A method for preparing B1-level wire and cable
By using a combination of fireproof sheathing material and nano-silver coating in B1-level wire cables, the problem of harmful gases produced by the combustion of flame retardants in the existing technology is solved, achieving efficient flame retardant effects and production without harmful gases. Improved fire safety.
Patent Information
- Application Number
- CN202210214766.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-04
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-03-04
AI Technical Summary
The flame retardant in existing B1-level cables will produce harmful gases when burned, leading to the expansion of fire accidents, and the flame retardant effect is insufficient.
A B1-level wire and cable preparation method composed of fireproof sheathing material and nano-silver coating is used. The nano-silver coating serves as a catalyst to catalyze carbon monoxide into carbon dioxide when the sheath layer burns, thereby preventing the sheath layer from further burning and achieving good resistance. It has a burning effect and no harmful gases are produced.
It achieves the high-efficiency flame retardant effect of B1-level cables, avoids the generation of harmful gases, and improves fire safety.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cables, and in particular to a method for preparing a B1-level wire cable. Background Art
[0002] According to relevant data, fires caused by wires and cables account for a large proportion of fires in my country. During a fire, the combustible insulation or sheath materials of wires and cables may cause the fire accident to expand further. The heat, toxic gases and thick smoke emitted when the insulation and sheath materials of wires and cables burn may cause further harm or damage to life and property. B1-level wires and cables refer to cables with a flame retardancy rating of ZB level. This level of cable has higher flame retardancy requirements. The flame retardancy of B1-level wires and cables in the prior art is mainly to add phosphorus and halogen flame retardants to the sheath material. This flame retardant produces harmful gases in the flame retardant material.
[0003] Therefore, in view of the shortcomings of the prior art, it is necessary to provide a method for preparing a B1-level wire cable to solve the shortcomings of the prior art. Summary of the invention
[0004] The purpose of the present invention is to avoid the shortcomings of the prior art and provide a method for preparing a B1-class wire and cable. The B1-class wire and cable prepared by the preparation method has good flame retardant effect and does not produce harmful gases.
[0005] The above-mentioned purpose of the present invention is achieved by the following technical measures:
[0006] Provided is a method for preparing a Class B1 cable, comprising a cable core, an insulating layer, a sheath layer made of a fireproof sheath material, and a nano-silver coating, wherein the insulating layer is coated on the outer surface of the cable core, the sheath layer is coated on the outer surface of the insulating layer, and the nano-silver coating is coated on the sheath layer.
[0007] Preferably, the coating method of the nano-silver coating is to spray the pre-prepared nano-silver coating slurry on the outer surface of the sheath layer, and then dry it to obtain a B1 grade wire cable.
[0008] Preferably, the nano silver coating slurry contains resin powder A, solvent, nano silver particles, coupling agent A, boron oxide and nano silicon dioxide.
[0009] Preferably, the raw materials of the fireproof sheath material include resin powder B with a polymerization degree of 1400-2000, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax.
[0010] In the nano silver coating slurry, in weight percentage,
[0011] Resin powder A: 1% to 6%;
[0012] Nano silver particles: 0.01% to 2.0%;
[0013] Coupling agent A: 0.2% to 2.0%;
[0014] Boron oxide: 0.5% to 3.0%;
[0015] Nano silicon dioxide: 0.5%~3.0%.
[0016] In the fireproof sheath material, by weight,
[0017] Resin powder B: 30 to 60 parts;
[0018] Dinonyl terephthalate: 5 to 25 parts;
[0019] Chlorinated paraffin: 2 to 10 parts;
[0020] Polyethylene wax: 0.05 to 0.3 parts;
[0021] Coupling agent B: 1 to 4 parts;
[0022] Nano calcium carbonate: 10 to 30 parts;
[0023] Flame retardant: 2 to 12 parts;
[0024] Nano silicon dioxide: 2 to 8 parts;
[0025] Boron oxide: 2 to 8 parts.
[0026] Further, in the nano silver coating slurry, in weight percentage,
[0027] Resin powder A: 2% to 4%;
[0028] Nano silver particles: 0.05% to 1.0%;
[0029] Coupling agent A: 0.5% to 1.0%;
[0030] Boron oxide: 1.0% to 2.0%;
[0031] Nano silicon dioxide: 1.0%~2.0%.
[0032] Further, in the fireproof sheath material, in parts by weight,
[0033] Resin powder B: 40 to 55 parts;
[0034] Dinonyl terephthalate: 10 to 20 parts;
[0035] Chlorinated paraffin: 5 to 8 parts;
[0036] Polyethylene wax: 0.1 to 0.2 parts;
[0037] Coupling agent B: 1.5 to 2 parts;
[0038] Nano calcium carbonate: 15 to 20 parts;
[0039] Flame retardant: 3 to 6 parts;
[0040] Nano silicon dioxide: 3 to 5 parts;
[0041] Boron oxide: 3 to 5 parts.
[0042] Preferably, the coupling agent A is a silane coupling agent or a titanate coupling agent.
[0043] Preferably, the resin powder A is polyurethane, ethyl cellulose or metallocene polyethylene.
