A method for rotating tin spraying on four sides of PCB

By setting air knives in four directions of the PCB board and rotating and flattening, the problems of hot air impact and inhomogeneity in traditional tin spraying are solved, uniform processing of the board and orifice protection are achieved, and the product yield is improved .

CN114666999BActive Publication Date: 2024-11-29VICTORY GIANT TECH HUIZHOU CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111631235.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-29
Publication Date
2024-11-29
Estimated Expiration
2041-12-29

AI Technical Summary

Technical Problem

In the PCB surface treatment, traditional vertical tin injection and horizontal tin injection have problems such as large thermal shock in hot air leveling, resulting in deformation of the plate, uneven tin injection thickness and fracture of the copper layer on the orifice.

Method used

The PCB four-sided rotary tin spraying method is adopted. By setting the air knife in the upper, lower, left and right directions of the PCB board, and rotating at a speed of 20 turns/min during the hot air leveling process, the air knife in the four directions is used for synchronous flattening. Reduce the pressure and impact of a single-sided air knife to achieve uniform leveling.

Benefits of technology

It effectively avoids deformation of the board, improves the uniformity of tin, and prevents the orifice copper layer from breaking, improving product yield.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a PCB four-sided rotating tin spraying method, comprising the following steps, S1: pre-treatment, pre-treatment of the PCB board according to a conventional tin spraying process; S2: transfer of the PCB board, after the PCB board is pre-treated, it is transferred by a conveyor belt to the upper part of the tin furnace; S3: tin spraying treatment, after the PCB board is moved to the upper part of the tin furnace, the PCB board is clamped by a transfer mechanism and equipment, and the PCB board is quickly moved into the tin furnace for immersion, and then the PCB board is automatically lifted up by the transfer mechanism or equipment; S4: wind knife blowing treatment, after the PCB board is tinned and lifted up, the PCB board immersed in tin liquid is subjected to wind knife blowing treatment to level the surface, the four sides of the PCB board are all provided with wind knives, and four wind knives act on the four sides of the PCB board synchronously, and during the wind knife blowing treatment, the PCB board surface rotates at a speed of 20 revolutions / minute. The PCB four-sided rotating tin spraying method of the present invention has the advantages of not easy deformation of the plate, good tinning uniformity, high product yield, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of circuit board manufacturing, in particular to a PCB four-sided rotary tin spraying method. Background Art

[0002] In PCB surface treatment, since tin spraying has formed a layer of tin, its solderability performance is most beneficial compared to gold-plated boards, OSP boards, etc., so it also occupies a large share in the market. There are two ways of tin spraying: vertical tin spraying and horizontal tin spraying.

[0003] At present, the traditional vertical tin spraying and horizontal tin spraying mainly adopt the method of setting wind knives on the upper and lower sides of the PCB board to achieve leveling. During the wind knife blowing process, the wind knife blows from the upper and lower directions to the middle. The wind knife layout is relatively dense, and the impact on the board is relatively large during hot air leveling.

[0004] The vertical tin spraying method is used to spray tin on the PCB. The shear force of the vertical tin spraying at a 45-degree angle is large, which can easily lead to uneven tin spraying, and the orifice is easy to dissolve copper. The thermal shock of hot air leveling is large, which can easily cause the plate to deform and cause large warping thermal stress. Although horizontal tin spraying improves the uniformity of tin spraying to a certain extent, the impact force on the orifice is more direct and greater, which can easily cause the copper layer at the orifice to break.

[0005] Therefore, the current traditional vertical tin spraying and horizontal tin spraying have the following specific problems: 1. The thermal shock of hot air leveling is large, which can easily cause the plate to deform and cause large thermal stress; 2. The thickness of the surface tin spraying is uneven; 3. It is easy to cause the copper thickness of the hole to be too thin, especially when the loss of thin plate is more than 10 microns, which can easily cause the copper layer at the hole to break. Summary of the invention

[0006] To this end, the applicant provides a PCB four-sided rotating tin spraying method that is not easy to deform, has good tinning uniformity, and has a high product yield.

[0007] In order to achieve the above purpose, the following technical solutions are adopted.

