A novel flame retardant epoxy potting resin and preparation method thereof

Through the combination of component A and component B of the new flame-retardant epoxy potting resin, combined with a specific stirring and degassing process, the problem of insufficient heat resistance and waterproof performance of epoxy resin in a condensate pump environment is solved, and the problem is achieved in Improved adhesion and sealing during hot and cold cycles extend product life.

CN114644812BActive Publication Date: 2024-10-01ZHENJIANG LEADER COMPOSITE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110276868.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-15
Publication Date
2024-10-01
Estimated Expiration
2041-03-15

AI Technical Summary

Technical Problem

Existing epoxy potting resins are difficult to meet the fireproof, waterproof and heat-resistant performance requirements in the special environment of condensate pumps, leading to problems such as cracking and peeling.

Method used

New flame-retardant epoxy potting resin using component A and component B. Component A includes epoxy resin, inorganic filler, diluent and flame retardant. It is combined with silane coupling agent through a specific stirring and degassing process. , wetting and dispersing agents, defoaming agents and leveling agents to optimize viscosity and fluidity. Component B is a curing agent and accelerator to ensure product adhesion and sealing during hot and cold cycles.

Benefits of technology

It improves the adhesion and sealing performance of the epoxy potting resin on the condensate pump, avoids the precipitation of inactive substances, enhances the heat resistance and waterproof performance, and extends the service life of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002977005410000111
    Figure BDA0002977005410000111
  • Figure BDA0002977005410000121
    Figure BDA0002977005410000121
Patent Text Reader

Abstract

This invention belongs to the field of epoxy resin technology, and more specifically relates to a novel flame-retardant epoxy potting resin and its preparation method. The novel flame-retardant epoxy potting resin comprises component A and component B; the weight ratio of component A to component B is 100:(20-50). The epoxy potting resin prepared by this invention can be prepared without the need for defoaming equipment, has suitable viscosity and good flowability, avoids the precipitation of inactive substances during use, and possesses durability. The epoxy potting resin prepared by this invention alters the heat resistance of the epoxy potting resin through the addition of fillers, and its use in this system avoids the impact of filler addition on the flexibility of the epoxy potting resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of epoxy resins, and more specifically relates to a novel flame retardant epoxy potting resin and a preparation method thereof. Background Art

[0002] At present, epoxy resin is widely used in various fields such as home appliances, automobiles, rail transportation, semiconductors, etc. due to its excellent electrical properties and thermal stability. Among them, the condensate pump has a specific use environment and has high requirements for the material in terms of waterproofing, dustproofing, and especially fireproofing. In order to ensure its normal use, it is often necessary to have good heat resistance and low temperature resistance, so as to avoid cracking and peeling when used in the condensate pump.

[0003] At present, there are many applications of epoxy potting resins, but there are few epoxy potting resins that are specifically used in condensate pumps and meet their special use environments. In order to improve its application in condensate pumps, a new type of epoxy potting resin has become an important task for researchers. Summary of the invention

[0004] In order to solve the above technical problems, the first aspect of the present invention provides a novel flame retardant epoxy potting resin, comprising component A and component B; the weight ratio of component A to component B is 100:(20-50).

[0005] The raw materials for preparing the component A include, by weight: 25-35 parts of epoxy resin, 20-35 parts of inorganic filler, 1-15 parts of diluent, and 1-5 parts of black paste;

[0006] The raw materials for preparing the B component include: a curing agent and an accelerator.

[0007] As a preferred technical solution, the raw materials for preparing the A component also include a silane coupling agent, a wetting dispersant, a defoaming agent, a leveling agent, and a flame retardant.

[0008] As a preferred technical solution, the raw materials for preparing component A also include 0.1-1 parts of silane coupling agent, 0.1-1 parts of wetting dispersant, 0.1-1 parts of defoaming agent, 0.1-1 parts of leveling agent, and 20-30 parts of flame retardant.

[0009] As a preferred technical solution, the weight ratio of the wetting dispersant, defoaming agent and leveling agent is (1-2): (1.5-2.5):1.

[0010] As a preferred technical solution, the inorganic filler is selected from one or more of aluminum hydroxide, silicon dioxide, calcium carbonate, mica powder, quartz powder, and talcum powder.