[0044] Preferably, the coupling agent B is a titanate coupling agent.
[0045] Preferably, the flame retardants are antimony trioxide and aluminum hydroxide.
[0046] Preferably, the preparation method of the nano silver coating slurry comprises:
[0047] Step A, adding nano silver particles and coupling agent A to a propylene glycol solution of resin powder A, and performing ultrasonic dispersion to obtain a mixed solution;
[0048] Step B: adding boron oxide and nano-silicon dioxide into the mixed solution, and dispersing by ultrasonic to obtain nano-silver coating slurry.
[0049] Preferably, the preparation of the fireproof sheath material comprises the following steps:
[0050] Step 1: firstly place resin powder B, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax in a high-speed kneader, heat to 90° C. to 110° C., knead and stir for 8 min to 15 min to obtain a mixture;
[0051] Step 3: placing the mixed material in a granulator and controlling the temperature to be 130° C. to 150° C. for extrusion granulation, and then cutting and cooling the mixed material to obtain the fireproof sheath material.
[0052] The method for preparing a Class B1 cable of the present invention comprises a cable core, an insulating layer, a sheath layer made of a fireproof sheath material, and a nano-silver coating, wherein the insulating layer is coated on the outer surface of the cable core, the sheath layer is coated on the outer surface of the insulating layer, and the nano-silver coating is coated on the sheath layer; the coating method of the nano-silver coating is to spray a pre-prepared nano-silver coating slurry on the outer surface of the sheath layer, and then dry it to obtain a Class B1 cable. The Class B1 cable of the present invention is coated with a nano-silver coating on the sheath layer, and the nano-silver coating acts as a catalyst to catalyze carbon monoxide generated when the sheath layer burns into carbon dioxide, and this part of carbon dioxide surrounds the sheath layer to prevent the sheath layer from further burning, thereby producing a better flame retardant effect, and no harmful gas is generated. DETAILED DESCRIPTION
[0053] The technical solution of the present invention is further described in conjunction with the following embodiments.
[0054] Example 1.
[0055] A method for preparing a B1-class wire cable comprises a cable core, an insulating layer, a sheath layer made of a fireproof sheath material and a nano-silver coating, wherein the insulating layer is coated on the outer surface of the cable core, the sheath layer is coated on the outer surface of the insulating layer, and the nano-silver coating is coated on the sheath layer.
[0056] The coating method of the nano silver coating is to spray the pre-prepared nano silver coating slurry on the outer surface of the sheath layer, and then dry it to obtain a B1 grade wire cable.
[0057] The nano silver coating slurry contains resin powder A, solvent, nano silver particles, coupling agent A, boron oxide and nano silicon dioxide.
[0058] The raw materials of the fireproof sheath material contain resin powder B with a polymerization degree of 1400-2000, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax.
[0059] In the nano silver coating slurry, in weight percentage,
[0060] Resin powder A: 1% to 6%;
[0061] Nano silver particles: 0.01% to 2.0%;
[0062] Coupling agent A: 0.2% to 2.0%;
[0063] Boron oxide: 0.5% to 3.0%;
[0064] Nano silicon dioxide: 0.5%~3.0%.
[0065] In the fireproof sheath material, by weight,
[0066] Resin powder B: 30 to 60 parts;
[0067] Dinonyl terephthalate: 5 to 25 parts;
[0068] Chlorinated paraffin: 2 to 10 parts;
[0069] Polyethylene wax: 0.05 to 0.3 parts;
[0070] Coupling agent B: 1 to 4 parts;
[0071] Nano calcium carbonate: 10 to 30 parts;
[0072] Flame retardant: 2 to 12 parts;
[0073] Nano silicon dioxide: 2 to 8 parts;
[0074] Boron oxide: 2 to 8 parts.
[0075] Wherein, coupling agent A is a silane coupling agent or a titanate coupling agent. Resin powder A is polyurethane, ethyl cellulose or metallocene polyethylene. Coupling agent B is a titanate coupling agent. Flame retardants are antimony trioxide and aluminum hydroxide.
[0076] Because the sheath layer surface is smooth, its surface energy is low, it is difficult to adsorb other substances, and the nano silver coating slurry will not dissolve or swell the sheath layer. The nano silver coating slurry of the present invention cooperates with the boron oxide and nano silicon dioxide in the fireproof sheath material to reduce the surface tension of the nano silver coating slurry in the fireproof sheath material, which is conducive to wet spreading in the sheath layer. The coupling agent A of the nano silver coating slurry and the coupling agent B of the fireproof sheath material produce a two-way coupling effect between the nano silver coating and the sheath layer, strengthen the boundary and the bonding force to improve the nano silver coating adhesion time.
[0077] The resin powder B with a polymerization degree of 1400 to 2000 of the present invention can improve elasticity and softness. Dinonyl terephthalate and chlorinated paraffin act as plasticizers to increase mechanical properties such as bending resistance and impact resistance of the resin powder B. Polyethylene wax acts as a lubricant to increase compatibility with the resin powder B. Nano calcium carbonate interacts with chlorinated paraffin to increase the stability of the present invention.
