All-solid-state battery

By using spinel-type active substances and halide solid electrolytes covering the lithium oxide layer in an all-solid battery, the problem of increasing heat generated by Si-based negative electrode active substances is solved, and safer and more efficient battery performance is achieved.

CN114665147BActive Publication Date: 2024-12-03TOYOTA JIDOSHA KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111457196.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-12-22
Filing Date
2021-12-02
Publication Date
2024-12-03
Estimated Expiration
2041-12-02

AI Technical Summary

Technical Problem

When the Si-based negative electrode active substance reacts with the positive electrode active substance in the battery, it may lead to an increase in the heat generation, affecting the safety and efficiency of the battery.

Method used

A composite positive electrode active material is used, in which the spinel-type active material is covered with a lithium oxide layer, and a halogen-containing halide solid electrolyte is used to form an all-solid battery structure to reduce the increase in heat generation.

Benefits of technology

The heat generation of the all-solid battery when using the Si-based negative electrode active substance is effectively reduced, the safety and efficiency of the battery are improved, and the reaction between the positive electrode active substance and the solid electrolyte is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114665147B_ABST
    Figure CN114665147B_ABST
Patent Text Reader

Abstract

The main purpose of the present disclosure is to provide an all-solid-state battery capable of reducing heat generation. In the present disclosure, the above-mentioned problem is solved by providing an all-solid-state battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer formed between the positive electrode layer and the negative electrode layer, the positive electrode layer containing a composite positive electrode active material and a halide solid electrolyte, the composite positive electrode active material having a spinel-type active material and a lithium oxide layer covering the surface of the spinel-type active material, the halide solid electrolyte containing an X element (X is a halogen) as a main component of an anion, and the negative electrode layer containing a Si-based negative electrode active material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to all-solid-state batteries. Background Art

[0002] An all-solid-state battery is a battery having a solid electrolyte layer between a positive electrode and a negative electrode, and has an advantage of easily simplifying a safety device as compared with a liquid-based battery having an electrolytic solution containing a flammable organic solvent.

[0003] For example, Patent Document 1 discloses a sulfide all-solid-state battery that uses an active material in which a spinel-type active material is covered with lithium niobate as a positive electrode active material, and uses a Si-based negative electrode active material as a negative electrode active material. Patent Document 2 discloses a solid electrolyte represented by Li 6-3z Y z X6 (where 0 < z < 2 and x is Br or Cl). Patent Document 3 discloses using Li3YI6 and Li2S-P2S5 in combination in the solid electrolyte layer of a battery. In addition, Patent Document 4 describes that the positive electrode layer and the solid electrolyte layer contain Li3YBr2Cl2I2, and the negative electrode layer contains Li2S-P2S5.

[0004] Prior Art Documents

[0005] Patent Document 1: Japanese Unexamined Patent Application Publication No. 2019-207793

[0006] Patent Document 2: International Publication No. 2018 / 025582

[0007] Patent Document 3: International Publication No. 2019 / 135323

[0008] Patent Document 4: International Publication No. 2019 / 146216 Summary of the Invention

[0009] The Si-based negative electrode active material has good capacity characteristics. On the other hand, when the Si-based negative electrode active material reacts with, for example, oxygen generated from the positive electrode active material, the calorific value may increase. The present disclosure has been completed in view of the above actual situation, and its main object is to provide an all-solid-state battery capable of reducing the calorific value.

[0010] To solve the above problems, in the present disclosure, there is provided an all-solid-state battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer formed between the positive electrode layer and the negative electrode layer, the positive electrode layer containing a composite positive electrode active material and a halide solid electrolyte, the composite positive electrode active material having a spinel-type active material and a lithium oxide layer covering the surface of the spinel-type active material, the halide solid electrolyte containing an X element (X is a halogen) as a main component of anions, and the negative electrode layer containing a Si-based negative electrode active material.

[0011] According to the present disclosure, the positive electrode layer contains a composite positive electrode active material in which the surface of a spinel active material is covered with a lithium oxide layer and a halide solid electrolyte, so an all-solid-state battery can be obtained that can reduce the increase in heat generation even when a Si-based negative electrode active material is used.