[0008] A method for rotating tin spraying on four sides of a PCB, characterized in that it comprises the following steps:

[0009] S1: Pre-treatment, pre-treatment of PCB board according to conventional tin spraying process;

[0010] S2: The PCB board is transferred by the conveyor belt to the top of the tin furnace after the PCB board is pre-treated;

[0011] S3: tin spraying treatment. After the PCB is moved to the position above the tin furnace, the PCB is clamped by the transfer mechanism or equipment, and the PCB is quickly moved into the tin furnace for immersion, and then the PCB is automatically lifted up by the transfer mechanism or equipment;

[0012] S4: air knife blowing treatment. After the PCB board is dipped in tin and lifted up, the PCB board dipped in tin liquid is treated with air knife blowing to level the surface. Air knives are arranged on the upper, lower, left, and right sides of the PCB board. Four air knives act on the four sides of the PCB board synchronously. During the air knife blowing treatment, the PCB board surface rotates at a speed of 20 revolutions / minute.

[0013] Furthermore, in S3: the tin spraying treatment step, the operation time of moving the PCB board into the tin furnace for immersion and then taking it out is 2s to 4s.

[0014] Furthermore, in S3: the tin-spraying step, the temperature of the tin furnace is 270°C.

[0015] Furthermore, the air knife spacing is 4 mm.

[0016] As one of the preferred solutions of the present invention, the tin spraying treatment is horizontal tin spraying. After the conveyor belt transfers the PCB to the tin furnace, the PCB board is horizontally clamped by a transfer mechanism or equipment. When horizontal tin spraying is performed, the air knife pressure is 0.1MPa~0.3MPa on the upper plate surface and 0.2MPa~0.4MPa on the lower plate surface, and the upper plate surface pressure is less than the lower plate surface pressure.

[0017] Furthermore, during the air knife blowing process, the PCB surface rotates clockwise at a speed of 20 revolutions per minute.

[0018] Furthermore, the wind directions of the four wind knives on the four sides of the PCB board are all distributed perpendicularly to the board surface at 90 degrees.

[0019] As the second preferred solution of the present invention, the tin spraying treatment is vertical tin spraying. After the conveyor belt transfers the PCB to the tin furnace, the PCB board is vertically clamped by a transfer mechanism or equipment. When vertically spraying tin, the air knife pressure is the same for the upper and lower plate surfaces, and the air knife pressures on the upper and lower surfaces are both 0.1MPa to 0.3MPa.

[0020] Furthermore, during the air knife blowing process, the PCB surface rotates counterclockwise at a speed of 20 revolutions per minute.

[0021] Furthermore, the wind directions of the four wind knives on the four sides of the PCB board are all perpendicular to the board surface and inclined upward by 4 degrees.

[0022] Compared with the prior art, the PCB four-sided rotary tin spraying method of the present invention has the following beneficial effects:

[0023] First, the plate is not easy to deform. The present invention adopts the method of setting wind knives on the four sides of the PCB board, and the wind knives in four directions are used to blow the PCB board synchronously, so that under the same wind pressure or wind speed, the existing wind knives in the upper and lower directions are set in the upper and lower, left and right directions of the PCB board, which can effectively increase the wind knife spacing and reduce the wind knife pressure on one side of the PCB board, that is, reduce the impact of the single-sided wind knife on the PCB board, so that the plate is not easy to deform;

[0024] Second, the tinning uniformity is good. The present invention adopts the method of setting air knives on the four sides of the PCB board, and the air knives in four directions are used to blow the PCB board synchronously to perform hot air leveling on the PCB board. In the hot air leveling process, the PCB board surface rotates at a speed of 20 circles / minute. The four-sided rotation method is used to make the air knives in four directions blow the board surface multiple times with a small pressure to achieve uniform leveling, thereby effectively improving the tinning uniformity of the PCB board.

[0025] Third, the product yield is high. The present invention arranges wind knives on four sides of the PCB board, and the wind knives in four directions simultaneously blow the PCB board to perform hot air leveling on the PCB board. In the hot air leveling process, the PCB board surface rotates at a speed of 20 circles / minute. The four-sided rotation method is adopted to make the wind knives in four directions blow the board surface with a small pressure for multiple times to effectively protect the copper layer at the orifice from breaking. DETAILED DESCRIPTION

[0026] The PCB four-side rotary tin spraying method of the present invention will be further described in detail below in conjunction with specific embodiments.

