A polyolefin composite diaphragm for lithium ion battery with good thermal stability and preparation method thereof, and lithium ion battery
By using a composite coating of porous inorganic materials and polyacrylonitrile colloids on the lithium-ion battery separator, the problems of separator thermal stability and capacity retention are solved, and the safety and electrochemical performance of lithium-ion batteries are improved.
Patent Information
- Application Number
- CN202011590025.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-12-29
AI Technical Summary
The separator of existing lithium-ion batteries has poor thermal stability, which can easily lead to combustion and explosion, and has a low capacity retention rate, which affects battery safety performance and rate performance.
Using polyolefin composite separator, the microscopic morphology of the stacking arrangement of porous inorganic material particles on the polyolefin base film and the addition of polyacrylonitrile colloids into their holes is formed to form a specific composite material coating to enhance the thermal stability of the separator. and conductivity.
It significantly improves the safety performance and electrochemical performance of lithium-ion batteries, reduces pinholes and microcrack defects, improves capacity retention and ionic conductivity, and reduces battery self-discharge. It has a simple process and low cost, which is suitable for large-scale production.
Smart Images

Figure BDA0002868678420000031 
Figure BDA0002868678420000071 
Figure BDA0002868678420000081
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-ion battery diaphragm materials, and relates to a polyolefin composite diaphragm and a preparation method thereof, and a lithium-ion battery, and in particular to a polyolefin composite diaphragm for a lithium-ion battery with good thermal stability and a preparation method thereof, and a lithium-ion battery. Background Art
[0002] As the core component of pure electric new energy vehicles, lithium-ion battery safety issues have become one of the key indicators that restrict its further development. In addition to battery pack design defects, abuse during use and external environmental impact, the causes of lithium-ion battery safety accidents are mainly related to the composition, design and manufacturing process of the single battery, among which the influence of battery composition on safety performance is particularly critical. As one of the four main materials of lithium-ion batteries, the diaphragm has an important influence on the comprehensive performance of lithium-ion batteries. The diaphragm is located between the positive and negative electrodes and plays a role in preventing battery short circuits and providing electrolyte ion channels. Studies on the kinetic mechanism of thermal runaway reactions of lithium-ion batteries have found that the entire process can be divided into three stages: (1) Internal thermal runaway stage of the battery. Due to heating, short circuit and other reasons, the internal temperature of the battery rises to about 100°C, the anode SEI film begins to decompose, and the lithium embedded in the graphite reacts with the electrolyte, further pushing up the internal temperature of the battery. (2) Battery swelling process. When the battery temperature rises to 200°C, the cathode material decomposes, releasing a large amount of heat and gas, and the lithium-embedded anode at 250-350°C begins to react with the electrolyte. (3) Thermal runaway of the battery as a whole. In this stage, as the internal pressure of the lithium-ion battery rises sharply, the outer packaging of the battery is broken, and the external oxygen, electrolyte vapor, and combustible smoke / combustible smoke generated by various reactions react with each other, and then burn and catch fire, resulting in thermal runaway of the lithium-ion battery as a whole. The diaphragm is an important component of the battery. The performance of the diaphragm will affect the key indicators of the lithium-ion battery such as capacity cycle performance and charge and discharge performance, and can also prevent the battery from short circuiting. Since lithium-ion batteries can catch fire and explode, which greatly threatens personal and property safety, their large-scale application in the field of electric vehicles and energy storage has been greatly hindered. The better the stability of the diaphragm, the lower the thermal shrinkage rate after heating, which can avoid battery combustion and explosion and improve the safety performance of the battery.
[0003] Therefore, improving the stability and safety of the diaphragm and improving the capacity retention rate are the key areas of current research. The importance of the diaphragm in lithium battery components is increasing, and its impact on lithium batteries is also receiving increasing attention. The key indicators that affect the performance of the diaphragm include thickness, air permeability, porosity, closed-cell temperature, thermal stability, wettability, tensile strength and puncture strength. The diaphragm material is mostly made of polyolefin materials to form a polymer porous film, including polypropylene microporous film (PP), polyethylene microporous film (PE), polypropylene / polyethylene (PP / PE) composite film, polypropylene / polyethylene / polypropylene (PP / PE / PP) composite film, etc. Due to material limitations, the thickness of the diaphragm is relatively low, there are many defects such as pinholes and microcracks, and the thermal stability is not good. For safety performance considerations, the current process is mostly focused on coating the surface of polyolefin diaphragms with ceramic functional coatings to enhance the thermal stability of the diaphragm. For example, inorganic ceramic materials such as alumina and boehmite are usually coated to improve the thermal stability and electrolyte wettability of the diaphragm. Although the use of ceramic coating can compensate for the defects caused by the thinning of the diaphragm thickness to a certain extent, the problems such as poor closed-cell performance and many pinhole / microcrack defects are still difficult to solve, and the steps are cumbersome and the cost is high. At the same time, the rate performance and capacity retention rate of lithium-ion batteries cannot be improved.
[0004] Therefore, how to find a suitable method to solve the above-mentioned problems existing in the existing diaphragms while ensuring that the comprehensive performance of the product is not affected has become one of the key technical issues that need to be urgently solved in the industry. Summary of the invention
[0005] In view of this, the technical problem to be solved by the present invention is to provide a polyolefin composite diaphragm and a preparation method thereof, and a lithium-ion battery, in particular, a polyolefin composite diaphragm with good thermal stability. The polyolefin composite diaphragm provided by the present invention can effectively enhance the thermal stability of polyolefin diaphragms, reduce defects such as pinholes and microcracks of polyolefin diaphragms, improve the safety performance of lithium-ion batteries, and also improve ionic conductivity and saturated liquid volume.