[0012] In the above disclosure, the above halide solid electrolyte may contain Li element, M element (M is a metal other than Li) and the above X element.

[0013] In the above disclosure, the above halide solid electrolyte may contain Y as the above M.

[0014] In the above disclosure, the above halide solid electrolyte may contain at least one of Br and Cl as the above X.

[0015] In the above disclosure, the above lithium oxide may be at least one of LiNbO3 and Li2WO4.

[0016] In the above disclosure, the average thickness of the lithium oxide layer is 2.3 times the average particle size (D) of the spinel type active material. 50 ) can be in a range of 0.05% to 5%.

[0017] In the above disclosure, the negative electrode layer and the solid electrolyte layer may each contain a sulfide solid electrolyte.

[0018] In the present disclosure, there is an effect of being able to reduce the increase in heat generation in the all-solid-state battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic cross-sectional view illustrating an all-solid-state battery in the present disclosure.

[0020] Figure 2 This is a schematic cross-sectional view illustrating a composite positive electrode active material in the present disclosure.

[0021] Description of Reference Numerals

[0022] 1… Positive electrode layer

[0023] 2…Negative electrode layer

[0024] 3…Solid electrolyte layer

[0025] 4…Positive electrode collector

[0026] 5…Negative electrode collector

[0027] 6…Spinel-type active substances

[0028] 7…Lithium oxide layer

[0029] 8…Composite positive electrode active material

[0030] 10…All-solid-state batteries DETAILED DESCRIPTION

[0031] Hereinafter, the all-solid-state battery in the present disclosure will be described in detail.

[0032] Figure 1 : is a schematic cross-sectional view illustrating an all-solid-state battery in the present disclosure. Figure 2 This is a schematic cross-sectional view illustrating a composite positive electrode active material in the present disclosure. Figure 1 The all-solid-state battery 10 shown has: a positive electrode layer 1, a negative electrode layer 2, an electrolyte layer 3 formed between the positive electrode layer 1 and the negative electrode layer 2, a positive electrode collector 4 for collecting current from the positive electrode layer 1, and a negative electrode collector 5 for collecting current from the negative electrode layer 2. The positive electrode layer 1 contains a composite positive electrode active material and a halide solid electrolyte. Figure 2 As shown, the composite positive electrode active material 8 has a spinel type active material 6 and a lithium oxide layer 7 covering the surface thereof. In addition, the halide solid electrolyte is a solid electrolyte containing an X element (X is a halogen) as the main component of the anion. On the other hand, the negative electrode layer 2 contains a Si-based negative electrode active material.

[0033] According to the present disclosure, the positive electrode layer contains a composite positive electrode active material in which the surface of a spinel active material is covered with a lithium oxide layer and a halide solid electrolyte, so it becomes an all-solid-state battery that can reduce the increase in heat generation even when a Si-based negative electrode active material is used.

[0034] As described above, the capacity characteristics of Si-based negative electrode active materials are good. On the other hand, when it reacts with oxygen generated from the positive electrode active material, the calorific value may increase. In particular, it is believed that the reactivity of Si-based negative electrode active materials that absorb lithium with oxygen becomes higher, and reaction heat is generated due to the reaction of O and Si. On the other hand, as shown in the embodiments described later, the inventors found that when the positive electrode layer contains a predetermined composite positive electrode active material and a halide solid electrolyte, the calorific value at the positive electrode is significantly suppressed. It is believed that this is due to the suppression of the amount of oxygen generated by the positive electrode active material. In addition, it is believed that the lithium oxide layer suppresses the reaction between the positive electrode active material and the solid electrolyte. The reason why the oxygen generation is suppressed is not clear, but it is believed that it is because the crystal structure of the spinel-type active material is stable and it is difficult to generate oxygen from the active material. In addition, it is believed that it is difficult for oxygen to escape from the positive electrode active material because the reactivity of the halide solid electrolyte with oxygen is low.

[0035] 1. Positive electrode layer

[0036] The positive electrode layer in the present disclosure contains at least a composite positive electrode active material and a halide solid electrolyte.

[0037] The composite positive electrode active material in the present disclosure includes a spinel-type active material and a lithium oxide layer covering the surface of the spinel-type active material.