[0011] As a preferred technical solution, the diluent is selected from active diluents and / or inactive diluents.

[0012] As a preferred technical solution, the active diluent is selected from at least one of benzyl glycidyl ether, carbon dodeca- to tetradecyl glycidyl ether, alkylene glycidyl ether, trimethylolpropane triglycidyl ether, and castor oil polyglycidyl ether.

[0013] As a preferred technical solution, the raw materials for preparing the B component include, by weight: 95-99 parts of a curing agent and 1-5 parts of an accelerator.

[0014] As a preferred technical solution, the curing agent is selected from methyltetrahydrophthalic anhydride and / or methylhexahydrophthalic anhydride.

[0015] The second aspect of the present invention provides a method for preparing a novel flame retardant epoxy potting resin, comprising the following steps:

[0016] S1. Preparation of component A: first add epoxy resin, silane coupling agent, black paste, wetting dispersant, defoamer and leveling agent into a stirring device, stir for 5-10 minutes, control the temperature at 15-30°C, then add flame retardant and inorganic filler, stir at low speed for 10 minutes, then stir at high speed for 45-60 minutes, control the temperature between 25-45°C, finally add diluent and stir at high speed for 30-40 minutes, turn on vacuum degassing, control the temperature at 25-45°C, and after 30-60 minutes, obtain the product;

[0017] Preparation of component S2.B: Add the curing agent and accelerator into a stirring kettle, evacuate the vessel, and stir for 30-40 minutes.

[0018] S3: Add component A and component B into a mixing barrel according to the required weight ratio and stir to obtain the product.

[0019] Beneficial effects: The epoxy potting resin prepared by the present invention has the following advantages:

[0020] 1. The epoxy potting resin prepared by the present invention can meet the situation that no defoaming equipment is present during the preparation process, the product has suitable viscosity and good fluidity, and the precipitation of inactive substances is avoided during use, and it has durability;

[0021] 2. The epoxy potting resin prepared by the present invention can improve its adhesion on metal parts when used in condensing pump equipment, ensuring that the condensing pump is not easy to crack during hot and cold cycle use, and has strong sealing, which indirectly ensures the wet heat performance and waterproof performance of the product;

[0022] 3. The epoxy potting resin prepared by the present invention changes the heat resistance of the epoxy potting resin by adding fillers. At the same time, when used in this system, the influence of the addition of fillers on the flexibility of the epoxy potting resin can be avoided. DETAILED DESCRIPTION

[0023] The content of the present invention can be more easily understood by selecting the following detailed description of the preferred implementation method of the present invention and the embodiments included. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art to which the present invention belongs. When there is a conflict, the definition in this specification shall prevail.

[0024] As used herein, the term "prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0025] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0026] When amount, concentration or other value or parameter is expressed as range, preferred range or a series of upper preferred value and lower preferred value limit range, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.

[0027] Singular forms include plural references unless the context clearly indicates otherwise. "Optional" or "either" means that the subsequently described event or incident may or may not occur, and that the description includes instances where the event occurs and instances where it does not.

[0028] Approximate terms in the specification and claims are used to modify quantities, indicating that the present invention is not limited to the specific quantity, but also includes acceptable and modified parts close to the quantity without causing changes in the relevant basic functions. Accordingly, the use of "about", "approximately", etc. to modify a numerical value means that the present invention is not limited to the exact numerical value. In some examples, the approximate terms may correspond to the accuracy of the instrument for measuring the numerical value. In the specification and claims of this application, range limitations can be combined and / or interchanged, and if not otherwise stated, these ranges include all subranges contained therein.

[0029] In addition, the indefinite articles "a" and "an" before the elements or components of the present invention have no restrictions on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number is obviously intended to be in the singular form.

[0030] In order to solve the above problems, the first aspect of the present invention provides a novel flame retardant epoxy potting resin, comprising component A and component B; the weight ratio of component A to component B is 100:(20-50).

[0031] The raw materials for preparing the component A include, by weight: 25-35 parts of epoxy resin, 20-35 parts of inorganic filler, 1-15 parts of diluent, and 1-5 parts of black paste;

[0032] The raw materials for preparing the B component include: a curing agent and an accelerator.