[0006] The present invention provides a polyolefin composite diaphragm, comprising a polyolefin base film;
[0007] A composite material coating laminated on at least one side of a polyolefin-based film;
[0008] The composite material coating has a microscopic morphology of stacked and arranged porous inorganic material particles;
[0009] Polyacrylonitrile colloid is compounded in the pores of the porous inorganic material particles.
[0010] Preferably, the porous inorganic material particles are evenly distributed on the surface of the polyolefin-based membrane;
[0011] The polyacrylonitrile colloid is compounded on the surface of the porous inorganic material particles;
[0012] The base film comprises a polyethylene base film and / or a polypropylene base film;
[0013] The polyolefin-based membrane is a microporous membrane.
[0014] Preferably, the polyacrylonitrile colloid comprises polyacrylonitrile colloid particles;
[0015] The porous inorganic material includes one or more of alumina, aluminum hydroxide, silicon dioxide, bentonite, expanded graphite, zeolite, diatomaceous earth, vermiculite, perlite and clay;
[0016] The particle size of the porous inorganic material particles is 0.3 to 1.5 μm;
[0017] The molecular weight of the polyacrylonitrile colloid is 1000-10000.
[0018] Preferably, the median pore size of the polyolefin base membrane is 10 to 100 nm;
[0019] The thickness of the polyolefin base film is 5 to 25 μm;
[0020] The thickness of the composite material coating is 0.5 to 3 μm;
[0021] The composite material coating is compounded on the polyolefin base film by mixed slurry.
[0022] Preferably, the mixed slurry, measured by percentage by mass of raw materials, comprises:
[0023]
[0024] Preferably, the porous inorganic material comprises one or more of alumina, aluminum hydroxide, silicon dioxide, bentonite, expanded graphite, zeolite, diatomaceous earth, vermiculite, perlite and clay;
[0025] The adhesive includes one or more of phenyl acrylic acid, polyacrylamide, polyvinyl alcohol, polyethylene oxide, modified paraffin resin, polyacrylate adhesive, polyurethane acrylate and polyacrylate copolymer emulsion;
[0026] The wetting agent includes one or more of alkyl sulfates, sulfonates, fatty acids or fatty acid ester sulfates, carboxylic acid soaps, phosphates, polyoxyethylene alkylphenol ethers, polyoxyethylene fatty alcohol ethers and polyoxyethylene polyoxypropylene block copolymers.
[0027] Preferably, the polyolefin-based film is prepared by a wet process;
[0028] The other side of the polyolefin-based film may also be compounded with other organic functional coatings.
[0029] The present invention provides a method for preparing a polyolefin composite diaphragm, comprising the following steps:
[0030] 1) ultrasonically mixing acrylonitrile monomer, porous inorganic filler and poly(ethylene-vinyl acetate), and then adding benzoyl peroxide to react to obtain a polyacrylonitrile / porous inorganic material composite material;
[0031] 2) mixing the composite material, adhesive, wetting agent and water obtained in the above steps by high-speed stirring to obtain a mixed slurry;
[0032] 3) The mixed slurry obtained in the above steps is evenly coated on the polyolefin base film, and after drying, a polyolefin composite diaphragm is obtained.
[0033] Preferably, the coating method includes one or more of spray coating, gravure coating, narrow slit coating and wet coating;
[0034] The high-speed stirring and mixing time is 30 to 120 minutes;
[0035] The rotation speed of the high-speed stirring and mixing is 600-2000 r / min;
[0036] The thickness of the mixed slurry coating is 1 to 3 μm;
[0037] The drying temperature is 40-80°C.
[0038] The present invention also provides a lithium ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte;
[0039] The diaphragm includes the polyolefin composite diaphragm described in any one of the above technical solutions or the polyolefin composite diaphragm prepared by the preparation method described in any one of the above technical solutions.
[0040] The present invention provides a polyolefin composite diaphragm, including a polyolefin base film; a composite material coating compounded on at least one side of the polyolefin base film; the composite material coating has a microscopic morphology of stacked and arranged porous inorganic material particles; and polyacrylonitrile colloid is compounded in the pores of the porous inorganic material particles. Compared with the prior art, the present invention is aimed at the existing lithium-ion battery diaphragm. As the thickness of the diaphragm decreases, the negative impact of other properties of the diaphragm increases, and the thermal stability is not good. The technical solution of the ceramic coating still has problems such as poor closed-cell performance, many pinhole / microcrack defects, and the steps are cumbersome, the cost is high, and the scale feasibility is low. In addition, the present invention is also aimed at similar methods using polyolefins and inorganic fillers in the art. Although the diaphragm can be closed at low temperatures, the modified diaphragm still has poor stability. Although the coating is uniform, it is easy to block the pores of the polyolefin diaphragm itself, thereby affecting the transmission efficiency of lithium ions and increasing the internal resistance of the lithium-ion battery.