[0038] A spinel-type active material is an active material having a spinel-type crystal structure. Whether or not it has a spinel-type crystal structure can be determined by conventionally known X-ray diffraction measurement (XRD). The spinel-type active material preferably contains, for example, Li element, Me element (Me is one or more transition metals) and O element. As Me, for example, Mn, Ni, and Ti can be cited. The spinel-type active material preferably contains at least Mn as Me. In addition, the spinel-type active material may contain only Mn as Me, or may contain Mn and transition metals other than Mn. In the latter case, it is particularly preferred that the spinel-type active material contains Mn and Ni as Me.

[0039] The spinel type active material preferably has a composition such as LiMe2O4 (Me is one or more transition metals). Me is the same as described above. Specific examples of such spinel type active materials include LiMn2O4, Li(Ni 0.5 Mn 1.5 )O4. In addition, the spinel type active material may be lithium titanate containing Li, Ti and O. As the composition of lithium titanate, for example, Li4Ti5O 12 In addition, as the spinel type active material in the composite positive electrode active material, only one type may be used, or two or more types may be used.

[0040] The shape of the spinel type active material may be, for example, a granular shape. The average particle size (D 50 ) is, for example, 0.1 μm or more, 0.5 μm or more, or 1 μm or more. On the other hand, the average particle size (D 50 ) is, for example, 50 μm or less, or 20 μm or less. The average particle size (D 50 ) can be calculated, for example, by measurement using a laser diffraction particle size distribution analyzer or a scanning electron microscope (SEM).

[0041] The lithium oxide layer is a layer covering at least a portion of the surface of the spinel-type active material and containing lithium oxide. The lithium oxide layer can function as a reaction inhibition layer, and can inhibit the generation of reaction heat caused by the reaction between the spinel-type active material and the solid electrolyte. The lithium oxide layer is generally a layer having Li ion conductivity.

[0042] The lithium oxide preferably contains, for example, the Li element, the Me' element (Me' is one or more transition metals) and the O element. As Me', for example, Nb and W can be mentioned. As specific examples of such lithium oxides, LiNbO3 and Li2WO4 can be mentioned. In addition, the lithium oxide can have the Li element and the PO4 structure. As a specific example of such lithium oxide, Li3PO4 can be mentioned. In addition, the lithium oxide can also be Li3PO4 nitride, that is, LiPON. In addition, the lithium oxide contained in the lithium oxide layer can be only one kind or two or more kinds.

[0043] The average thickness of the lithium oxide layer is, for example, more than 10 nm, more than 30 nm, or more than 50 nm. On the other hand, the average thickness of the lithium oxide layer is, for example, less than 100 nm, less than 80 nm, or less than 60 nm. When the average thickness of the lithium oxide layer is too thin, the reaction between the spinel active material and the solid electrolyte cannot be fully suppressed. On the other hand, when the average thickness of the lithium oxide layer is too thick, the spinel active material cannot be fully covered. The average thickness of the lithium oxide layer can be measured, for example, using a transmission electron microscope (TEM). Specifically, it can be obtained by obtaining a cross-sectional SEM image of the composite positive electrode active material and measuring the thickness of any portion to calculate the average value.

[0044] The coverage of the lithium oxide layer is, for example, 70% or more, 80% or more, or 90% or more. On the other hand, the coverage may be 100% or less. The coverage can be determined by X-ray photoelectron spectroscopy (XPS).

[0045] Here, in the composite positive electrode active material of the present disclosure, the average thickness of the lithium oxide layer is 100 times the average particle size (D 50 ) is preferably within a predetermined range. The above ratio is, for example, greater than 0.05%, may be greater than 0.07%, or may be greater than 0.1%. On the other hand, the above ratio is, for example, less than 5%, may be less than 3%, may be less than 1%, or may be less than 0.5%. If it is within the above range, the reaction between the spinel active material and the solid electrolyte can be fully suppressed, thereby suppressing the increase in resistance of the all-solid-state battery.

