thickness of the second corrosion-resistant coating 301b is less than 1 nanometer, it will be difficult for the second corrosion-resistant coating 301b to suppress the generation of large grains in the first corrosion-resistant coating 301a. If large grains are generated in the first corrosion-resistant coating 301a, the large grains will be corroded first, and the plasma will penetrate and corrode along the grain boundaries between the large grains and the surrounding grains, destroying the bonding between the large grains and the surrounding grains. When the critical bonding strength is exceeded, large particles will fall off to form tiny particle contaminants, which are scattered in the etching chamber and cannot better meet the process requirements. If the thickness of the second corrosion-resistant coating 301b is greater than 100 nanometers, it will cause a sudden change in the corrosion resistance of the first corrosion-resistant coating 301a and the second corrosion-resistant coating 301b, resulting in unstable performance.
[0059] In this embodiment, the grain size of the first corrosion-resistant coating 301a is larger than the grain size of the second corrosion-resistant coating 301b. Specifically, the grain width size of the first corrosion-resistant coating 301a is larger than 100 nanometers; the grain width size of the second corrosion-resistant coating 301b is smaller than 100 nanometers. The significance of such a setting is that the second corrosion-resistant coating 301b can not only play a role in limiting the abnormal growth of large particles in the first corrosion-resistant coating 301a, but also maintain a smooth transition of the corrosion-resistant effects of the first corrosion-resistant coating 301a and the second corrosion-resistant coating 301b, and maintain the stability of the environment in the reaction chamber.
[0060] In this embodiment, the first corrosion-resistant coating 301a is distributed on the surface of the component body 300 and the surface of the composite coating 301. The significance of this arrangement is that the grains of the first corrosion-resistant coating 301a are columnar crystals with larger grains. Compared with fine grains, the bonding strength with the component body 300 is higher. Therefore, as the first layer combined with the component body 300, the bonding strength of the composite coating 301 as a whole with the component body 300 is stronger. At the same time, the grains of the first corrosion-resistant coating 301a are columnar crystals with larger grains. Compared with fine grains, it has fewer grain boundaries and better corrosion resistance. Therefore, as the outermost coating of the composite coating 301, the corrosion resistance effect is fully exerted.
[0061] Figure 4 The present invention is a process flow chart for forming a composite coating on the surface of a component body.
[0062] Please refer to Figure 4 Step S1: providing a component body; Step S2: forming the above-mentioned composite coating on the surface of the component body, the composite coating comprising a first corrosion-resistant coating and a second corrosion-resistant coating alternately arranged, the grain size of the first corrosion-resistant coating is larger than the grain size of the second corrosion-resistant coating, the outermost layer of the composite coating and the layer in contact with the component body are both the first corrosion-resistant coating, and the second corrosion-resistant coating is used to inhibit the grain growth of the first corrosion-resistant coating.
[0063] The following is a detailed description of the device schematic diagram used for the physical vapor deposition process:
[0064] Figure 5 It is a schematic diagram of the device used for physical vapor deposition process of the present invention.
[0065] Please refer to Figure 5, The device for physical vapor deposition process includes: a vacuum chamber 400; a target 401 located at the bottom inside the vacuum chamber 400; a component body 300 located inside the vacuum chamber 400 and disposed opposite to the target 401; an excitation device 402 for exciting atoms in the target 401 to form a composite coating 301 on the surface of the component body 300.
[0066] In one embodiment, the method for forming the composite coating 301 on the surface of the component body 300 includes: the melting point of the composite coating 301 is T m , the temperature range T1 of the component body 300 is 1 / 3T m ~1 / 2T m , to form a first corrosion-resistant coating 301a on the surface of the component body 300; after forming the first corrosion-resistant coating 301a, the temperature range T2 of the component body 300 is less than 1 / 3T m , to form a second corrosion-resistant coating 301b on the surface of the first corrosion-resistant coating 301a, and the composite coating 301 is formed through multiple cycles. The composite coating 301 includes a number of alternately arranged first corrosion-resistant coatings 301a and second corrosion-resistant coatings 301b.
[0067] The principle of forming the composite coating 301 by changing the temperature of the component body 300 includes: when the heating temperature of the component body 300 is lower than 1 / 3 of the melting point T of the composite coating 301 m , the growth of the composite coating 301 is limited by the diffusion of molecular flow on the surface of the component body 300, showing a fragmented grain growth mode; when the temperature of the component body 300 is higher than 1 / 3 of the melting point T of the composite coating 301 m , due to the diffusion of molecular flow on the deposition surface, a columnar grain growth mode will be shown.
[0068] The device for physical vapor deposition process further includes: an auxiliary enhancement source (not shown in the figure), and the auxiliary enhancement source is used to increase the diffusion of molecular flow on the surface of the component body, and plays a role in improving the deposition morphology characteristics of the composite coating 301 while reducing the temperature of the component body 300. Among them, the auxiliary enhancement source includes at least one of a plasma source, an ion beam source, a microwave source or a radio frequency source.