[0041] The present invention provides a polyolefin composite diaphragm, which creatively adopts a composite material coating with a specific composition and morphology. The functional coating has good compatibility with the polyolefin base film, utilizes a specific composite form of inorganic porous filler and polyacrylonitrile colloid, and has a specific stacked morphology. Polyacrylonitrile can expand at low temperatures, increase in volume, and hinder the passage of ions. The colloidal particles have strong polarity, which can significantly improve the ability to absorb and retain liquid. The porous inorganic filler can significantly improve the stability and capacity retention rate of the diaphragm, thereby improving the rate performance of the battery. Further, the stacked morphology has gaps, which will not affect the transmission efficiency of lithium ions, avoid the problem of increasing the internal resistance of the lithium ion battery, and can also achieve a low-temperature closed-cell function. The present invention can achieve a low-temperature closed-cell function, and can also effectively improve the thermal stability of polyolefin diaphragms, reduce defects such as pinholes and microcracks of polyolefin diaphragms, and improve the safety performance of lithium ion batteries; it can also effectively solve the problem that the existing diaphragms make the capacity retention rate of lithium ion batteries low, and improve the ionic conductivity and saturated liquid volume.
[0042] In the polyolefin composite diaphragm provided by the present invention, polyacrylonitrile can improve the liquid absorption and liquid retention capacity, and the porous inorganic filler can improve the thermal stability of the diaphragm and the battery capacity retention rate, thereby effectively enhancing the stability of the diaphragm, and at the same time making it have good liquid absorption and liquid retention capacity for the electrolyte solution, improving the liquid retention capacity and ionic conductivity, and more effectively reducing the defects such as pinholes and microcracks of the polyolefin diaphragm, reducing the battery self-discharge, and improving the battery use efficiency. The preparation process provided by the present invention is simple, convenient to coat, low in cost, high in efficiency of coating the diaphragm, and high in yield. It is easy to mass-produce, has good compatibility with the polyolefin base film, and significantly improves the overall performance of the battery.
[0043] The experimental results show that the polyolefin separator with high thermal stability provided by the present invention can significantly improve the safety performance and electrochemical performance of lithium-ion batteries. At the same time, the functional coating can effectively reduce defects such as microcracks and pores in the polyolefin separator, and can significantly improve the cycle performance and rate performance of lithium-ion batteries. The process is simple, the cost is low, and it has high practicality. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 This is a SEM scanning electron microscope image of the polyolefin composite diaphragm prepared in the present invention. DETAILED DESCRIPTION
[0045] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention.
[0046] All raw materials of the present invention are not particularly limited in their sources and can be purchased from the market or prepared according to conventional methods well known to those skilled in the art.
[0047] There is no particular restriction on the purity of all raw materials in the present invention. The present invention preferably uses analytically pure materials or materials of conventional purity used in the field of lithium ion battery separator preparation.
[0048] The present invention provides a polyolefin composite diaphragm, comprising a polyolefin base film;
[0049] A composite material coating laminated on at least one side of a polyolefin-based film;
[0050] The composite material coating has a microscopic morphology of stacked and arranged porous inorganic material particles;
[0051] Polyacrylonitrile colloid is compounded in the pores of the porous inorganic material particles.
[0052] In the present invention, the composite material coating has a microscopic morphology of stacked and arranged porous inorganic material particles, and polyacrylonitrile colloidal particles are compounded in the pores of the porous inorganic material particles. Compared with the existing uniform and dense arrangement, which affects the lithium ion transmission efficiency and increases the internal resistance of the battery, the stacked morphology has tiny gaps, which is conducive to lithium ion transmission, thereby avoiding affecting its transmission efficiency, and thus has little effect on the internal resistance of the lithium ion battery, and can achieve low-temperature closed-cell function. The colloidal particles dispersed in the pores of the porous inorganic material particles can improve the liquid absorption and liquid retention capabilities. At the same time, the stacked structure has a certain self-aggregation effect on the base film defects.
[0053] In the present invention, the porous inorganic material particles are preferably evenly distributed on the surface of the polyolefin base film. The pores of the porous inorganic material particles are compounded with polyacrylonitrile colloid. The present invention adopts in-situ polymerization, so that the polyacrylonitrile colloid is polymerized in the pores of the porous inorganic material. In the present invention, the polyacrylonitrile colloid compounded in the pores of the porous inorganic material particles preferably includes polyacrylonitrile colloid particles. Further, the polyacrylonitrile colloid is also preferably compounded on the surface of the porous inorganic material particles.
[0054] In principle, the present invention has no particular restrictions on the type of the polyolefin base film, and those skilled in the art can select and adjust it according to actual application conditions, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of polyolefin-based diaphragms, reduce the defects of polyolefin-based diaphragms themselves, and better improve the safety performance, ionic conductivity and saturated liquid volume of lithium-ion batteries, the base film preferably includes a polyethylene base film and / or a polypropylene base film, and is more preferably a polyethylene base film or a polypropylene base film.
[0055] In principle, the present invention has no particular restrictions on the selection of the polyolefin-based membrane. Those skilled in the art can select and adjust according to actual application conditions, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of polyolefin-based membranes, reduce the defects of polyolefin-based membranes themselves, and better improve the safety performance, ionic conductivity and saturated liquid volume of lithium-ion batteries, the polyolefin-based membrane preferably includes a microporous membrane. Further, the median pore size of the polyolefin-based membrane is preferably 10 to 100 nm, more preferably 10 to 80 nm, more preferably 25 to 60 nm, and more preferably 30 to 50 nm.