[0046] The shape of the composite positive electrode active material may be, for example, a granular shape. The average particle size (D 50)For example, it can be 0.1 μm or more, can be 0.5 μm or more, and can also be 1 μm or more. On the other hand, the average particle diameter of the composite positive electrode active material is, for example, 50 μm or less, and can also be 20 μm or less. The average particle diameter of the composite positive electrode active material can be calculated, for example, by measurement using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0047] The positive electrode layer in the present disclosure contains a halide solid electrolyte. The halide solid electrolyte contains an X element (X is a halogen) as the main component of anions. The so-called "containing an X element as the main component of anions" means that among all anions constituting the halide solid electrolyte, the proportion (molar ratio) of the X element is the largest. The proportion of the X element relative to all anions constituting the halide solid electrolyte is, for example, 50 mol% or more, can be 70 mol% or more, can be 90 mol% or more, and can also be 100 mol%. The X element can be one kind or two or more kinds. In the latter case, the total of two or more X elements is taken as the above-mentioned "proportion of the X element". In addition, the halide solid electrolyte can also be a solid electrolyte that does not contain a sulfur element (S element).

[0048] The halide solid electrolyte preferably contains a Li element, an M element (M is a metal other than Li), and an X element (X is a halogen). As X, for example, F, Cl, Br, and I can be cited. In particular, the halide solid electrolyte preferably contains at least one of Br and Cl as the above-mentioned X. In addition, as M, for example, metal elements such as Sc, Y, B, Al, Ga, and In can be cited. In particular, the halide solid electrolyte in the present disclosure preferably contains at least Y as the above-mentioned M.

[0049] In addition, the composition of the halide solid electrolyte in the present disclosure is not particularly limited, but preferably consists of Li 6- 3a M a Br b Cl c (wherein M is a metal other than Li, a satisfies 0 < a < 2, b and c satisfy 0 ≤ b ≤ 6, satisfy 0 ≤ c ≤ 6 and satisfy b + c = 6.) is represented. a can be 0.75 or more, and can also be 1 or more. On the other hand, a can be 1.5 or less. b can be 1 or more, and can also be 2 or more. In addition, c can be 3 or more, and can also be 4 or more. As specific halide solid electrolytes, Li3YBr6, Li3YCl6, and Li3YBr2Cl4 can be cited. The positive electrode layer can contain only one kind of halide solid electrolyte or can contain two or more kinds of halide solid electrolytes.

[0050] As the shape of the halide solid electrolyte, for example, a granular shape can be cited. The average particle diameter (D 50) is not particularly limited, and may be, for example, 0.05 μm or more, or 0.1 μm or more. On the other hand, the average particle size of the halide solid electrolyte may be, for example, 50 μm or less, or 20 μm or less. The average particle size (D 50 ) can be calculated, for example, by measurement using a laser diffraction particle size distribution analyzer or a scanning electron microscope (SEM).

[0051] The positive electrode layer may contain only a halide solid electrolyte as a solid electrolyte, or may contain a solid electrolyte other than a halide solid electrolyte, but the former is preferred. In the latter case, the ratio of the halide solid electrolyte to the total amount of the solid electrolyte contained in the positive electrode layer is, for example, 50% by volume or more, 70% by volume or more, or 90% by volume or more. On the other hand, the above ratio is, for example, 99% by volume or less. As solid electrolytes other than halide solid electrolytes, the solid electrolytes described in "2. Negative electrode layer" described later can be cited.

[0052] In addition, as required, the positive electrode layer may also contain at least one of a conductive material and a binder. As a conductive material, for example, a carbon material, a metal particle, a conductive polymer can be cited. As a carbon material, for example, acetylene black (AB), Ketjen black (KB) and other granular carbon materials, carbon fiber, carbon nanotube (CNT), carbon nanofiber (CNF) and other fibrous carbon materials can be cited. In addition, as a binder, for example, a rubber-based binder such as butene rubber (BR), a fluoride-based binder such as polyvinylidene fluoride (PVDF) can be cited.

[0053] The thickness of the positive electrode layer is, for example, not less than 0.1 μm and not more than 1000 μm.

[0054] 2. Negative electrode layer

[0055] The negative electrode layer of the present disclosure contains at least a Si-based negative electrode active material. In addition, the negative electrode layer preferably contains a sulfide solid electrolyte. In addition, as required, the positive electrode layer may also contain at least one of a conductive material and a binder. Regarding the conductive material and the binder, the contents described in "1. Positive electrode layer" are the same, so the description here is omitted.