[0033] As a preferred embodiment, the raw materials for preparing the A component further include a silane coupling agent, a wetting dispersant, a defoaming agent, a leveling agent, and a flame retardant.

[0034] As a preferred embodiment, the raw materials for preparing component A also include 0.1-1 parts of silane coupling agent, 0.1-1 parts of wetting dispersant, 0.1-1 parts of defoaming agent, 0.1-1 parts of leveling agent, and 20-30 parts of flame retardant.

[0035] As a preferred embodiment, the weight ratio of the wetting dispersant, the defoaming agent and the leveling agent is (1-2): (1.5-2.5):1.

[0036] As a preferred embodiment, the defoaming agent includes but is not limited to BYK-555, BYK-A501, BYK-A500, BYK-A515, BYK065, and ACP5500.

[0037] As a preferred embodiment, the leveling agent includes but is not limited to BYK320, BYK077, BYK333, BYK300, BYK301, BYK306, BYK322, BYK323, BYK331, and BYK345.

[0038] As a preferred embodiment, the wetting dispersant includes but is not limited to BYK110, BYK-W996, and BYK-160.

[0039] As a preferred embodiment, the flame retardant is selected from halogen-free flame retardants.

[0040] As a preferred embodiment, the silane coupling agent is selected from KH560.

[0041] Epoxy potting resin has a high viscosity, so vacuum degassing equipment is generally required during preparation. However, sometimes the production conditions do not meet the requirements, and vacuum degassing equipment is difficult to achieve. Therefore, it is necessary to ensure that the product itself has a good self-degassing effect. The applicant has found through a large number of creative experiments that when the weight ratio of the wetting dispersant, defoamer, and leveling agent is (1-2): (1.5-2.5): 1, the viscosity of the product can be reduced and its flow properties can be improved. The applicant unexpectedly found that when the weight ratio of the selected wetting dispersant, defoamer, and leveling agent is 2:2:1, the obtained product can have good durability. The applicant speculates that the possible reasons are: a certain weight of wetting dispersant added to the epoxy resin can improve the mixing stability, and the synergistic defoamer and leveling agent can form a micro-crosslinked state with the active groups in the system. When used for condensation pumps, it can form a "cage" effect on the inactive substances in the product during long-term use, avoiding the precipitation of inactive substances, and ensuring the durability of the product when used in condensation pumps.

[0042] In addition, the applicant has found that if too much wetting dispersant is added, the steric hindrance in the system will be too large, thus affecting the stability of the product.

[0043] As a preferred embodiment, the inorganic filler is selected from one or more of aluminum hydroxide, silicon dioxide, calcium carbonate, mica powder, quartz powder, and talc powder.

[0044] As a preferred embodiment, the filler is selected from aluminum hydroxide.

[0045] As a preferred embodiment, the filler is selected from silicon dioxide.

[0046] As a preferred embodiment, the filler is selected from aluminum hydroxide and silicon dioxide.

[0047] As a preferred embodiment, the weight ratio of the aluminum hydroxide to silicon dioxide is 1:(1-3).

[0048] As a preferred embodiment, the weight ratio of aluminum hydroxide to silicon dioxide is 1:2.

[0049] During the experiment, the applicant found that adding aluminum hydroxide and silicon dioxide would enhance the heat resistance of epoxy potting resin, but the applicant found that adding too much aluminum hydroxide may increase the processing difficulty in the system. After a large number of creative experiments, the applicant found that when the weight ratio of aluminum hydroxide and silicon dioxide is 1: (1-3), the heat resistance of epoxy potting resin can be maximized under the condition of ensuring the appropriate viscosity of the system. The applicant speculates that the possible reason is: with the addition of aluminum hydroxide and silicon dioxide in a weight ratio of 1: (1-3) to the system, under the synergistic effect of silane coupling agent, defoamer, wetting dispersant, and leveling agent, aluminum hydroxide and silicon dioxide will form a stable heat-conducting "network" in the epoxy resin. When subjected to high temperature, heat flow can be quickly transmitted along the "network", avoiding the influence of local heating on the material, thereby avoiding the migration of aluminum hydroxide and silicon dioxide, and ensuring the product safety and stability used for epoxy potting resin.