[0078] The preparation method of the nano silver coating slurry of the present invention comprises:
[0079] Step A, adding nano silver particles and coupling agent A to a propylene glycol solution of resin powder A, and performing ultrasonic dispersion to obtain a mixed solution;
[0080] Step B: adding boron oxide and nano-silicon dioxide into the mixed solution, and dispersing by ultrasonic to obtain nano-silver coating slurry.
[0081] The B1-class wire and cable obtained by the preparation method of the B1-class wire and cable of the present invention is coated with a nano-silver coating on the sheath layer. The nano-silver coating acts as a catalyst to catalyze carbon monoxide generated when the sheath layer burns into carbon dioxide. This part of carbon dioxide surrounds the sheath layer to prevent the sheath layer from further burning, thereby producing a better flame retardant effect without generating harmful gases.
[0082] Example 2.
[0083] A method for preparing a B1-class wire cable comprises a cable core, an insulating layer, a sheath layer made of a fireproof sheath material and a nano-silver coating, wherein the insulating layer is coated on the outer surface of the cable core, the sheath layer is coated on the outer surface of the insulating layer, and the nano-silver coating is coated on the sheath layer.
[0084] The coating method of the nano silver coating is to spray the pre-prepared nano silver coating slurry on the outer surface of the sheath layer, and then dry it to obtain a B1 grade wire cable.
[0085] The nano silver coating slurry contains resin powder A, solvent, nano silver particles, coupling agent A, boron oxide and nano silicon dioxide.
[0086] The raw materials of the fireproof sheath material contain resin powder B with a polymerization degree of 1400-2000, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax.
[0087] In the nano silver coating slurry, in weight percentage,
[0088] Resin powder A: 2% to 4%;
[0089] Nano silver particles: 0.05% to 1.0%;
[0090] Coupling agent A: 0.5% to 1.0%;
[0091] Boron oxide: 1.0% to 2.0%;
[0092] Nano silicon dioxide: 1.0%~2.0%.
[0093] In the fireproof sheath material, by weight,
[0094] Resin powder B: 40 to 55 parts;
[0095] Dinonyl terephthalate: 10 to 20 parts;
[0096] Chlorinated paraffin: 5 to 8 parts;
[0097] Polyethylene wax: 0.1 to 0.2 parts;
[0098] Coupling agent B: 1.5 to 2 parts;
[0099] Nano calcium carbonate: 15 to 20 parts;
[0100] Flame retardant: 3 to 6 parts;
[0101] Nano silicon dioxide: 3 to 5 parts;
[0102] Boron oxide: 3 to 5 parts.
[0103] Wherein, coupling agent A is a silane coupling agent or a titanate coupling agent. Resin powder A is polyurethane, ethyl cellulose or metallocene polyethylene. Coupling agent B is a titanate coupling agent. Flame retardants are antimony trioxide and aluminum hydroxide.
[0104] Compared with Example 1, the flame retardant effect, elasticity and wear resistance of the B1 grade wire and cable preparation method of this embodiment are better than those of Example 1.
[0105] Example 3.
[0106] A method for preparing a B1-class wire cable comprises a cable core, an insulating layer, a sheath layer made of a fireproof sheath material and a nano-silver coating, wherein the insulating layer is coated on the outer surface of the cable core, the sheath layer is coated on the outer surface of the insulating layer, and the nano-silver coating is coated on the sheath layer.
[0107] The coating method of the nano silver coating is to spray the pre-prepared nano silver coating slurry on the outer surface of the sheath layer, and then dry it to obtain a B1 grade wire cable.
[0108] The nano silver coating slurry contains resin powder A, solvent, nano silver particles, coupling agent A, boron oxide and nano silicon dioxide.
[0109] The raw materials of the fireproof sheath material contain resin powder B with a polymerization degree of 1890, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax.
[0110] In the nano silver coating slurry, in weight percentage,
[0111] Resin powder A: 1%;
[0112] Nanosilver particles: 0.01%;
[0113] Coupling agent A: 0.2%;
[0114] Boron oxide: 0.5%;
[0115] Nano silicon dioxide: 0.5%.
[0116] In the fireproof sheath material, by weight,
[0117] Resin powder B: 30 parts;
[0118] Dinonyl terephthalate: 5 parts;
[0119] Chlorinated paraffin: 2 parts;
[0120] Polyethylene wax: 0.05 parts;
[0121] Coupling agent B: 1 part;
[0122] Nano calcium carbonate: 10 parts;
[0123] Flame retardant: 2 parts;
[0124] Nano silicon dioxide: 2 parts;
[0125] Boron oxide: 2 parts.
[0126] Wherein, coupling agent A is a silane coupling agent, resin powder A is ethyl cellulose, coupling agent B is a titanate coupling agent, and flame retardants are antimony trioxide and aluminum hydroxide.