[0056] Si-based negative electrode active materials are active materials containing Si element. Examples of Si-based negative electrode active materials include Si element and Si alloy. Si alloy preferably contains Si element as the main component. Examples of the shape of Si-based negative electrode active materials include granular. The average particle size (D 50 ) is, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D 50 ) is, for example, 50 μm or less, or 20 μm or less. The average particle size (D50 ) can be calculated, for example, by measurement using a laser diffraction particle size distribution analyzer or a scanning electron microscope (SEM).

[0057] The proportion of Si-based negative electrode active material in the negative electrode layer is, for example, 20% by volume or more, 40% by volume or more, or 60% by volume or more. When the proportion of Si-based negative electrode active material is too small, it may not be possible to achieve an increase in volume energy density. On the other hand, the proportion of Si-based negative electrode active material in the negative electrode layer is, for example, 80% by volume or less. When the proportion of Si-based negative electrode active material is too much, it may not be possible to form a good electron conduction path and ion conduction path.

[0058] The negative electrode layer preferably contains a sulfide solid electrolyte. The negative electrode layer may contain only a sulfide solid electrolyte as a solid electrolyte, or may also contain a solid electrolyte other than a sulfide solid electrolyte, but the former is preferred. In the latter case, the ratio of the sulfide solid electrolyte to the total amount of the solid electrolyte contained in the negative electrode layer is, for example, 50% by volume or more, may be 70% by volume or more, or may be 90% by volume or more. On the other hand, the above ratio is, for example, 99% by volume or less. Furthermore, the negative electrode layer, as a negative electrode solid electrolyte, preferably does not contain the above-mentioned halide solid electrolyte. Because the halide solid electrolyte generally has low reduction resistance, the halide solid electrolyte is reduced and decomposed during charging, and the battery resistance may increase.

[0059] As a sulfide solid electrolyte, for example, a solid electrolyte containing Li element, X element (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, In) and S element can be mentioned. In addition, the sulfide solid electrolyte may also contain at least one of O element and halogen element. As a halogen element, for example, F element, Cl element, Br element, I element can be mentioned. The sulfide solid electrolyte can be glass (amorphous) or glass ceramic. As a sulfide solid electrolyte, for example, Li2S-P2S5, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-SiS2, Li2S-GeS2, Li2S-P2S5-GeS2 can be mentioned.

[0060] Examples of solid electrolytes other than sulfide solid electrolytes include inorganic solid electrolytes such as hydride solid electrolytes, oxide solid electrolytes, and nitride solid electrolytes.

[0061] In addition, the shape of the solid electrolyte may be, for example, a granular shape. The average particle size (D 50) is not particularly limited, and may be, for example, 0.05 μm or more, or 0.1 μm or more. On the other hand, the average particle size of the solid electrolyte may be, for example, 50 μm or less, or 20 μm or less. The average particle size (D 50 ) can be calculated, for example, by measurement using a laser diffraction particle size distribution analyzer or a scanning electron microscope (SEM).

[0062] The thickness of the negative electrode layer is, for example, 0.1 μm or more and 1000 μm or less.

[0063] 3. Solid electrolyte layer

[0064] The solid electrolyte layer in the present disclosure is a layer formed between the above-mentioned positive electrode layer and the above-mentioned negative electrode layer, and contains a solid electrolyte. In addition, the solid electrolyte layer preferably contains a sulfide solid electrolyte as a solid electrolyte. In addition, the solid electrolyte layer may contain a solid electrolyte other than a sulfide solid electrolyte, or may not contain it. Furthermore, the solid electrolyte layer preferably does not contain a halide solid electrolyte. Because during charging, the halide solid electrolyte is reduced and decomposed at the interface between it and the negative electrode layer, the battery resistance may increase. Regarding the types and proportions of solid electrolytes other than sulfide solid electrolytes and sulfide solid electrolytes, they are the same as those described in "2. Negative electrode layer", so they are omitted here.