[0050] However, the applicant has found that the total weight of fillers added to the system is too large, which has a certain impact on the flexibility and adhesion of the product.

[0051] As a preferred embodiment, the diluent is selected from active diluents and / or inactive diluents.

[0052] As a preferred embodiment, the diluent is selected from active diluents.

[0053] As a preferred embodiment, the active diluent is selected from at least one of benzyl glycidyl ether, carbon dodeca- to tetradecyl glycidyl ether, alkylene glycidyl ether, trimethylolpropane triglycidyl ether, and castor oil polyglycidyl ether.

[0054] As a preferred embodiment, the active diluent is selected from benzyl glycidyl ether.

[0055] Benzyl glycidyl ether was purchased from Suzhou Senfeida Chemical Co., Ltd.

[0056] As a preferred embodiment, the active diluent is selected from carbon dodeca- to tetradecyl glycidyl ether.

[0057] C12-14 alkyl glycidyl ether, model number KDS6465465, was purchased from Kangdisi Chemical (Hubei) Co., Ltd.

[0058] As a preferred embodiment, the active diluent is selected from benzyl glycidyl ether and carbon dodeca- to tetradecyl glycidyl ether.

[0059] As a preferred embodiment, the weight ratio of benzyl glycidyl ether to carbon dodeca- to tetradecyl glycidyl ether is (0.2-0.5):1.

[0060] In order to solve the problem of excessive hardness and low adhesion of the product caused by the addition of a large amount of fillers, the applicant has found through a large number of creative experiments in the experimental process that the selection of benzyl glycidyl ether and carbon twelve to tetradecyl glycidyl ether in this application not only improves the flexibility of the product, but also improves its adhesion on the condensate pump and metal parts when its weight ratio is (0.2-0.5): 1. The applicant speculates the possible reasons: benzyl glycidyl ether and carbon twelve to tetradecyl glycidyl ether are added to the epoxy resin system, wherein the addition of carbon twelve to tetradecyl glycidyl ether can improve the rigidity of the bisphenol A type epoxy resin system, and at the same time, in conjunction with benzyl glycidyl ether, the originally regular cross-linked network is destroyed, the distance between molecules is significantly increased, the cross-linking density is reduced, and the cohesion is reduced, thereby improving its adhesion on the surface of the condensate pump.

[0061] As a preferred embodiment, the amount of aluminum hydroxide used is 20-30 times that of the wetting dispersant.

[0062] The applicant found that the addition of aluminum hydroxide would affect the viscosity and heat resistance of the system. However, the applicant found that if the amount of aluminum hydroxide is 20-30 times the weight of the wetting dispersant, the excellent high and low temperature resistance of the epoxy potting resin when used in the condensation pump can be improved under the premise of ensuring the stability and viscosity of the system. The applicant found that when the weight of aluminum hydroxide is too large, the hydroxyl groups on the surface of aluminum hydroxide will chemically bond and physically adsorb with active groups such as epoxy resin. As the amount of aluminum hydroxide increases, the force increases, resulting in the phenomenon of difficult processing in the system; however, when the weight of aluminum hydroxide is reduced, the product will be affected by low or high temperature, the heat transfer energy will be limited, the local temperature will be too high or too low, and the condensation pump will crack during the hot and cold cycle, and the resin will be removed, affecting the use of the condensation pump.

[0063] In this application, the black paste can be made by yourself or purchased; there is no special restriction on the manufacturer of purchase, and the preparation method can refer to the following steps:

[0064] Mix carbon black and 128 base resin in a weight ratio of 1:1.5 and grind to obtain the product.

[0065] The carbon black is commonly available on the market, and the 128 base resin is purchased from Jiangsu Yangnong Chemical Co., Ltd.

[0066] As a preferred embodiment, the epoxy resin in component A is selected from bisphenol A epoxy resin.