[0127] Among them, ethyl cellulose and resin powder B were purchased from Ningbo Weiye Plastic Co., Ltd., dinonyl terephthalate was purchased from Liaocheng Ruibang Plastic Additive Co., Ltd., chlorinated paraffin and polyethylene wax were purchased from Yangzhou Roland New Materials Co., Ltd., polyethylene oxide was purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd., nano calcium carbonate was purchased from Zhongshan Deyuan Trading Co., Ltd., boric oxide was purchased from Shandong Haoshun Chemical Co., Ltd., nano nickel powder was purchased from Zhuozhou Yourong New Materials Technology Co., Ltd., nano silicon dioxide was purchased from Hangzhou Hengge Nano Technology Co., Ltd., silane coupling agent and titanate coupling agent were purchased from Nanjing Xuanhao New Materials Technology Co., Ltd., antimony trioxide was purchased from Shijiazhuang Pinbai Chemical Technology Co., Ltd., aluminum hydroxide was purchased from Jinan Chenxing Chemical Co., Ltd., and nano silver particles were purchased from Guangzhou Hongwu Materials Technology Co., Ltd.
[0128] Compared with Example 1, the flame retardant effect, elasticity and wear resistance of the B1 grade wire and cable preparation method of this embodiment are better than those of Example 1.
[0129] Example 4.
[0130] A method for preparing a B1-class wire cable comprises a cable core, an insulating layer, a sheath layer made of a fireproof sheath material and a nano-silver coating, wherein the insulating layer is coated on the outer surface of the cable core, the sheath layer is coated on the outer surface of the insulating layer, and the nano-silver coating is coated on the sheath layer.
[0131] The coating method of the nano silver coating is to spray the pre-prepared nano silver coating slurry on the outer surface of the sheath layer, and then dry it to obtain a B1 grade wire cable.
[0132] The nano silver coating slurry contains resin powder A, solvent, nano silver particles, coupling agent A, boron oxide and nano silicon dioxide.
[0133] The raw materials of the fireproof sheath material contain resin powder B with a polymerization degree of 1850, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax.
[0134] In the nano silver coating slurry, in weight percentage,
[0135] Resin powder A: 6%;
[0136] Nanosilver particles: 2.0%;
[0137] Coupling agent A: 2.0%;
[0138] Boron oxide: 3.0%;
[0139] Nano-silicon dioxide: 3.0%.
[0140] In the fireproof sheath material, by weight,
[0141] Resin powder B: 60 parts;
[0142] Dinonyl terephthalate: 25 parts;
[0143] Chlorinated paraffin: 10 parts;
[0144] Polyethylene wax: 0.3 parts;
[0145] Coupling agent B: 4 parts;
[0146] Nano calcium carbonate: 30 parts;
[0147] Flame retardant: 12 parts;
[0148] Nano silicon dioxide: 8 parts;
[0149] Boron oxide: 8 parts.
[0150] Wherein, coupling agent A is a silane coupling agent, resin powder A is polyurethane, coupling agent B is a titanate coupling agent, and flame retardants are antimony trioxide and aluminum hydroxide.
[0151] Among them, polyurethane and resin powder B were purchased from Ningbo Weiye Plastic Chemical Co., Ltd., dinonyl terephthalate was purchased from Liaocheng Ruibang Plastic Additive Co., Ltd., chlorinated paraffin and polyethylene wax were purchased from Yangzhou Roland New Materials Co., Ltd., polyethylene oxide was purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd., nano calcium carbonate was purchased from Zhongshan Deyuan Trading Co., Ltd., boric oxide was purchased from Shandong Haoshun Chemical Co., Ltd., nano nickel powder was purchased from Zhuozhou Yourong New Materials Technology Co., Ltd., nano silicon dioxide was purchased from Hangzhou Hengge Nano Technology Co., Ltd., silane coupling agent and titanate coupling agent were purchased from Nanjing Xuanhao New Materials Technology Co., Ltd., antimony trioxide was purchased from Shijiazhuang Pinbai Chemical Technology Co., Ltd., aluminum hydroxide was purchased from Jinan Chenxing Chemical Co., Ltd., and nano silver particles were purchased from Guangzhou Hongwu Materials Technology Co., Ltd.
[0152] Compared with Example 1, the flame retardant effect, elasticity and wear resistance of the B1 grade wire and cable preparation method of this embodiment are better than those of Example 1.
[0153] Example 5.
[0154] A method for preparing a B1-class wire cable comprises a cable core, an insulating layer, a sheath layer made of a fireproof sheath material and a nano-silver coating, wherein the insulating layer is coated on the outer surface of the cable core, the sheath layer is coated on the outer surface of the insulating layer, and the nano-silver coating is coated on the sheath layer.
[0155] The coating method of the nano silver coating is to spray the pre-prepared nano silver coating slurry on the outer surface of the sheath layer, and then dry it to obtain a B1 grade wire cable.
[0156] The nano silver coating slurry contains resin powder A, solvent, nano silver particles, coupling agent A, boron oxide and nano silicon dioxide.
[0157] The raw materials of the fireproof sheath material contain resin powder B with a polymerization degree of 2000, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax.
[0158] In the nano silver coating slurry, in weight percentage,
[0159] Resin powder A: 2%;
[0160] Nanosilver particles: 0.05%;
[0161] Coupling agent A: 0.5%;
[0162] Boron oxide: 1.0%;
[0163] Nano-silicon dioxide: 1.0%.