[0027] Example 1

[0028] A method for rotating tin spraying on four sides of a PCB comprises the following steps:

[0029] S1: Pre-treatment, pre-treatment of PCB board according to conventional tin spraying process;

[0030] S2: The PCB board is transferred by the conveyor belt to the top of the tin furnace after the PCB board is pre-treated;

[0031] S3: Horizontal tin spraying treatment. After the PCB is moved to the position above the tin furnace, the PCB is clamped horizontally by the transfer mechanism and equipment, and the PCB is quickly moved into the 270°C tin furnace for immersion. The PCB is then automatically lifted up by the transfer mechanism or equipment. The entire process of this step takes 2s to 4s.

[0032] S4: air knife blowing treatment. After the PCB board is dipped in tin and lifted up, the PCB board dipped in tin liquid begins to be treated with air knife blowing to perform hot air flattening on the surface. At this time, the air knife pressure is 0.1MPa~0.3MPa on the upper surface, and 0.2MPa~0.4MPa on the lower surface. The upper surface pressure is less than the lower surface pressure. Specifically, air knives are arranged on the outside of the four surrounding surfaces of the PCB board. The four air knives act on the four surrounding surfaces of the PCB board synchronously. The wind directions of the four air knives on the four surrounding surfaces of the PCB board are all distributed vertically at 90 degrees to the board surface. The distance between the air knives is 4mm. During the air knife blowing treatment, the PCB board surface rotates clockwise at a speed of 20 revolutions / minute.

[0033] In this embodiment, the horizontal tin-spraying hot air leveling adopts the method of setting air knives on the four sides of the PCB board, and performing hot air leveling treatment on the PCB board from four directions: up, down, left and right. During this process, the upper board surface pressure is 0.1MPa-0.3MPa, and the lower board surface pressure is 0.2MPa-0.4MPa. On the one hand, compared with the traditional horizontal tin-spraying hot air leveling of the PCB board from top to bottom, the air knife ejection pressure is about half of the traditional horizontal tin-spraying air knife ejection pressure, and the ejection pressure is greatly reduced, which effectively reduces the pressure shock received by the PCB board during the hot air leveling process and avoids deformation of the board; in this embodiment, During the hot air leveling process, the overall air knife spray pressure of the upper board surface is smaller than the overall air knife spray pressure of the lower board surface. The inconsistent air knife pressures on the upper and lower surfaces of the PCB can effectively eliminate the influence of the earth's gravity. During the hot air leveling process, the PCB board surface rotates clockwise at a speed of 20 circles / minute. The four-sided rotation method is used to make the air knives in four directions blow the board surface with a small pressure for multiple times, which can achieve uniform leveling, thereby effectively improving the uniformity of tinning on the PCB board, and effectively preventing the orifice from dissolving copper too quickly due to excessive force, causing the copper layer at the orifice to break, thereby effectively protecting the orifice from breaking.

[0034] Example 2

[0035] A method for rotating tin spraying on four sides of a PCB comprises the following steps:

[0036] S1: Pre-treatment, pre-treatment of PCB board according to conventional tin spraying process;

[0037] S2: The PCB board is transferred by the conveyor belt to the top of the tin furnace after the PCB board is pre-treated;

[0038] S3: vertical tin spraying treatment. After the PCB is moved to the position above the tin furnace, the PCB is vertically clamped by the transfer mechanism and equipment, and the PCB is quickly moved into the 270°C tin furnace for immersion. The PCB is then automatically lifted up by the transfer mechanism or equipment. The entire process of this step takes 2s to 4s.

[0039] S4: air knife blowing treatment. After the PCB board is dipped in tin and lifted up, the PCB board dipped in tin liquid begins to be treated with air knife blowing to perform hot air flattening on the surface. At this time, the air knife pressure is the same for the upper and lower surfaces, and the air knife pressures on the upper and lower surfaces are both 0.1MPa to 0.3MPa. Specifically, air knives are arranged on the outside of the four surrounding surfaces of the PCB board, and four air knives act on the four surrounding surfaces of the PCB board synchronously. The wind directions of the four air knives on the four surrounding surfaces of the PCB board are all inclined 4 degrees upward perpendicular to the board surface, and the distance between the air knives is 4mm. During the air knife blowing treatment, the PCB board surface rotates counterclockwise at a speed of 20 revolutions / minute.