[0067] As a preferred embodiment, the raw materials for preparing component A include, by weight: 25-35 parts of bisphenol A epoxy resin, 1-5 parts of black paste, 0.1-1 parts of silane coupling agent, 0.1-1 parts of wetting dispersant, 0.1-1 parts of defoaming agent, 0.1-1 parts of leveling agent, 20-30 parts of flame retardant, 20-35 parts of inorganic filler, and 1-15 parts of diluent.

[0068] As a preferred embodiment, the raw materials for preparing the B component include, by weight: 95-99 parts of a curing agent and 1-5 parts of an accelerator.

[0069] As a preferred embodiment, the curing agent is selected from methyltetrahydrophthalic anhydride and / or methylhexahydrophthalic anhydride.

[0070] As a preferred embodiment, the accelerator is selected from at least one of N,N-dimethylbenzylamine, 2-ethyl-4-methylimidazole and N-methylimidazole.

[0071] The second aspect of the present invention provides a method for preparing a novel flame retardant epoxy potting resin, comprising the following steps:

[0072] S1. Preparation of component A: first add epoxy resin, silane coupling agent, black paste, wetting dispersant, defoamer and leveling agent into a stirring device, stir for 5-10 minutes, control the temperature at 15-30°C, then add flame retardant and inorganic filler, stir at low speed for 10 minutes, then stir at high speed for 45-60 minutes, control the temperature between 25-45°C, finally add diluent and stir at high speed for 30-40 minutes, turn on vacuum degassing, control the temperature at 25-45°C, and after 30-60 minutes, obtain the product;

[0073] Preparation of component S2.B: Add the curing agent and accelerator into a stirring kettle, evacuate the vessel, and stir for 30-40 minutes.

[0074] S3: Add component A and component B into a mixing barrel according to the required weight ratio and stir to obtain the product.

[0075] The present invention is described in detail below by way of examples. It is necessary to point out here that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by professionals and technicians in this field based on the above content of the present invention still belong to the scope of protection of the present invention.

[0076] In addition, unless otherwise stated, all raw materials used were commercially available.

[0077] Example

[0078] Example 1

[0079] A novel flame retardant epoxy potting resin comprises a component A and a component B; the weight ratio of the component A to the component B is 100:30.

[0080] The raw materials for preparing component A include, by weight: 25 parts of bisphenol A epoxy resin, 1 part of black paste, 0.1 part of silane coupling agent, 1 part of wetting dispersant, 1 part of defoaming agent, 0.5 part of leveling agent, 20 parts of flame retardant, 20 parts of inorganic filler, and 1 part of diluent.

[0081] The silane coupling agent is selected from KH560;

[0082] The wetting dispersant is selected from BYK110;

[0083] The defoamer is selected from BYK065;

[0084] The leveling agent is selected from BYK320;

[0085] The flame retardant is selected from phosphorus-nitrogen flame retardants;

[0086] The inorganic filler is selected from aluminum hydroxide;

[0087] The diluent is selected from benzyl glycidyl ether, which is purchased from Suzhou Senfeida Chemical Co., Ltd.

[0088] Bisphenol A epoxy resin was purchased from Hubei Shixing Chemical Co., Ltd.

[0089] The preparation method of the black paste refers to the following steps: mix carbon black and 128 base resin in a weight ratio of 1:1.5, grind, and obtain the black paste.

[0090] The carbon black is commonly available on the market, and the 128 base resin is purchased from Jiangsu Yangnong Chemical Co., Ltd.

[0091] The raw materials for preparing component B include, by weight: 95 parts of curing agent and 5 parts of accelerator.

[0092] The curing agent is selected from methyltetrahydrophthalic anhydride;

[0093] The accelerator is selected from N,N-dimethylbenzylamine.

[0094] A method for preparing a novel flame retardant epoxy potting resin comprises the following steps:

[0095] Preparation of component S1.A: first add epoxy resin, silane coupling agent, black paste, wetting dispersant, defoamer and leveling agent into a stirring device, stir for 10 minutes, control the temperature at 25°C, then add flame retardant and inorganic filler, stir at a low speed of 50 rpm for 10 minutes, then stir at a high speed of 600 rpm for 60 minutes, control the temperature at 40°C, finally add diluent and stir at 600 rpm for 40 minutes, turn on vacuum degassing, control the temperature at 40°C, and obtain after 60 minutes;

[0096] Preparation of component S2.B: Add the curing agent and accelerator into a stirring kettle, evacuate the vessel, and stir for 40 minutes.