[0065] In addition, the solid electrolyte layer may further contain a binder as required. The binder is the same as described in "1. Positive electrode layer", so the description here is omitted. The thickness of the solid electrolyte layer is, for example, 0.1 μm or more and 1000 μm or less.

[0066] 4. All-solid-state batteries

[0067] The all-solid battery in the present disclosure generally has a positive electrode collector for collecting current in the positive electrode layer, and a negative electrode collector for collecting current in the negative electrode layer. As the positive electrode collector, for example, Al foil can be cited. As the negative electrode collector, for example, Ni foil can be cited. In addition, the all-solid battery in the present disclosure can have a constraint fixture that applies a constraint pressure to the stacking direction of the positive electrode layer, the negative electrode layer, and the solid electrolyte layer. The constraint pressure is, for example, more than 0.1MPa, can be more than 1MPa, and can also be more than 5MPa. On the other hand, the constraint pressure is, for example, less than 100MPa, can be less than 50MPa, and can also be less than 20MPa.

[0068] The type of all-solid-state battery in the present disclosure is not particularly limited, and a typical example is a lithium-ion battery. In addition, the all-solid-state battery in the present disclosure may be a primary battery or a secondary battery, wherein a secondary battery is preferred. Because it can be repeatedly charged and discharged, it is useful as, for example, a vehicle-mounted battery.

[0069] The all-solid battery in the present disclosure may be a single cell or a stacked battery. The stacked battery may be a monopolar stacked battery (a stacked battery of a parallel type) or a bipolar stacked battery (a stacked battery of a series type). As the shape of the all-solid battery, for example, a coin type, a laminated type, a cylindrical type, and a square type may be cited.

[0070] The present disclosure is not limited to the above-mentioned embodiments. The above-mentioned embodiments are illustrative, and all schemes having substantially the same technical concept as that described in the claims of the present disclosure and having the same functions and effects are included in the technical scope of the present disclosure.

[0071] [Example]

[0072] [Example 1]

[0073] (Preparation of Composite Positive Electrode Active Material)

[0074] Using a rotary flow coating device (MP-01 manufactured by POWREX), a LiNbO3 precursor sol-gel solution is applied to the surface of the positive electrode active material (spinel lithium manganese oxide: LiMn2O4) and dried. Then, it is calcined at 200°C for 5 hours. Thus, a composite positive electrode active material having a LiNbO3 layer as a lithium oxide layer is obtained. The average particle size of the positive electrode active material is measured using a wet particle size distribution measuring device (SALD-7500 manufactured by Shimadzu Corporation). In addition, the thickness of the lithium oxide layer is calculated as follows. First, the composite positive electrode active material obtained by filling with resin is cross-sectioned using an ion milling device (IM4000PLUS manufactured by Hitachi High-Technologies) and observed by SEM. Then, the thickness of the lithium oxide layer is measured at any 5 points, and the average value is calculated.

[0075] (Production of positive electrode)

[0076] The dispersion medium (butyl butyrate), the binder (butyl butyrate solution of 5 wt% polyvinylidene fluoride binder), the conductive material (vapor-grown carbon fiber (VGCF)) and the halide solid electrolyte (Li3YBr2Cl4) are added to the mixing container of the filling mixer (30-L type made by PRIMIX) and stirred at 20000 rpm for 30 minutes. The above-mentioned composite positive electrode active material is added to the mixing container so that the volume ratio of the composite positive electrode active material to the halide solid electrolyte becomes 7:3, and the filling mixer is stirred at 15000 rpm for 60 minutes. Then, using a coater, it is applied to the positive electrode collector (Al foil) by a doctor blade method. The coated electrode is naturally dried and then dried on a hot plate at 100°C for 30 minutes. Thus, a positive electrode having a positive electrode collector and a positive electrode layer is obtained.