[0056] In principle, the present invention has no particular restriction on the thickness of the polyolefin base film. Those skilled in the art can select and adjust it according to the actual application conditions, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of the polyolefin separator, reduce the defects of the polyolefin separator itself, and better improve the safety performance, ionic conductivity and saturated liquid volume of lithium-ion batteries, the thickness of the polyolefin base film is preferably 5 to 25 μm, more preferably 6 to 20 μm, and more preferably 7 to 16 μm.
[0057] In principle, the present invention has no particular restriction on the selection of the porous inorganic material. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of the polyolefin separator, reduce the defects of the polyolefin separator itself, and better improve the safety performance, ionic conductivity and saturated liquid volume of the lithium-ion battery, the porous inorganic material preferably includes one or more of aluminum oxide, aluminum hydroxide, silicon dioxide, bentonite, expanded graphite, zeolite, diatomaceous earth, vermiculite, perlite and clay, and more preferably aluminum oxide, aluminum hydroxide, silicon dioxide, bentonite, expanded graphite, zeolite, diatomaceous earth, vermiculite, perlite or clay.
[0058] In principle, the present invention has no particular restriction on the particle size of the porous inorganic material particles. Those skilled in the art can select and adjust according to actual application conditions, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of polyolefin-type diaphragms, reduce the defects of polyolefin-type diaphragms themselves, and better improve the safety performance, ionic conductivity and saturated liquid volume of lithium-ion batteries, the particle size of the porous inorganic material particles is preferably 0.3-1.5 μm, more preferably 0.5-1.3 μm, and more preferably 0.7-1.1 μm.
[0059] In principle, the present invention has no particular limitation on the molecular weight of the polyacrylonitrile colloid, and those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of the polyolefin separator, reduce the defects of the polyolefin separator itself, and better improve the safety performance, ionic conductivity and saturated liquid volume of the lithium-ion battery, the molecular weight of the polyacrylonitrile colloid is preferably 1000-10000, more preferably 3000-8000, and more preferably 5000-6000.
[0060] In principle, the present invention has no particular restriction on the thickness of the composite material coating. Those skilled in the art can select and adjust it according to the actual application conditions, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of the polyolefin diaphragm, reduce the defects of the polyolefin diaphragm itself, and better improve the safety performance, ionic conductivity and saturated liquid volume of the lithium-ion battery, the thickness of the composite material coating is preferably 0.5 to 3 μm, more preferably 1 to 2.5 μm, and more preferably 1.5 to 2 μm.
[0061] The present invention completes and refines the overall preparation process, better improves the low-temperature closed-cell effect, enhances the thermal stability of polyolefin separators, reduces the defects of polyolefin separators themselves, and better improves the safety performance, ionic conductivity and saturated liquid volume of lithium-ion batteries. The composite material coating is preferably composited on the polyolefin base film by a mixed slurry.
[0062] In principle, the present invention has no particular limitation on the specific composition of the mixed slurry. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of the polyolefin separator, reduce the defects of the polyolefin separator itself, and better improve the safety performance, ion conductivity and saturated liquid volume of the lithium-ion battery, the mixed slurry, calculated by the mass percentage of the raw materials, preferably includes:
[0063]
[0064]
[0065] The amount of the polyacrylonitrile / porous inorganic material composite material added is preferably 30 to 75 parts by weight, more preferably 40 to 65 parts by weight, and more preferably 50 to 55 parts by weight. More specifically, the amount of the polyacrylonitrile is preferably 10 to 35 parts by weight, more preferably 15 to 30 parts by weight, and more preferably 20 to 25 parts by weight. In the present invention, the amount of polyacrylonitrile added is calculated based on the amount of polyacrylonitrile obtained after the acrylonitrile monomer is polymerized alone. The amount of the porous inorganic material is preferably 20 to 40 parts by weight, more preferably 22 to 38 parts by weight, more preferably 25 to 35 parts by weight, and more preferably 28 to 32 parts by weight.
[0066] In principle, the present invention has no particular restriction on the selection of the porous inorganic material. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of the polyolefin separator, reduce the defects of the polyolefin separator itself, and better improve the safety performance, ionic conductivity and saturated liquid volume of the lithium-ion battery, the porous inorganic material preferably includes one or more of aluminum oxide, aluminum hydroxide, silicon dioxide, bentonite, expanded graphite, zeolite, diatomaceous earth, vermiculite, perlite and clay, and more preferably aluminum oxide, aluminum hydroxide, silicon dioxide, bentonite, expanded graphite, zeolite, diatomaceous earth, vermiculite, perlite or clay.
[0067] The amount of water added in the present invention is preferably 25 to 70 parts by weight, more preferably 35 to 60 parts by weight, and more preferably 45 to 50 parts by weight.
[0068] The amount of the adhesive added in the present invention is preferably 1 to 5 parts by weight, more preferably 1.5 to 4.5 parts by weight, more preferably 2 to 4 parts by weight, and more preferably 2.5 to 3.5 parts by weight. In principle, the present invention has no particular restrictions on the selection of the adhesive, and those skilled in the art can select and adjust according to actual application conditions, product requirements and quality requirements. The present invention is to better improve the low-temperature closed-cell effect, enhance the thermal stability of polyolefin separators, reduce the defects of polyolefin separators themselves, and better improve the safety performance, ionic conductivity and saturated liquid volume of lithium-ion batteries. The adhesive preferably includes one or more of phenylacrylic acid, polyacrylamide, polyvinyl alcohol, polyethylene oxide, modified paraffin resin, polyacrylate adhesive, polyurethane acrylate and polyacrylate copolymer emulsion, and more preferably phenylacrylic acid, polyacrylamide, polyvinyl alcohol, polyethylene oxide, modified paraffin resin, polyacrylate adhesive, polyurethane acrylate or polyacrylate copolymer emulsion.