[0164] In the fireproof sheath material, by weight,
[0165] Resin powder B: 40 parts;
[0166] Dinonyl terephthalate: 10 parts;
[0167] Chlorinated paraffin: 5 parts;
[0168] Polyethylene wax: 0.1 part;
[0169] Coupling agent B: 1.5 parts;
[0170] Nano calcium carbonate: 15 parts;
[0171] Flame retardant: 3 parts;
[0172] Nano silicon dioxide: 3 parts;
[0173] Boron oxide: 3 parts.
[0174] Wherein, coupling agent A is a silane coupling agent, resin powder A is polyurethane, coupling agent B is a titanate coupling agent, and flame retardants are antimony trioxide and aluminum hydroxide.
[0175] Among them, polyurethane and resin powder B were purchased from Ningbo Weiye Plastic Chemical Co., Ltd., dinonyl terephthalate was purchased from Liaocheng Ruibang Plastic Additive Co., Ltd., chlorinated paraffin and polyethylene wax were purchased from Yangzhou Roland New Materials Co., Ltd., polyethylene oxide was purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd., nano calcium carbonate was purchased from Zhongshan Deyuan Trading Co., Ltd., boric oxide was purchased from Shandong Haoshun Chemical Co., Ltd., nano nickel powder was purchased from Zhuozhou Yourong New Materials Technology Co., Ltd., nano silicon dioxide was purchased from Hangzhou Hengge Nano Technology Co., Ltd., silane coupling agent and titanate coupling agent were purchased from Nanjing Xuanhao New Materials Technology Co., Ltd., antimony trioxide was purchased from Shijiazhuang Pinbai Chemical Technology Co., Ltd., aluminum hydroxide was purchased from Jinan Chenxing Chemical Co., Ltd., and nano silver particles were purchased from Guangzhou Hongwu Materials Technology Co., Ltd.
[0176] Compared with Example 1, the flame retardant effect, elasticity and wear resistance of the B1 grade wire and cable preparation method of this embodiment are better than those of Example 1.
[0177] Example 6.
[0178] A method for preparing a B1-class wire cable comprises a cable core, an insulating layer, a sheath layer made of a fireproof sheath material and a nano-silver coating, wherein the insulating layer is coated on the outer surface of the cable core, the sheath layer is coated on the outer surface of the insulating layer, and the nano-silver coating is coated on the sheath layer.
[0179] The coating method of the nano silver coating is to spray the pre-prepared nano silver coating slurry on the outer surface of the sheath layer, and then dry it to obtain a B1 grade wire cable.
[0180] The nano silver coating slurry contains resin powder A, solvent, nano silver particles, coupling agent A, boron oxide and nano silicon dioxide.
[0181] The raw materials of the fireproof sheath material contain resin powder B with a polymerization degree of 1400, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax.
[0182] In the nano silver coating slurry, in weight percentage,
[0183] Resin powder A: 4%;
[0184] Nanosilver particles: 1.0%;
[0185] Coupling agent A: 1.0%;
[0186] Boron oxide: 2.0%;
[0187] Nano-silicon dioxide: 2.0%.
[0188] In the fireproof sheath material, by weight,
[0189] Resin powder B: 55 parts;
[0190] Dinonyl terephthalate: 20 parts;
[0191] Chlorinated paraffin: 8 parts;
[0192] Polyethylene wax: 0.2 parts;
[0193] Coupling agent B: 2 parts;
[0194] Nano calcium carbonate: 20 parts;
[0195] Flame retardant: 6 parts;
[0196] Nano silicon dioxide: 5 parts;
[0197] Boron oxide: 5 parts.
[0198] Wherein, coupling agent A is a silane coupling agent, resin powder A is polyurethane and metallocene polyethylene, coupling agent B is a titanate coupling agent, and flame retardants are antimony trioxide and aluminum hydroxide.
[0199] Among them, polyurethane and resin powder B were purchased from Ningbo Weiye Plastic Chemical Co., Ltd., dinonyl terephthalate was purchased from Liaocheng Ruibang Plastic Additive Co., Ltd., chlorinated paraffin and polyethylene wax were purchased from Yangzhou Roland New Materials Co., Ltd., polyethylene oxide was purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd., nano calcium carbonate was purchased from Zhongshan Deyuan Trading Co., Ltd., boric oxide was purchased from Shandong Haoshun Chemical Co., Ltd., nano nickel powder was purchased from Zhuozhou Yourong New Materials Technology Co., Ltd., nano silicon dioxide was purchased from Hangzhou Hengge Nano Technology Co., Ltd., silane coupling agent and titanate coupling agent were purchased from Nanjing Xuanhao New Materials Technology Co., Ltd., antimony trioxide was purchased from Shijiazhuang Pinbai Chemical Technology Co., Ltd., aluminum hydroxide was purchased from Jinan Chenxing Chemical Co., Ltd., nano silver particles were purchased from Guangzhou Hongwu Materials Technology Co., Ltd., and metallocene polyethylene was purchased from ExxonMobil.
[0200] Compared with Example 1, the flame retardant effect, elasticity and wear resistance of the B1 grade wire and cable preparation method of this embodiment are better than those of Example 1.
[0201] Example 7.