[0097] S3: Add component A and component B into a mixing barrel according to the required weight ratio and stir to obtain the product.

[0098] Example 2

[0099] A novel flame retardant epoxy potting resin comprises a component A and a component B; the weight ratio of the component A to the component B is 100:30.

[0100] The raw materials for preparing component A include, by weight: 35 parts of bisphenol A epoxy resin, 5 parts of black paste, 1 part of silane coupling agent, 1 part of wetting dispersant, 1 part of defoaming agent, 0.5 parts of leveling agent, 30 parts of flame retardant, 30 parts of inorganic filler, and 15 parts of diluent.

[0101] The silane coupling agent is selected from KH560;

[0102] The wetting dispersant is selected from BYK110;

[0103] The defoamer is selected from BYK065;

[0104] The leveling agent is selected from BYK320;

[0105] The flame retardant is selected from phosphorus-nitrogen flame retardants;

[0106] The inorganic filler is selected from silicon dioxide;

[0107] The diluent is selected from benzyl glycidyl ether, which is purchased from Suzhou Senfeida Chemical Co., Ltd.

[0108] Bisphenol A epoxy resin was purchased from Hubei Shixing Chemical Co., Ltd.

[0109] The preparation method of the black paste refers to the following steps: mix carbon black and 128 base resin in a weight ratio of 1:1.5, grind, and obtain the black paste.

[0110] The carbon black is commonly available on the market, and the 128 base resin is purchased from Jiangsu Yangnong Chemical Co., Ltd.

[0111] The raw materials for preparing component B include, by weight: 99 parts of curing agent and 1 part of accelerator.

[0112] The curing agent is selected from methyltetrahydrophthalic anhydride;

[0113] The accelerator is selected from N,N-dimethylbenzylamine.

[0114] A method for preparing a novel flame retardant epoxy potting resin comprises the following steps:

[0115] Preparation of component S1.A: first add epoxy resin, silane coupling agent, black paste, wetting dispersant, defoamer and leveling agent into a stirring device, stir for 10 minutes, control the temperature at 25°C, then add flame retardant and inorganic filler, stir at a low speed of 50 rpm for 10 minutes, then stir at a high speed of 600 rpm for 60 minutes, control the temperature at 40°C, finally add diluent and stir at 600 rpm for 40 minutes, turn on vacuum degassing, control the temperature at 40°C, and obtain after 60 minutes;

[0116] Preparation of component S2.B: Add the curing agent and accelerator into a stirring kettle, evacuate the vessel, and stir for 40 minutes.

[0117] S3: Add component A and component B into a mixing barrel according to the required weight ratio and stir to obtain the product.

[0118] Example 3

[0119] A novel flame retardant epoxy potting resin comprises a component A and a component B; the weight ratio of the component A to the component B is 100:30.

[0120] The raw materials for preparing component A include, by weight: 30 parts of bisphenol A epoxy resin, 3 parts of black paste, 0.6 parts of silane coupling agent, 0.4 parts of wetting dispersant, 0.4 parts of defoaming agent, 0.2 parts of leveling agent, 25 parts of flame retardant, 30 parts of inorganic filler, and 8 parts of diluent.

[0121] The silane coupling agent is selected from KH560;

[0122] The wetting dispersant is selected from BYK110;

[0123] The defoamer is selected from BYK065;

[0124] The leveling agent is selected from BYK320;

[0125] The flame retardant is selected from phosphorus-nitrogen flame retardants;

[0126] The inorganic filler is selected from aluminum hydroxide and silicon dioxide, and the weight ratio thereof is 1:2;

[0127] The diluent is selected from benzyl glycidyl ether and carbon 12-14 alkyl glycidyl ether, and the weight ratio thereof is 0.4:1.

[0128] Benzyl glycidyl ether was purchased from Suzhou Senfida Chemical Co., Ltd.; C12-14 alkyl glycidyl ether, model KDS6465465, was purchased from Kangdisi Chemical (Hubei) Co., Ltd.