[0069] The amount of the wetting agent added in the present invention is preferably 0.1 to 1 parts by weight, more preferably 0.3 to 0.8 parts by weight, and more preferably 0.5 to 0.6 parts by weight. In principle, the present invention has no particular restrictions on the selection of the wetting agent, and those skilled in the art can select and adjust according to actual application conditions, product requirements and quality requirements. The present invention is to better improve the low-temperature closed-cell effect, enhance the thermal stability of polyolefin separators, reduce the defects of polyolefin separators themselves, and better improve the safety performance, ionic conductivity and saturated liquid volume of lithium-ion batteries. The wetting agent preferably includes alkyl sulfates, sulfonates, fatty acids or fatty acid ester sulfates, carboxylic acid soaps, phosphates, polyoxyethylene alkylphenol ethers, polyoxyethylene fatty alcohol ethers and polyoxyethylene polyoxypropylene block copolymers. One or more, more preferably alkyl sulfates, sulfonates, fatty acids or fatty acid ester sulfates, carboxylic acid soaps, phosphates, polyoxyethylene alkylphenol ethers, polyoxyethylene fatty alcohol ethers or polyoxyethylene polyoxypropylene block copolymers.
[0070] The present invention completes and refines the overall preparation process, better improves the low-temperature closed-cell effect, enhances the thermal stability of the polyolefin diaphragm, reduces the defects of the polyolefin diaphragm itself, and better improves the safety performance, ionic conductivity and saturated liquid volume of the lithium-ion battery. The polyolefin-based membrane is preferably prepared by a wet process.
[0071] The present invention completes and refines the overall preparation process, better improves the low-temperature closed-cell effect, enhances the thermal stability of the polyolefin separator, reduces the defects of the polyolefin separator itself, and better improves the safety performance, ionic conductivity and saturated liquid volume of the lithium-ion battery. The other side of the polyolefin-based film can preferably be composited with other organic functional coatings.
[0072] The present invention provides a method for preparing a polyolefin composite diaphragm, comprising the following steps:
[0073] 1) ultrasonically mixing acrylonitrile monomer, porous inorganic filler and poly(ethylene-vinyl acetate), and then adding benzoyl peroxide to react to obtain a polyacrylonitrile / porous inorganic material composite material;
[0074] 2) mixing the composite material, adhesive, wetting agent and water obtained in the above steps by high-speed stirring to obtain a mixed slurry;
[0075] 3) The mixed slurry obtained in the above steps is evenly coated on the polyolefin base film, and after drying, a polyolefin composite diaphragm is obtained.
[0076] The structure, composition and parameters of the raw materials involved in the preparation method of the present invention, as well as the corresponding preferred principles, can correspond to the structure, composition and parameters of the materials in the aforementioned polyolefin composite diaphragm, as well as the corresponding preferred principles, and will not be elaborated here one by one.
[0077] The invention firstly mixes acrylonitrile monomer, porous inorganic filler and poly(ethylene-vinyl acetate) by ultrasonic mixing, then adds benzoyl peroxide to react, and obtains a polyacrylonitrile / porous inorganic material composite material.
[0078] In principle, the present invention has no particular restrictions on the parameters of the reaction, and those skilled in the art can select and adjust them according to actual application conditions, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of polyolefin separators, reduce the defects of polyolefin separators themselves, and better improve the safety performance, ionic conductivity and saturated liquid volume of lithium-ion batteries, the temperature of the reaction is preferably 75 to 85°C, more preferably 77 to 83°C, and more preferably 79 to 81°C. The reaction (polymerization reaction) time is 15 to 30 hours, more preferably 18 to 28 hours, and more preferably 20 to 25 hours.
[0079] In the present invention, the composite material obtained in the above steps, the adhesive, the wetting agent and the water are mixed by high-speed stirring to obtain a mixed slurry.
[0080] In principle, the present invention has no particular restriction on the time of the high-speed stirring and mixing. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of the polyolefin diaphragm, reduce the defects of the polyolefin diaphragm itself, and better improve the safety performance, ionic conductivity and saturated liquid volume of the lithium-ion battery, the time of the high-speed stirring and mixing is preferably 30 to 120 minutes, more preferably 50 to 100 minutes, and more preferably 70 to 80 minutes.
[0081] In principle, the present invention has no particular restriction on the rotation speed of the high-speed stirring and mixing. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of the polyolefin diaphragm, reduce the defects of the polyolefin diaphragm itself, and better improve the safety performance, ionic conductivity and saturated liquid volume of the lithium-ion battery, the rotation speed of the high-speed stirring and mixing is preferably 600-2000r / min, more preferably 900-1700r / min, and more preferably 1200-1500r / min.
[0082] Finally, the mixed slurry is evenly coated on the polyolefin base film, and after drying, a polyolefin composite diaphragm is obtained.
[0083] In principle, the present invention has no particular limitation on the coating method, and those skilled in the art can select and adjust it according to the actual application conditions, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of polyolefin separators, reduce the defects of polyolefin separators themselves, and better improve the safety performance, ionic conductivity and saturated liquid volume of lithium-ion batteries, the coating method preferably includes one or more of spray coating, gravure coating, narrow slit coating and wet coating, and more preferably spray coating, gravure coating, narrow slit coating or wet coating.