[0069] Taking Y2O3 as an example, under the condition of no auxiliary enhancement source, 800 degrees Celsius < T1 < 1200 degrees Celsius, T2 < 800 degrees Celsius; under the condition of the auxiliary enhancement source, the heating temperature of the component body can be greatly reduced, T1 < 300 degrees Celsius, T2 < 200 degrees Celsius.
[0070] In another embodiment, the method for forming a composite coating 301 on the surface of the component body 300 includes: using the auxiliary enhancement source, when the power of the auxiliary enhancement source is the first power P1, forming a first corrosion-resistant coating 301a on the surface of the component body 300; after forming the first corrosion-resistant coating 301a, using the auxiliary enhancement source, when the power of the auxiliary enhancement source is the second power P2, and the second power P2 is less than 1 / 2 of the first power P1, forming a second corrosion-resistant coating 301b on the surface of the first corrosion-resistant coating 301a, after multiple cycles, the auxiliary enhancement source is switched between the first power P1 and the second power P2 to form the composite coating 301, the composite coating 301 includes multiple layers of alternately stacked first corrosion-resistant coatings 301a and second corrosion-resistant coatings 301b. Taking Y2O3 as an example, under the condition of a plasma-assisted enhancement source, when the first power P1 is 6kw, the second power P2 can be 1kw or lower.
[0071] In another embodiment, the method for forming the composite coating 301 on the surface of the component body 300 includes: adjusting the excitation energy of the target material 401 so that the deposition rate is a first rate V1, and forming a first corrosion-resistant coating 301a on the surface of the component body 300; after forming the first corrosion-resistant coating 301a, adjusting the excitation energy of the target material 401 so that the deposition rate is a second rate V2, and forming a second corrosion-resistant coating 301b on the surface of the first corrosion-resistant coating 301a; after multiple cycles, the deposition rate is switched between the first rate V1 and the second rate V2 to form the composite coating 301, and the composite coating 301 includes multiple layers of alternately stacked first corrosion-resistant coatings 301a and second corrosion-resistant coatings 301b.
[0072] The principle of adjusting the excitation energy of the target material and the deposition rate to form the first corrosion-resistant coating 301a and the second corrosion-resistant coating 301b includes: when the molecular flow excited by the target material 401 is in an oversaturated deposition environment, there are sufficient molecules to nucleate and grow in the growth process of the grains, thereby forming the first corrosion-resistant coating 301a with a columnar crystal structure; when the molecular flow excited by the target material 401 is in an undersaturated deposition environment, the growth process of the grains is limited by the number of molecular nuclei and can only proceed in a fine grain growth manner, that is, a finely crystalline second corrosion-resistant coating 301b is formed.
[0073] Taking Y2O3 as an example, when the first rate V1 of forming the first corrosion-resistant coating 301a is between 0.5 nm / s and 5 nm / s, the second rate V2 of forming the second corrosion-resistant coating 301b is between 0.01 nm / s and 0.3 nm / s.
[0074] The principle that the second corrosion-resistant coating 301b can play the role of limiting the grain growth of the first corrosion-resistant coating 101 includes: in the physical vapor deposition process, the excited molecular flow is transported to the surface of the component body 300, nucleates and grows to form the first corrosion-resistant coating 301a. In these processes, the molecular flow of the first corrosion-resistant coating 101 grows on the component body 300 in a columnar manner, and the continuous accumulation of its crystallization thermal effect causes the barrier required for the nucleation and growth of the molecular flow that arrives subsequently to be continuously reduced. When it is reduced to below the critical value, the rapid generation of grains will occur to form nuclei and grow, forming abnormally large grains. Before reaching the critical value, by regulating the environmental conditions required for the molecular flow nucleation and growth mode, such as the temperature of the component body, the energy of the auxiliary enhancement source, and the deposition rate, the growth mode of the molecular flow on the component body 300 is changed from the columnar grain mode to the fine grain mode, thereby reducing the generation of random large particles.
[0075] The formation process of the first corrosion-resistant coating 301a and the second corrosion-resistant coating 301b may be at least one of a chemical vapor deposition process or an atomic layer deposition process in addition to the above-mentioned physical vapor deposition process.