[0202] A method for preparing a B1-class wire cable comprises a cable core, an insulating layer, a sheath layer made of a fireproof sheath material and a nano-silver coating, wherein the insulating layer is coated on the outer surface of the cable core, the sheath layer is coated on the outer surface of the insulating layer, and the nano-silver coating is coated on the sheath layer.
[0203] The coating method of the nano silver coating is to spray the pre-prepared nano silver coating slurry on the outer surface of the sheath layer, and then dry it to obtain a B1 grade wire cable.
[0204] The nano silver coating slurry contains resin powder A, solvent, nano silver particles, coupling agent A, boron oxide and nano silicon dioxide.
[0205] The raw materials of the fireproof sheath material contain resin powder B with a polymerization degree of 1650, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax.
[0206] In the nano silver coating slurry, in weight percentage,
[0207] Resin powder A: 4.5%;
[0208] Nanosilver particles: 1.33%;
[0209] Coupling agent A: 1.05%;
[0210] Boron oxide: 1.5%;
[0211] Nano silicon dioxide: 2.5%.
[0212] In the fireproof sheath material, by weight,
[0213] Resin powder B: 48 parts;
[0214] Dinonyl terephthalate: 12;
[0215] Chlorinated paraffin: 6 parts;
[0216] Polyethylene wax: 0.25 parts;
[0217] Coupling agent B: 2.6 parts;
[0218] Nano calcium carbonate: 25 parts;
[0219] Flame retardant: 8 parts;
[0220] Nano silicon dioxide: 6 parts;
[0221] Boron oxide: 4 parts.
[0222] Wherein, coupling agent A is a silane coupling agent, resin powder A is polyurethane and ethyl cellulose, coupling agent B is a titanate coupling agent, and flame retardants are antimony trioxide and aluminum hydroxide.
[0223] Among them, resin powder B was purchased from Ningbo Weiye Plastic Chemical Co., Ltd., dinonyl terephthalate was purchased from Liaocheng Ruibang Plastic Additive Co., Ltd., chlorinated paraffin and polyethylene wax were purchased from Yangzhou Roland New Materials Co., Ltd., polyethylene oxide was purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd., nano calcium carbonate was purchased from Zhongshan Deyuan Trading Co., Ltd., boric oxide was purchased from Shandong Haoshun Chemical Co., Ltd., nano nickel powder was purchased from Zhuozhou Yourong New Materials Technology Co., Ltd., nano silicon dioxide was purchased from Hangzhou Hengge Nano Technology Co., Ltd., silane coupling agent and titanate coupling agent were purchased from Nanjing Xuanhao New Materials Technology Co., Ltd., antimony trioxide was purchased from Shijiazhuang Pinbai Chemical Technology Co., Ltd., aluminum hydroxide was purchased from Jinan Chenxing Chemical Co., Ltd., nano silver particles were purchased from Guangzhou Hongwu Materials Technology Co., Ltd., and metallocene polyethylene was purchased from ExxonMobil.
[0224] Compared with Example 1, the flame retardant effect, elasticity and wear resistance of the B1 grade wire and cable preparation method of this embodiment are better than those of Example 1.
[0225] Example 8.
[0226] A method for preparing a B1-class wire cable comprises a cable core, an insulating layer, a sheath layer made of a fireproof sheath material and a nano-silver coating, wherein the insulating layer is coated on the outer surface of the cable core, the sheath layer is coated on the outer surface of the insulating layer, and the nano-silver coating is coated on the sheath layer.
[0227] The coating method of the nano silver coating is to spray the pre-prepared nano silver coating slurry on the outer surface of the sheath layer, and then dry it to obtain a B1 grade wire cable.
[0228] The nano silver coating slurry contains resin powder A, solvent, nano silver particles, coupling agent A, boron oxide and nano silicon dioxide.
[0229] The raw materials of the fireproof sheath material contain resin powder B with a polymerization degree of 1700, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax.
[0230] In the nano silver coating slurry, in weight percentage,
[0231] Resin powder A: 3%;
[0232] Nanosilver particles: 0.7%;
[0233] Coupling agent A: 00.8%;
[0234] Boron oxide: 1.6%;
[0235] Nano-silicon dioxide: 1.4%.
[0236] In the fireproof sheath material, by weight,
[0237] Resin powder B: 53 parts;
[0238] Dinonyl terephthalate: 17 parts;
[0239] Chlorinated paraffin: 6.4 parts;
[0240] Polyethylene wax: 0.14 parts;
[0241] Coupling agent B: 1.7 parts;
[0242] Nano calcium carbonate: 1.9 parts;
[0243] Flame retardant: 5.4 parts;
[0244] Nano silicon dioxide: 4.1 parts;
[0245] Boron oxide: 4.3 parts.
[0246] Wherein, coupling agent A is titanate coupling agent, resin powder A is metallocene polyethylene, coupling agent B is titanate coupling agent, and flame retardants are antimony trioxide and aluminum hydroxide.