[0084] In principle, the present invention has no particular restriction on the thickness of the mixed slurry coating. Those skilled in the art can select and adjust it according to the actual application conditions, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of the polyolefin diaphragm, reduce the defects of the polyolefin diaphragm itself, and better improve the safety performance, ionic conductivity and saturated liquid volume of the lithium-ion battery, the thickness of the mixed slurry coating is preferably 1-3 μm, more preferably 1.4-2.6 μm, and more preferably 1.8-2.2 μm.
[0085] In principle, the present invention has no particular limitation on the drying temperature, and those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. In order to better improve the low-temperature closed-cell effect, enhance the thermal stability of the polyolefin diaphragm, reduce the defects of the polyolefin diaphragm itself, and better improve the safety performance, ionic conductivity and saturated liquid volume of the lithium-ion battery, the drying temperature is preferably 40-80°C, more preferably 45-75°C, more preferably 50-70°C, and more preferably 55-65°C.
[0086] The present invention provides a lithium ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte;
[0087] The diaphragm includes the polyolefin composite diaphragm described in any one of the above technical solutions or the polyolefin composite diaphragm prepared by the preparation method described in any one of the above technical solutions.
[0088] The above steps of the present invention provide a polyolefin composite diaphragm for lithium ion batteries with good thermal stability, a preparation method thereof, and a lithium ion battery. The polyolefin composite diaphragm adopts a composite material coating with a specific composition and morphology. The functional coating has good compatibility with the polyolefin base film. Through in-situ polymerization, a specific composite form of inorganic porous filler and polyacrylonitrile colloid is obtained, and the composite material has a specific stacked morphology. Polyacrylonitrile can expand at low temperatures, increase in volume, and hinder the passage of ions. The colloidal particles have strong polarity and can significantly improve the ability to absorb and retain liquid. The porous inorganic filler can significantly improve the stability and capacity retention rate of the diaphragm, thereby improving the rate performance of the battery. Further, the stacked morphology has gaps, which will not affect the transmission efficiency of lithium ions and avoid the problem of increasing the internal resistance of the lithium ion battery. The present invention can achieve the low-temperature closed-cell function, and can also effectively improve the thermal stability of polyolefin diaphragms, reduce defects such as pinholes and microcracks of polyolefin diaphragms, and improve the safety performance of lithium ion batteries; it can also effectively solve the problem that the existing diaphragm makes the capacity retention rate of lithium ion batteries low, and improve the ionic conductivity and saturated liquid volume.
[0089] In the polyolefin composite diaphragm provided by the present invention, polyacrylonitrile can improve the liquid absorption and liquid retention capacity, and the porous inorganic filler can improve the thermal stability of the diaphragm and the battery capacity retention rate, thereby effectively enhancing the stability of the diaphragm, and at the same time making it have good liquid absorption and liquid retention capacity for the electrolyte solution, improving the liquid retention capacity and ionic conductivity, and more effectively reducing the defects such as pinholes and microcracks of the polyolefin diaphragm, reducing the battery self-discharge, and improving the battery use efficiency. The preparation process provided by the present invention is simple, convenient to coat, low in cost, high in efficiency of coating the diaphragm, and high in yield. It is easy to mass-produce, has good compatibility with the polyolefin base film, and significantly improves the overall performance of the battery.
[0090] The experimental results show that the polyolefin separator with high thermal stability provided by the present invention can significantly improve the safety performance and electrochemical performance of lithium-ion batteries. At the same time, the functional coating can effectively reduce defects such as microcracks and pores in the polyolefin separator, and can significantly improve the cycle performance and rate performance of lithium-ion batteries. The process is simple, the cost is low, and it has high practicality.
[0091] In order to further illustrate the present invention, a polyolefin composite diaphragm and a preparation method thereof, and a lithium-ion battery provided by the present invention are described in detail below in combination with embodiments. However, it should be understood that these embodiments are implemented on the premise of the technical scheme of the present invention, and detailed implementation methods and specific operating processes are given only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention. The protection scope of the present invention is not limited to the following embodiments.
[0092] Example 1
[0093] 1) After ultrasonically mixing acrylonitrile monomer, alumina and poly(ethylene-vinyl acetate) for 10 minutes, the temperature was raised to 80° C., benzoyl peroxide was added dropwise and the temperature was raised to carry out in-situ polymerization reaction for 15 hours to obtain a polyacrylonitrile / porous inorganic material composite material; wherein the amount of polyacrylonitrile (calculated amount) and alumina was 1:1.
[0094] 2) The composite material, polymethyl acrylate, polyoxyethylene polyoxypropylene and deionized water in a mass ratio of 30:3:1:66 are mixed and stirred at high speed to obtain a mixed slurry.
[0095] 3) The mixed slurry was coated on the polyethylene diaphragm by spray coating, and the coating thickness was controlled at 1 μm to obtain a mixed slurry composite polyethylene diaphragm, which was placed in a vacuum oven at 60° C. for 12 h to obtain a finished composite diaphragm.
[0096] The performance of the polyolefin composite diaphragm prepared in Example 1 of the present invention was tested.