[0077] (Production of negative electrode)

[0078] The dispersion medium (butyl butyrate), the binder (5 wt % butyl butyrate solution of polyvinylidene fluoride binder), the negative electrode active material (silicon particles, average particle size D 50 = 2.5 μm), conductive material (vapor-grown carbon fiber (VGCF)) and sulfide solid electrolyte (Li2S-P2S5 glass ceramic containing LiI, average particle size D 50 =0.8μm) was added to a polypropylene (PP) container. Next, the PP container was stirred for 30 seconds using an ultrasonic disperser (UH-50 manufactured by SMT). Next, the PP container was vibrated for 30 minutes using a vibrator (TTM-1 manufactured by Shibata Science Co., Ltd.). Then, using a coater, it was applied to the negative electrode collector (Ni foil) by a doctor blade method. The coated electrode was naturally dried and then dried on a hot plate at 100°C for 30 minutes. Thus, a negative electrode having a negative electrode collector and a negative electrode layer was obtained.

[0079] (Fabrication of Solid Electrolyte Layer)

[0080] The dispersion medium (heptane), the binder (a 5 wt% heptane solution of a butene rubber-based binder), the sulfide solid electrolyte (a Li2S-P2S5-based glass ceramic containing LiI, an average particle size D 50 =2.5μm) was added to a PP container. Next, the PP container was stirred for 30 seconds using an ultrasonic dispersion device (UH-50 manufactured by SMT). Next, the PP container was vibrated for 30 minutes using a vibrator (TTM-1 manufactured by Shibata Science Co., Ltd.). Then, a coating device was used to apply it to a substrate (Al foil) by a doctor blade method. The applied solid electrolyte layer was naturally dried and then dried on a hot plate at 100°C for 30 minutes. Thus, a solid electrolyte layer was obtained.

[0081] (Production of Evaluation Batteries)

[0082] Place the solid electrolyte layer into 1 cm 2 In the mold, 1 ton / cm 2 Next, a positive electrode was placed on one side of the solid electrolyte layer and pressed at 1 ton / cm 2 Next, a negative electrode was placed on the other side of the solid electrolyte layer at 6 tons / cm 2 The positive and negative terminals were connected to the laminated body obtained after pressing, and sandwiched and welded with a laminate film to produce an evaluation battery. Next, the battery was restrained with a metal plate so that a pressure of 5 MPa was applied to the battery.

[0083] [Examples 2 to 4]

[0084] A composite positive electrode active material was prepared in the same manner as in Example 1 except that the ratio of the thickness of the lithium oxide layer to the average particle size of the spinel active material was set to the value shown in Table 1. An evaluation battery was prepared in the same manner as in Example 1 except that the obtained composite positive electrode active material was used.

[0085] [Examples 5 and 6]

[0086] An evaluation battery was produced in the same manner as in Example 1 except that Li 2 WO 4 was used as the lithium oxide and the ratio of the thickness of the lithium oxide layer to the average particle size of the spinel type active material was set to the value shown in Table 1.

[0087] [Comparative Example 1]

[0088] Using lithium nickel cobalt aluminum oxide (LiNi 0.82 Co 0.15 Al 0.03 O2) as the positive electrode active material, the solid electrolyte used in the positive electrode layer was changed to a sulfide solid electrolyte (Li2S-P2S5 glass ceramic containing LiI, with an average particle size of D 50 =0.8 μm), and the ratio of the thickness of the lithium oxide layer to the average particle size of the positive electrode active material was set to the value shown in Table 1. A composite positive electrode active material was prepared in the same manner as in Example 1. An evaluation battery was prepared in the same manner as in Example 1, using the obtained composite positive electrode active material.

[0089] [Comparative Example 2]

[0090] Using lithium nickel cobalt aluminum oxide (LiNi 0.82 Co 0.15 Al 0.03 O2) as the positive electrode active material, and the ratio of the thickness of the lithium oxide layer to the average particle size of the positive electrode active material was set to the value shown in Table 1, and a composite positive electrode active material was prepared in the same manner as in Example 1. Using the obtained composite positive electrode active material, an evaluation battery was prepared in the same manner as in Example 1, except that

[0091] [Comparative Example 3]

[0092] The solid electrolyte used in the positive electrode layer was changed to a sulfide solid electrolyte (Li2S-P2S5 glass ceramic containing LiI, with an average particle size of D 50 =0.8 μm), and except that the ratio of the thickness of the lithium oxide layer to the average particle size of the positive electrode active material was set to the value shown in Table 1, a composite positive electrode active material and an evaluation battery were prepared in the same manner as in Example 1.