[0129] Bisphenol A epoxy resin was purchased from Hubei Shixing Chemical Co., Ltd.

[0130] The preparation method of the black paste refers to the following steps: mix carbon black and 128 base resin in a weight ratio of 1:1.5, grind, and obtain the black paste.

[0131] The carbon black is commonly available on the market, and the 128 base resin is purchased from Jiangsu Yangnong Chemical Co., Ltd.

[0132] The raw materials for preparing component B include, by weight: 97 parts of curing agent and 3 parts of accelerator.

[0133] The curing agent is selected from methyltetrahydrophthalic anhydride;

[0134] The accelerator is selected from N,N-dimethylbenzylamine.

[0135] A method for preparing a novel flame retardant epoxy potting resin comprises the following steps:

[0136] Preparation of component S1.A: first add epoxy resin, silane coupling agent, black paste, wetting dispersant, defoamer and leveling agent into a stirring device, stir for 10 minutes, control the temperature at 25°C, then add flame retardant and inorganic filler, stir at a low speed of 50 rpm for 10 minutes, then stir at a high speed of 600 rpm for 60 minutes, control the temperature at 40°C, finally add diluent and stir at 600 rpm for 40 minutes, turn on vacuum degassing, control the temperature at 40°C, and obtain after 60 minutes;

[0137] Preparation of component S2.B: Add the curing agent and accelerator into a stirring kettle, evacuate the vessel, and stir for 40 minutes.

[0138] S3: Add component A and component B into a mixing barrel according to the required weight ratio and stir to obtain the product.

[0139] Example 4

[0140] A novel flame retardant epoxy potting resin, the specific implementation manner of which is the same as that of Example 3, except that the weight ratio of aluminum hydroxide to silicon dioxide in the inorganic filler is 1:1.

[0141] Example 5

[0142] A novel flame retardant epoxy potting resin, the specific implementation manner of which is the same as that of Example 3, except that the weight ratio of aluminum hydroxide to silicon dioxide in the inorganic filler is 2:1.

[0143] Example 6

[0144] A novel flame retardant epoxy potting resin, the specific implementation manner of which is the same as that of Example 3, except that the weight portion of the leveling agent is 0.4 parts.

[0145] Example 7

[0146] A novel flame retardant epoxy potting resin, the specific implementation manner of which is the same as that of Example 3, except that the weight portion of the defoaming agent is 0.8 parts.

[0147] Performance Test:

[0148] 1. The product obtained in Example 1 was tested for the viscosity of component A, the viscosity of component B, the mixed viscosity, the specific gravity of component A, the specific gravity of component B, and the gelation time, and the test results are summarized in the following Table 1.

[0149] Table 1:

[0150]

[0151]

[0152] 2. Flame retardant performance test: After the epoxy potting resin prepared in Examples 1-3 was used in a condensing pump, a flame retardant performance test was performed. The test standard was based on EN 13501-1:2018, and the test results were statistically summarized in Table 2 below.

[0153] 3. Ball pressure test: The epoxy potting resin prepared in Examples 1-3 was used for a condensing pump and subjected to a ball pressure test. The resin was placed in an environment at 25°C and a humidity of 30%-90% for 24 hours, and then pressed with a 5mm steel ball with a force of 20N, and then placed in an oven at 125°C±2°C. After one hour, the steel ball was removed and the component was placed in cold water for 10 seconds to cool to room temperature. The pressure surface diameter that did not exceed 2mm was considered qualified, and the test results were statistically shown in Table 2 below.

[0154] 4. Wet heat test: The epoxy potting resin prepared in Example 1-3 is used for the condensing pump, and the wet heat test is carried out. The test method refers to GB / T2423.3, the test cycle is 4d, and the insulation resistance of the motor after the test should be above 1MΩ, and it can withstand a voltage of 1275V for 1min. If there is no breakdown or flashover phenomenon, it is considered qualified, and the test results are statistically summarized in Table 2 below.