[0097] 4) The prepared diaphragm was assembled and tested for 2Ah soft-pack square battery, with the positive electrode being nickel-cobalt-manganese (NCM523) and the negative electrode being graphite, and then the rate performance and impedance tests were performed at 25°C and 1C;
[0098] 5) The prepared diaphragm was placed in a vacuum oven for high temperature treatment at a temperature of 100° C. for 15 min, and then the shrinkage rate of the diaphragm was tested.
[0099] Example 2
[0100] 1) After ultrasonically mixing acrylonitrile monomer, zirconium oxide, silicon dioxide and poly(ethylene-vinyl acetate) for 10 minutes, the temperature was raised to 80°C, benzoyl peroxide was added dropwise and the temperature was raised to carry out in-situ polymerization for 15 hours to obtain a polyacrylonitrile / porous inorganic material composite material; wherein the amount of polyacrylonitrile (calculated amount) and (zirconia and silicon dioxide) was 2:3.
[0101] 2) The composite material, polymethyl acrylate, polyoxyethylene polyoxypropylene and deionized water in a mass ratio of 50:3:1:46 are mixed and stirred at high speed to obtain a mixed slurry.
[0102] 3) The mixed slurry was coated on the polyethylene diaphragm by spray coating, and the coating thickness was controlled at 1 μm to obtain a mixed slurry composite polyethylene diaphragm, which was placed in a vacuum oven at 60° C. for 12 h to obtain a finished composite diaphragm.
[0103] The polyolefin composite diaphragm prepared by the present invention is characterized.
[0104] See also Figure 1 , Figure 1 This is a SEM scanning electron microscope image of the polyolefin composite diaphragm prepared in the present invention.
[0105] Depend on Figure 1 It can be seen that the composite material coating presents a microscopic morphology of obvious stacked arrangement of porous inorganic material particles with stacked voids. The porous inorganic material particles are evenly dispersed and compounded on the base membrane. The polyacrylonitrile colloid particles are dispersed in the pores of the porous inorganic material particles, and polyacrylonitrile colloid may also be partially compounded on the surface of some porous inorganic material particles.
[0106] The performance of the polyolefin composite diaphragm prepared in Example 2 of the present invention was tested.
[0107] 4) The prepared diaphragm was assembled and tested for 2Ah soft-pack square battery, with the positive electrode being nickel-cobalt-manganese (NCM523) and the negative electrode being graphite, and then the rate performance and impedance tests were performed at 25°C and 1C;
[0108] 5) The prepared diaphragm was placed in a vacuum oven for high temperature treatment at a temperature of 110° C. for 15 min, and then the shrinkage rate of the diaphragm was tested.
[0109] Example 3
[0110] 1) After ultrasonically mixing acrylonitrile monomer, alumina, silica and poly(ethylene-vinyl acetate) for 10 minutes, the temperature was raised to 75°C, benzoyl peroxide was added dropwise and the temperature was raised to carry out in-situ polymerization for 15 hours to obtain a polyacrylonitrile / porous inorganic material composite material; wherein the amount of polyacrylonitrile (calculated amount) and (alumina + silica) was 1:1.
[0111] 2) The composite material, polymethyl acrylate, polyoxyethylene polyoxypropylene and deionized water in a mass ratio of 50:3:1:46 are mixed and stirred at high speed to obtain a mixed slurry.
[0112] 3) The mixed slurry was coated on the polyethylene diaphragm by spray coating, and the coating thickness was controlled at 1 μm to obtain a mixed slurry composite polyethylene diaphragm, which was placed in a vacuum oven at 60° C. for 12 h to obtain a finished composite diaphragm.
[0113] The performance of the polyolefin composite diaphragm prepared in Example 3 of the present invention was tested.
[0114] 4) The prepared diaphragm was assembled and tested for 2Ah soft-pack square battery, with the positive electrode being nickel-cobalt-manganese (NCM523) and the negative electrode being graphite, and then the rate performance and impedance tests were performed at 25°C and 1C;
[0115] 5) The prepared diaphragm was placed in a vacuum oven for high temperature treatment at 120° C. for 15 min, and then the shrinkage rate of the diaphragm was tested.
[0116] Example 4
[0117] 1) After ultrasonically mixing acrylonitrile monomer, alumina, silica and poly(ethylene-vinyl acetate) for 10 minutes, the temperature was raised to 75°C, benzoyl peroxide was added dropwise and the temperature was raised to carry out in-situ polymerization for 15 hours to obtain a polyacrylonitrile / porous inorganic material composite material; wherein the amount of polyacrylonitrile (calculated amount) and (zirconia + silica) was 3:2.
[0118] 2) The composite material, polymethyl acrylate, polyoxyethylene polyoxypropylene and deionized water in a mass ratio of 50:3:1:46 are mixed and stirred at high speed to obtain a mixed slurry.
[0119] 3) The mixed slurry was coated on the polyethylene diaphragm by spray coating, and the coating thickness was controlled at 1 μm to obtain a mixed slurry composite polyethylene diaphragm, which was placed in a vacuum oven at 60° C. for 12 h to obtain a finished composite diaphragm.
[0120] The performance of the polyolefin composite diaphragm prepared in Example 4 of the present invention was tested.
[0121] 4) The prepared diaphragm was assembled and tested for 2Ah soft-pack square battery, with the positive electrode being nickel-cobalt-manganese (NCM523) and the negative electrode being graphite, and then the rate performance and impedance tests were performed at 25°C and 1C;
[0122] 5) The prepared diaphragm was placed in a vacuum oven for high temperature treatment at a temperature of 130° C. for 15 min, and then the shrinkage rate of the diaphragm was tested.