[0247] Among them, ethyl cellulose, polyurethane and resin powder B were purchased from Ningbo Weiye Plastic Co., Ltd., dinonyl terephthalate was purchased from Liaocheng Ruibang Plastic Additive Co., Ltd., chlorinated paraffin and polyethylene wax were purchased from Yangzhou Roland New Materials Co., Ltd., polyethylene oxide was purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd., nano calcium carbonate was purchased from Zhongshan Deyuan Trading Co., Ltd., boric oxide was purchased from Shandong Haoshun Chemical Co., Ltd., nano nickel powder was purchased from Zhuozhou Yourong New Materials Technology Co., Ltd., nano silicon dioxide was purchased from Hangzhou Hengge Nano Technology Co., Ltd., silane coupling agent and titanate coupling agent were purchased from Nanjing Xuanhao New Materials Technology Co., Ltd., antimony trioxide was purchased from Shijiazhuang Pinbai Chemical Technology Co., Ltd., aluminum hydroxide was purchased from Jinan Chenxing Chemical Co., Ltd., and nano silver particles were purchased from Guangzhou Hongwu Materials Technology Co., Ltd.
[0248] Compared with Example 1, the flame retardant effect, elasticity and wear resistance of the B1 grade wire and cable preparation method of this embodiment are better than those of Example 1.
[0249] Example 9.
[0250] A method for preparing a B1-class wire and cable, using the raw material ratio of any one of the fire-resistant sheath materials in Examples 3 to 8, the steps of preparing the fire-resistant sheath material include:
[0251] Step 1: firstly place resin powder B, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax in a high-speed kneader, heat to 90° C. to 110° C., knead and stir for 8 min to 15 min to obtain a mixture;
[0252] Step 3: placing the mixed material in a granulator and controlling the temperature to be 130° C. to 150° C. for extrusion granulation, and then cutting and cooling the mixed material to obtain the fireproof sheath material.
[0253] The B1-class wire and cable obtained by the B1-class wire and cable preparation method is coated with a nano-silver coating on the sheath layer. The nano-silver coating acts as a catalyst to catalyze carbon monoxide generated when the sheath layer burns into carbon dioxide. This part of carbon dioxide surrounds the sheath layer to prevent the sheath layer from further burning, thereby producing a better flame retardant effect without generating harmful gases.
[0254] Example 10.
[0255] A method for preparing a B1-class wire and cable, using the raw material ratio of any one of the fire-resistant sheath materials in Examples 3 to 8, the steps of preparing the fire-resistant sheath material include:
[0256] Step 1: firstly place resin powder B, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax in a high-speed kneader, heat to 90° C., knead and stir for 8 minutes to obtain a mixture;
[0257] Step 3: placing the mixed material in a granulator and controlling the temperature to 130° C. for extrusion granulation, and then cutting and cooling the mixed material to obtain the fireproof sheath material.
[0258] The B1-class wire and cable obtained by the B1-class wire and cable preparation method is coated with a nano-silver coating on the sheath layer. The nano-silver coating acts as a catalyst to catalyze carbon monoxide generated when the sheath layer burns into carbon dioxide. This part of carbon dioxide surrounds the sheath layer to prevent the sheath layer from further burning, thereby producing a better flame retardant effect without generating harmful gases.
[0259] Example 11.
[0260] A method for preparing a B1-class wire and cable, using the raw material ratio of any one of the fire-resistant sheath materials in Examples 3 to 8, the steps of preparing the fire-resistant sheath material include:
[0261] Step 1: firstly place resin powder B, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax in a high-speed kneader, heat to 110° C., knead and stir for 15 minutes to obtain a mixture;
[0262] Step 3: placing the mixed material in a granulator and controlling the temperature to 150° C. for extrusion granulation, and then cutting and cooling the mixed material to obtain the fireproof sheath material.
[0263] The B1-class wire and cable obtained by the B1-class wire and cable preparation method is coated with a nano-silver coating on the sheath layer. The nano-silver coating acts as a catalyst to catalyze carbon monoxide generated when the sheath layer burns into carbon dioxide. This part of carbon dioxide surrounds the sheath layer to prevent the sheath layer from further burning, thereby producing a better flame retardant effect without generating harmful gases.
[0264] Example 12.
[0265] A method for preparing a B1-class wire and cable, using the raw material ratio of any one of the fire-resistant sheath materials in Examples 3 to 8, the steps of preparing the fire-resistant sheath material include:
[0266] Step 1: firstly place resin powder B, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax in a high-speed kneader, heat to 100° C. and knead and stir for 9 minutes to obtain a mixture;
[0267] Step 3: placing the mixed material in a granulator and controlling the temperature to 145° C. for extrusion granulation, and then cutting and cooling the mixed material to obtain the fireproof sheath material.
[0268] The B1-class wire and cable obtained by the B1-class wire and cable preparation method is coated with a nano-silver coating on the sheath layer. The nano-silver coating acts as a catalyst to catalyze carbon monoxide generated when the sheath layer burns into carbon dioxide. This part of carbon dioxide surrounds the sheath layer to prevent the sheath layer from further burning, thereby producing a better flame retardant effect without generating harmful gases.
[0269] The present invention obtains a sheath material sample group of the B1 grade wire and cable preparation method of the present invention by using the raw material ratios of Examples 3-8 and the process for obtaining the fireproof sheath material of Examples 10-12.