[0076] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A semiconductor component, characterized in that: include: Component body; The composite coating is located on the surface of the component body, including a first corrosion-resistant coating and a second corrosion-resistant coating that are alternately arranged. The grain size of the first corrosion-resistant coating is larger than the grain size of the second corrosion-resistant coating. The outermost layer of the composite coating and the layer in contact with the component body are both the first corrosion-resistant coating. The second corrosion-resistant coating is used to inhibit the grain growth size of the first corrosion-resistant coating. The first corrosion-resistant coating and the second corrosion-resistant coating are formed by a physical vapor deposition process. The grains of the first corrosion-resistant coating are columnar grains; the grains of the second corrosion-resistant coating are finely divided grains. The thickness of the first corrosion-resistant coating is 10 nanometers to 5000 nanometers; the thickness of the second corrosion-resistant coating is 1 nanometer to 100 nanometers.
2. The semiconductor component according to claim 1, wherein: The first corrosion-resistant coating and the second corrosion-resistant coating may be made of the same or different materials.
3. The semiconductor component according to claim 2, wherein: The first corrosion-resistant coating and the second corrosion-resistant coating are crystalline composite compounds formed by rare earth elements, oxygen and fluorine, and the crystalline composite compounds formed by rare earth elements, oxygen and fluorine include: YOF, Y5O4F7, Y6O5F8, Y7O6F9, Y 17 O 14 F 23 , at least one of LaOF, CeOF, CeO6F2, PrOF, NdOF, SmOF, EuOF, Eu3O2F5, Eu5O4F7, GdOF, Gd5O4F7, TbOF, DyOF, HoOF, ErOF, Er3O2F5, Er5O4F7, TmOF, YbOF, Yb5O4F7, Yb6O5F8, LuOF, Lu3O2F5, Lu5O4F7 or Lu7O6F9.
4. The semiconductor component according to claim 2, wherein: The first corrosion-resistant coating and the second corrosion-resistant coating are crystalline composite compounds formed by rare earth elements and aluminum oxide, and the crystalline composite compounds formed by rare earth elements and aluminum oxide include: Y4Al2O9, YAlO3, Y3Al5O 12 ,LaAlO3,CeAlO3,Ce6AlO3,Pr4Al2O9,PrAlO3,PrAl 11 O 18 ,Nd4Al2O9,NdAlO3,NdAl 11 O 18 ,Sm4Al2O9,SmAlO3,Eu4Al2O9,EuAlO3,Eu3Al5O 12 ,Gd4Al2O9,GdAlO3,Gd3Al5O 12 ,Tb4Al2O9,TbAlO3,Tb3Al5O 12 ,Dy4Al2O9,DyAlO3,Dy3Al5O 12 ,Ho4Al2O9,HoAlO3,Ho3Al5O 12 ,Er4Al2O9,ErAlO3,Er3Al5O 12 ,Tm4Al2O9,TmAlO3,Tm3Al5O 12 ,Yb4Al2O9,Yb6Al 10 O 24 ,Lu4Al2O9,LuAlO3 or Lu3Al5O 12 At least one of .
5. The semiconductor component according to claim 2, wherein: The first corrosion-resistant coating and the second corrosion-resistant coating are crystalline composite compounds formed by rare earth elements and silicon oxide, and the crystalline composite compounds formed by rare earth elements and silicon oxide include: Y2SiO5, Y2Si2O7, La2SiO5, La2Si2O7, Ce2SiO5, Pr2SiO5, Pr2Si2O7, Nd2SiO5, Nd4Si3O 12 ,Nd2Si2O7,Sm2SiO5,Sm4Si3O 12 ,Sm2Si2O7,Eu2SiO5,EuSiO3,Eu2Si2O7,Gd2SiO5,Gd4Si3O 12 ,Gd2Si2O7,Tb2SiO5,Tb2Si2O7,Dy2SiO5,Dy4Si3O 12 ,Dy2Si2O7,Ho2SiO5,Er2Si2O7,Er2SiO5,Er4Si3O 12 ,Er2Si2O7,Tm2SiO5,Tm2Si2O7,Yb2SiO5,Yb4Si3O 12 ,Yb2Si2O7,Lu2SiO5,Lu4Si3O 12 Or at least one of Lu2Si2O7.
6. The semiconductor component according to claim 2, wherein: The first corrosion-resistant coating and the second corrosion-resistant coating are crystalline oxides of rare earth metals, and the crystalline oxides of rare earth metals include LaO, La2O3, CeO, Ce2O3, CeO2, PrO, Pr2O3, Pr6O 11 , at least one of PrO2, NdO, Nd2O3, SmO, Sm2O3, EuO, Eu2O3, Gd2O3, Tb2O3, Tb4O7, TbO2, Dy2O3, Ho2O3, Er2O3, Tm2O3, YbO, Yb2O3 or Lu2O3.
7. The semiconductor component according to claim 2, wherein: The first corrosion-resistant coating and the second corrosion-resistant coating are crystalline fluorides of rare earth metals, and the crystalline fluorides of rare earth metals include at least one of YF3, LaF3, CeF3, CeF4, PrCl3, PrCl4, NdF3, SmF2, SmF3, EuF2, EuF3, GdF3, TbF3, TbF4, DyF3, HoF3, ErF3, TmF2, TmF3, YbF3 or LuF3.