[0123] See Table 1, which shows the thermal shrinkage of the polyolefin composite diaphragm prepared by the present invention at a temperature of 100 to 130°C.
[0124] Table 1
[0125]
[0126] See Table 2, which shows the performance test results of the polyolefin composite diaphragm assembled battery prepared by the present invention.
[0127] Table 2
[0128]
[0129] It can be seen from the test data that after high temperature treatment, the stability of the diaphragm is improved. At the same time, the electrochemical performance test shows that the battery capacity retention rate and rate performance are also significantly improved. This shows that the polyolefin diaphragm with high thermal stability disclosed in the present invention can significantly improve the safety performance and electrochemical performance of lithium-ion batteries. At the same time, the functional coating can effectively reduce defects such as microcracks and pores in the polyolefin diaphragm, and can significantly improve the cycle performance and rate performance of lithium-ion batteries. The process is simple, the cost is low, and it has high practicality.
[0130] The above is a detailed introduction to a polyolefin composite diaphragm for lithium ion batteries with good thermal stability and a preparation method thereof, and a lithium ion battery provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method and core ideas of the present invention, including the best mode, and also enables any technician in the field to practice the present invention, including manufacturing and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements that are not different from the text of the claims, or if they include equivalent structural elements that are not substantially different from the text of the claims, then these other embodiments should also be included in the scope of the claims.
Claims
1. A polyolefin composite diaphragm, characterized in that: including a polyolefin-based film; A composite material coating laminated on at least one side of a polyolefin-based film; The composite material coating has a microscopic morphology of stacked and arranged porous inorganic material particles; The pores of the porous inorganic material particles are compounded with polyacrylonitrile colloid particles; The polyacrylonitrile colloidal particles are compounded on the surface of the porous inorganic material particles; The porous inorganic material particles are evenly distributed on the surface of the polyolefin base film; The porous inorganic material includes one or more of alumina, aluminum hydroxide, silicon dioxide, bentonite, expanded graphite, zeolite, diatomaceous earth, vermiculite, perlite and clay; The particle size of the porous inorganic material particles is 0.3-1.5 μm; The thickness of the composite material coating is 0.5-3 μm.
2. The polyolefin composite diaphragm according to claim 1, characterized in that: The base film comprises a polyethylene base film and / or a polypropylene base film; The polyolefin-based membrane is a microporous membrane.
3. The polyolefin composite diaphragm according to claim 1, characterized in that: The molecular weight of the polyacrylonitrile colloid particles is 1000-10000.
4. The polyolefin separator according to claim 1, characterized in that: The median pore size of the polyolefin base film is 10-100 nm; The thickness of the polyolefin base film is 5 to 25 μm; The composite material coating is compounded on the polyolefin base film by mixed slurry.
5. The polyolefin composite diaphragm according to claim 4, characterized in that: The mixed slurry, calculated by raw material mass percentage, comprises: 30-75 parts by weight of polyacrylonitrile / porous inorganic material composite material; Water 25-70 parts by weight; 1-5 parts by weight of adhesive; Wetting agent 0.1~1 parts by weight.
6. The polyolefin composite diaphragm according to claim 5, characterized in that: The porous inorganic material includes one or more of alumina, aluminum hydroxide, silicon dioxide, bentonite, expanded graphite, zeolite, diatomaceous earth, vermiculite, perlite and clay; The adhesive includes one or more of phenyl acrylic acid, polyacrylamide, polyvinyl alcohol, polyethylene oxide, modified paraffin resin, polyacrylate adhesive, polyurethane acrylate and polyacrylate copolymer emulsion; The wetting agent includes one or more of alkyl sulfates, sulfonates, fatty acids or fatty acid ester sulfates, carboxylic acid soaps, phosphates, polyoxyethylene alkylphenol ethers, polyoxyethylene fatty alcohol ethers and polyoxyethylene polyoxypropylene block copolymers.
7. The polyolefin composite diaphragm according to claim 1, characterized in that: The polyolefin-based film is prepared by a wet process; The other side of the polyolefin-based film may also be compounded with other organic functional coatings.
8. A method for preparing a polyolefin composite diaphragm according to any one of claims 1 to 7, characterized in that: The following steps are involved: 1) After ultrasonically mixing acrylonitrile monomer, porous inorganic filler and poly(ethylene-vinyl acetate), benzoyl peroxide is added to react to obtain a polyacrylonitrile / porous inorganic material composite material; 2) The composite material, adhesive, wetting agent and water obtained in the above steps are mixed by high-speed stirring to obtain a mixed slurry; 3) The mixed slurry obtained in the above steps is evenly coated on the polyolefin base film, and after drying, a polyolefin composite diaphragm is obtained.
9. The preparation method according to claim 8, characterized in that The coating method includes one or more of spray coating, gravure coating, narrow slit coating and wet coating; The high-speed stirring and mixing time is 30 to 120 minutes; The rotation speed of the high-speed stirring and mixing is 600-2000 r / min; The thickness of the mixed slurry coating is 1-3 μm; The drying temperature is 40-80°C.
10. A lithium ion battery, characterized in that: Including positive electrode, negative electrode, separator and electrolyte; The diaphragm comprises the polyolefin composite diaphragm according to any one of claims 1 to 7 or the polyolefin composite diaphragm prepared by the preparation method according to any one of claims 8 to 9.