[0093] [evaluate]

[0094] (Oxygen production)

[0095] The oxygen generation of each evaluation battery was evaluated by calculating the cumulative calorific value as follows. First, in a glove box filled with inert gas, the evaluation battery in the charged state was disassembled, and only the positive electrode layer was taken out and processed into a predetermined size. Then, differential scanning calorimetry (DSC) was performed at 10°C / min in a He atmosphere. The result after integrating the calorific value below 500°C was divided by the weight of the positive electrode active material in the positive electrode layer to obtain the cumulative calorific value. The results are shown in Table 1.

[0096] (Resistance increase rate)

[0097] For each evaluation battery produced, constant current-constant voltage charging and discharging were performed at a rate of 1 / 3C to confirm the capacity. Afterwards, the SOC was adjusted to 50% at a rate of 1 / 3C. Then, the AC impedance was measured at an applied voltage of 10mV and a measurement frequency range of 0.1 to 106Hz. The obtained Cole-Cole diagram was fitted with an arc, and the distance between the two points of intersection of the fitted arc and the real axis was taken as the reaction resistance (reaction resistance before the storage test). After the reaction resistance was measured, it was adjusted to SOC100% and stored in a constant temperature bath maintained at 60°C for 30 days. Then, it was adjusted to SOC50% again, and the reaction resistance (reaction resistance after the storage test) was measured in the same way, and the resistance change before and after the storage test was taken as the resistance increase rate. The results are shown in Table 1.

[0098] Table 1

[0099]

[0100] As shown in Table 1, in Examples 1 to 6, the calorific value (oxygen generation) of the positive electrode is small. On the other hand, according to the results of Comparative Examples 1 to 3, when the positive electrode layer contains only one of the composite positive electrode active material (composite positive electrode active material whose surface is covered with a lithium oxide layer) and the halide solid electrolyte, the calorific value of the positive electrode is reduced, but it is more than that of Examples 1 to 6. Therefore, it is confirmed that, as in the present invention, by combining a predetermined composite positive electrode active material and a halide solid electrolyte, the calorific value can be significantly reduced. In addition, from Examples 3 to 6, it is confirmed that if the average thickness of the lithium oxide layer is relative to the average particle size (D 50 ) is within a predetermined range, the heat generation can be further reduced and the resistance increase rate can be suppressed.

[0101] Here, as the reason for the low calorific value of the positive electrode in Examples 1 to 6, it is believed that the reaction between the positive electrode active material and the solid electrolyte is suppressed by the lithium oxide layer, the crystal structure of the spinel type active material is stable, and the reactivity of the halide solid electrolyte with oxygen is low. Furthermore, it is believed that the nickel cobalt aluminum oxide (rock salt layered active material) used in Comparative Examples 1 and 2 is an active material that easily releases oxygen. In addition, it is believed that in Comparative Example 3, in the area not covered by LiNbO3, Mn in the positive electrode active material reacts with S in the sulfide solid electrolyte, and the calorific value increases.

Claims

1. An all-solid-state battery comprising a positive electrode layer, a negative electrode layer, and a solid electrolyte layer formed between the positive electrode layer and the negative electrode layer, The positive electrode layer contains a composite positive electrode active material and a halide solid electrolyte. The composite positive electrode active material comprises a spinel-type active material and a lithium oxide layer covering the surface of the spinel-type active material. The halide solid electrolyte contains an element X as a main component of anions, wherein X is a halogen. The negative electrode layer contains Si-based negative electrode active material, The spinel active material has a composition of LiMe2O4, wherein: Me is Mn, or a combination of Mn and Ni, The lithium oxide is at least one of LiNbO3 and Li2WO4, The halide solid electrolyte has Li3YBr b Cl c , wherein b and c satisfy 0≤b≤6, 0≤c≤6 and b+c=6, The average thickness of the lithium oxide layer relative to the average particle size D of the spinel type active material 50 The ratio is 3.0% or more and 5% or less. 2 . The all-solid-state battery according to claim 1 , wherein both the negative electrode layer and the solid electrolyte layer contain a sulfide solid electrolyte.

3. According to the all-solid-state battery according to claim 1, the spinel active material is LiMn2O4, and the halide solid electrolyte is Li3YBr2Cl4.