8. The semiconductor component according to claim 1, wherein: The grain size of the first corrosion-resistant coating in the width direction is greater than 100 nanometers; the grain size of the second corrosion-resistant coating in the width direction is less than 100 nanometers.
9. The semiconductor component according to claim 1, wherein: The first corrosion-resistant coating and the second corrosion-resistant coating are crystalline structures or amorphous structures.
10. A plasma processing device, characterized in that: include: A reaction chamber, wherein the interior of the chamber is a plasma environment; The semiconductor component according to any one of claims 1 to 9, located in the reaction chamber and exposed to the plasma environment.
11. The plasma processing apparatus according to claim 10, wherein: The plasma environment contains at least one of fluorine, chlorine, oxygen or hydrogen plasma.
12. The plasma processing apparatus according to claim 10, wherein: The plasma processing device is a plasma etching device or a plasma cleaning device.
13. The plasma processing apparatus according to claim 12, wherein: When the plasma processing device is an inductively coupled plasma processing device, the components include: at least one of a ceramic plate, an inner sleeve, a gas nozzle, a gas distribution plate, a gas pipe flange, an electrostatic chuck assembly, a cover ring, a focusing ring, an insulating ring or a plasma confinement device.
14. The plasma processing apparatus according to claim 12, wherein: When the plasma processing device is a capacitively coupled plasma processing device, the components include: at least one of a shower head, an upper grounding ring, a moving ring, a gas distribution plate, a gas buffer plate, an electrostatic chuck assembly, a lower grounding ring, a cover ring, a focusing ring, an insulating ring or a plasma confinement device.
15. A method for forming a composite coating on the surface of a component body, characterized in that: include: Provide the parts body; A composite coating as claimed in any one of claims 1 to 9 is formed on the surface of the component body, the composite coating includes a first corrosion-resistant coating and a second corrosion-resistant coating alternately arranged, the grain size of the first corrosion-resistant coating is larger than the grain size of the second corrosion-resistant coating, the outermost layer of the composite coating and the layer in contact with the component body are both the first corrosion-resistant coating, the second corrosion-resistant coating is used to inhibit the grain growth size of the first corrosion-resistant coating, the first corrosion-resistant coating and the second corrosion-resistant coating are formed by a physical vapor deposition process, the grains of the first corrosion-resistant coating are columnar grains; the grains of the second corrosion-resistant coating are finely divided grains, the thickness of the first corrosion-resistant coating is 10 nanometers to 5000 nanometers; the thickness of the second corrosion-resistant coating is 1 nanometer to 100 nanometers.
16. The method for forming a composite coating on the surface of a component body according to claim 15, characterized in that: The melting point of the composite coating is T m ; The temperature range for forming the first corrosion-resistant coating is: 1 / 3T m ~1 / 2T m , the temperature range for forming the second corrosion-resistant coating is less than 1 / 3T m .
17. The method for forming a composite coating on the surface of a component body according to claim 16, characterized in that: When the material of the composite coating is yttrium oxide, the temperature range for forming the first corrosion-resistant coating is 800 degrees Celsius to 1200 degrees Celsius, and the temperature range for forming the second corrosion-resistant coating is less than 800 degrees Celsius.
18. The method for forming a composite coating on the surface of a component body according to claim 15, characterized in that: The rate of forming the first corrosion-resistant coating is a first rate, and the rate of forming the second corrosion-resistant coating is a second rate, and the second rate is less than 1 / 2 of the first rate.
19. The method for forming a composite coating on the surface of a component body according to claim 18, characterized in that: When the composite coating is yttrium oxide, the first rate ranges from 0.5 nm / s to 5 nm / s, and the second rate ranges from 0.01 nm / s to 0.3 nm / s.
20. The method for forming a composite coating on the surface of a component body according to claim 15, characterized in that: The process of forming the composite coating also includes: using an auxiliary enhancement source for processing; the auxiliary enhancement source includes: at least one of a plasma source, an ion beam source, a microwave source or a radio frequency source.
21. The method for forming a composite coating on the surface of a component body according to claim 20, characterized in that: Under the action of the auxiliary enhancement source, the power for forming the first corrosion-resistant coating is the first power, and the power for forming the second corrosion-resistant coating is the second power, and the second power is less than 1 / 2 of the first power.
Citation Information
Patent Citations
Erosion resistant yttrium comprising metal with oxidized coating for plasma chamber components
CN102732857A
Plasma erosion resistant thin film coating for high temperature application
CN111254436A
Semiconductor component and plasma processing apparatus
CN214175968U
Corrosion resistant member and method for manufacturing the same
US20050282034A1
Zone-controlled rare-earth oxide ALD and CVD coatings
US20190309413A1