[0270] Table 1. Sample group of B1 grade wire and cable preparation method
[0271] Sample set Raw material ratio Preparation method Sample 1 Example 3 Embodiment 11 Sample 2 Example 4 Embodiment 11 Sample 3 Example 5 Embodiment 11 Sample 4 Example 6 Embodiment 11 Sample 5 Example 7 Embodiment 11 Sample 6 Example 8 Embodiment 11 Sample 8 Example 5 Example 10 Sample 9 Example 5 Example 10 Sample 10 Example 7 Example 12
[0272] Under the same experimental conditions, Table 2 shows the performance test of the nano silver coating sheath layer of the fireproof sheath material of Sample 1-11. The relevant performance is shown in Table 2:
[0273] Table 2. Corresponding test performance of samples prepared into sheath layer
[0274]
[0275]
[0276] It can be seen from Table 2 that the sheath layer of the present invention obtained by combining resin powder B and other components has good tensile strength and elongation, and the critical oxygen index of the B1 grade wire and cable of the present invention after being coated with nano silver coating is above 30, which has good flame retardant effect.
[0277] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a B1-level wire and cable, characterized in that: A cable core, an insulating layer, a sheath layer made of a fireproof sheath material and a nano-silver coating are provided, wherein the insulating layer is coated on the outer surface of the cable core, the sheath layer is coated on the outer surface of the insulating layer, and the nano-silver coating is coated on the sheath layer; The coating method of the nano silver coating is to spray the pre-prepared nano silver coating slurry on the outer surface of the sheath layer, and then dry it to obtain a B1 grade wire cable; The nano silver coating slurry contains resin powder A, solvent, nano silver particles, coupling agent A, boron oxide and nano silicon dioxide; the raw materials of the fireproof sheath material contain resin powder B with a polymerization degree of 1400-2000, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax; in the nano silver coating slurry, in weight percentage, Resin powder A: 1% to 6%; Nano silver particles: 0.01% to 2.0%; Coupling agent A: 0.2% to 2.0%; Boron oxide: 0.5% to 3.0%; Nano silicon dioxide: 0.5%~3.0%.
2. The method for preparing a Class B1 wire and cable according to claim 1, characterized in that: In the fireproof sheath material, by weight, Resin powder B: 30 to 60 parts; Dinonyl terephthalate: 5 to 25 parts; Chlorinated paraffin: 2 to 10 parts; Polyethylene wax: 0.05 to 0.3 parts; Coupling agent B: 1 to 4 parts; Nano calcium carbonate: 10 to 30 parts; Flame retardant: 2 to 12 parts; Nano silicon dioxide: 2 to 8 parts; Boron oxide: 2 to 8 parts.
3. The method for preparing a Class B1 wire and cable according to claim 2, characterized in that: In the nano silver coating slurry, in weight percentage, Resin powder A: 2% to 4%; Nano silver particles: 0.05% to 1.0%; Coupling agent A: 0.5% to 1.0%; Boron oxide: 1.0% to 2.0%; Nano silicon dioxide: 1.0%~2.0%.
4. The method for preparing a Class B1 wire and cable according to claim 3, characterized in that: In the fireproof sheath material, by weight, Resin powder B: 40 to 55 parts; Dinonyl terephthalate: 10 to 20 parts; Chlorinated paraffin: 5 to 8 parts; Polyethylene wax: 0.1 to 0.2 parts; Coupling agent B: 1.5 to 2 parts; Nano calcium carbonate: 15 to 20 parts; Flame retardant: 3 to 6 parts; Nano silicon dioxide: 3 to 5 parts; Boron oxide: 3 to 5 parts.
5. The method for preparing a Class B1 wire and cable according to claim 4, characterized in that: The coupling agent A is a silane coupling agent or a titanate coupling agent; The resin powder A is polyurethane, ethyl cellulose or metallocene polyethylene; The coupling agent B is a titanate coupling agent; The flame retardants are antimony trioxide and aluminum hydroxide.
6. The method for preparing a Class B1 wire and cable according to claim 5, characterized in that: The preparation method of the nano silver coating slurry comprises: Step A, adding nano silver particles and coupling agent A to a propylene glycol solution of resin powder A, and performing ultrasonic dispersion to obtain a mixed solution; Step B: adding boron oxide and nano-silicon dioxide to the mixed solution, and dispersing by ultrasonic to obtain nano-silver coating slurry.
7. The method for preparing a Class B1 wire and cable according to claim 6, characterized in that: The preparation of the fireproof sheath material comprises the following steps: Step 1: firstly place resin powder B, dinonyl terephthalate, chlorinated paraffin, polyethylene oxide, flame retardant, nano calcium carbonate, coupling agent B, boron oxide, nano silicon dioxide and polyethylene wax in a high-speed kneader, heat to 90° C. to 110° C., knead and stir for 8 min to 15 min to obtain a mixture; Step 3: placing the mixed material in a granulator and controlling the temperature to be 130° C. to 150° C. for extrusion granulation, and then cutting and cooling the mixed material to obtain the fireproof sheath material.