[0155] Table 2:

[0156] experiment Flame retardant properties Ball pressure performance test Damp heat test Example 1 A1 qualified qualified Example 2 A1 qualified qualified Example 3 A1 qualified qualified

[0157] 4. Thermal shock performance test: The epoxy potting resin prepared in Examples 3-7 was subjected to a thermal shock performance test and placed in a high-temperature oven at 80°C ± 3°C for 24 hours. It is stipulated that the epoxy potting resin without deformation or bubbling is recorded as having excellent thermal shock performance; the epoxy potting resin with slight deformation or bubbling is recorded as having good thermal shock performance; the epoxy potting resin with severe deformation or bubbling is recorded as having poor thermal shock performance, and the results are summarized in the following Table 3.

[0158] 5. Adhesion test: The epoxy potting resin prepared in Example 3-7 was used for a condensation pump to perform an adhesion test. The test method was based on GB / T 9286-88, and the test results are summarized in Table 3 below.

[0159] 6. Low temperature freezing test: The epoxy potting resin prepared in Example 3-7 is used for a condensing pump, and then a low temperature freezing test is performed. The pump is placed in a -20°C ± 3°C low temperature box for 48 hours. After being taken out, the motor housing surface and the epoxy resin are observed for cracks or damage. The test results are summarized in Table 3 below.

[0160] Table 3:

[0161] experiment Thermal shock performance Adhesion Low temperature freezing performance Example 3 excellent 0 No cracks, no damage Example 4 good 0 Cracks appear Example 5 Difference 1 Cracks appear Example 6 good 0 No cracking Example 7 Difference 1 No cracking

[0162] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A novel flame retardant epoxy potting resin, characterized in that: The invention comprises a component A and a component B; the weight ratio of the component A to the component B is 100:(20-50); The raw materials for preparing the component A include, by weight: 25-35 parts of epoxy resin, 20-35 parts of inorganic filler, 1-15 parts of diluent, and 1-5 parts of black paste; The raw materials for preparing the B component include: a curing agent and an accelerator; The raw materials for preparing the A component also include a silane coupling agent, a wetting dispersant, a defoaming agent, a leveling agent, and a flame retardant; The raw materials for preparing the A component also include 0.1-1 parts of silane coupling agent, 0.1-1 parts of wetting dispersant, 0.1-1 parts of defoaming agent, 0.1-1 parts of leveling agent, and 20-30 parts of flame retardant; The weight ratio of the wetting dispersant, defoamer and leveling agent is (1-2): (1.5-2.5): 1; The inorganic filler is selected from aluminum hydroxide and silicon dioxide, and the weight ratio of the aluminum hydroxide to silicon dioxide is 1:

2.

2. The novel flame retardant epoxy potting resin according to claim 1, characterized in that: The diluent is selected from active diluents and / or inactive diluents.

3. The novel flame retardant epoxy potting resin according to claim 2, characterized in that: The active diluent is selected from at least one of benzyl glycidyl ether, carbon 12-14 alkyl glycidyl ether, alkylene glycidyl ether, trimethylolpropane triglycidyl ether and castor oil polyglycidyl ether.

4. The novel flame retardant epoxy potting resin according to claim 1, characterized in that: The raw materials for preparing the B component include, by weight: 95-99 parts of a curing agent and 1-5 parts of an accelerator.

5. The novel flame retardant epoxy potting resin according to claim 4, characterized in that: The curing agent is selected from methyltetrahydrophthalic anhydride and / or methylhexahydrophthalic anhydride.

6. A method for preparing the novel flame retardant epoxy potting resin according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Preparation of component A: first add epoxy resin, silane coupling agent, black paste, wetting dispersant, defoamer and leveling agent into a stirring device, stir for 5-10 minutes, control the temperature at 15-30°C, then add flame retardant and inorganic filler, stir at low speed for 10 minutes, then stir at high speed for 45-60 minutes, control the temperature between 25-45°C, finally add diluent and stir at high speed for 30-40 minutes, turn on vacuum degassing, control the temperature at 25-45°C, and after 30-60 minutes, obtain the product; Preparation of S2.B component: Add the curing agent and accelerator into a stirring kettle, evacuate the kettle, and stir for 30-40 minutes to obtain the product; S3: Add component A and component B into a mixing barrel according to the required weight ratio and stir to obtain the product.