[0040] In this embodiment, the vertical tin spraying hot air leveling adopts the method of setting wind knives on the four sides of the PCB board, and performing hot air leveling treatment on the PCB board from four directions of top, bottom, left and right. In this process, the upper and lower board surface pressure is 0.1MPa~0.3MPa, which is relatively large compared with the traditional vertical tin spraying at a 45-degree angle, resulting in uneven tin spraying and easy copper dissolution at the hole. The pressure impact on the PCB board during the hot air leveling process is effectively reduced, the deformation of the board is avoided, and the internal copper is squeezed and broken due to short production time and high pressure in the prior art is effectively avoided. Crack; During the hot air leveling process, the PCB board surface rotates counterclockwise at a speed of 20 circles / minute. This four-sided rotation method is used to make the wind knives in four directions blow the board surface with a small pressure for multiple times, and each wind direction is cut vertically and upwardly at an angle of 4 degrees with the board surface, which can effectively eliminate the influence of the earth's gravity caused by vertical tin spraying, thereby achieving uniform leveling, effectively improving the uniformity of tinning of the PCB board, and effectively preventing the hole from being too fast due to excessive force. Dissolving copper causes the copper layer at the hole to break, thereby effectively protecting the hole from breaking.

Claims

1. A method for rotating tin spraying on four sides of a PCB, characterized in that: The following steps are included: S1: Pre-treatment, pre-treatment of PCB board according to conventional tin spraying process; S2: The PCB board is transferred by the conveyor belt to the top of the tin furnace after the PCB board is pre-treated; S3: tin spraying treatment. After the PCB is moved to the position above the tin furnace, the PCB is clamped by the transfer mechanism or equipment, and the PCB is quickly moved into the tin furnace for immersion, and then the PCB is automatically lifted up by the transfer mechanism or equipment; S4: air knife blowing treatment. After the PCB board is dipped in tin and lifted up, the PCB board dipped in tin liquid is treated with air knife blowing to level the surface. Air knives are arranged on the upper, lower, left, and right sides of the PCB board. Four air knives act on the four sides of the PCB board synchronously. During the air knife blowing treatment, the PCB board surface rotates at a speed of 20 revolutions / minute.

2. The PCB four-sided rotary tin spraying method according to claim 1, characterized in that: S3: In the tin spraying step, the operation time of moving the PCB board into the tin furnace for immersion and then taking it out is 2s to 4s.

3. The PCB four-sided rotary tin spraying method according to claim 2, characterized in that: S3: In the tin spraying treatment step, the tin furnace temperature is 270°C.

4. The PCB four-sided rotary tin spraying method according to claim 3, characterized in that: The air knife spacing is 4 mm.

5. The PCB four-sided rotary tin spraying method according to claim 4, characterized in that: The tin spraying process is horizontal tin spraying. After the conveyor belt transfers the PCB to the tin furnace, the PCB board is horizontally clamped by a transfer mechanism or equipment. When horizontal tin spraying, the air knife pressure is 0.1MPa~0.3MPa on the upper plate surface and 0.2MPa~0.4Mpa on the lower plate surface. The upper plate surface pressure is less than the lower plate surface pressure.

6. The PCB four-sided rotary tin spraying method according to claim 5, characterized in that: During the air knife blowing process, the PCB surface rotates clockwise at a speed of 20 revolutions per minute.

7. The PCB four-sided rotary tin spraying method according to claim 5, characterized in that: The wind directions of the four wind knives on the four sides of the PCB board are all distributed vertically at 90 degrees to the board surface.

8. The PCB four-sided rotary tin spraying method according to claim 4, characterized in that: The tin spraying process is vertical tin spraying. After the conveyor belt transfers the PCB to the tin furnace, the PCB board is vertically clamped by a transfer mechanism or equipment. When vertically spraying tin, the air knife pressure is the same for the upper and lower board surfaces, and the air knife pressures on both the upper and lower surfaces are 0.1MPa to 0.3MPa.

9. The PCB four-sided rotary tin spraying method according to claim 8, characterized in that: During the air knife blowing process, the PCB surface rotates counterclockwise at a speed of 20 revolutions per minute.

10. The PCB four-sided rotary tin spraying method according to claim 8, characterized in that: The wind directions of the four wind knives on the four sides of the PCB board are all perpendicular to the board surface and inclined upward by 4 degrees.

Citation Information

Patent Citations

  • Hot air levelling machine for processing circuit board

    CN101697665A

  • Antioxidation treatment method for PCB (Printed Circuit Board)

    CN113347803A