A high nitrogen content non-precious metal single atom catalyst and its preparation method and application

By using materials such as urea, glucose and sodium chloride to prepare non-noble metal single-atom catalysts with high nitrogen content, and forming hierarchical pore structures and single-atom metal active sites through multi-step pyrolysis treatment, the complexity and cost of catalyst preparation in the existing technology are solved. The problem of high environmental pollution and environmental pollution improves the activity of the catalyst and the utilization rate of metal atoms.

CN114713255BInactive Publication Date: 2024-10-01HANGZHOU DIANZI UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111423444.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-26
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing technology, the catalyst preparation process is complex, costly and environmentally polluting. In particular, the high price and poor stability of noble metal catalysts limit their industrial application. In addition, the utilization rate of metal atoms in transition metal single-atom catalysts during the pyrolysis process is low, which affects oxygen. reduction reaction activity.

Method used

Low-cost materials such as urea, glucose and sodium chloride are used to prepare non-noble metal single-atom catalysts with high nitrogen content. Sodium chloride is used as a pore-forming agent and multi-step pyrolysis is performed to inhibit metal agglomeration and nitrogen decomposition and increase the nitrogen content of the catalyst. and metal atom anchor sites to form hierarchical pore structures and single-atom metal active sites.

Benefits of technology

It achieves low-cost, environmentally friendly catalyst preparation, improves metal atom utilization and catalytic activity, improves oxygen reduction reaction efficiency, and solves the problems of low catalyst activity and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003378226660000011
    Figure HDA0003378226660000011
  • Figure HDA0003378226660000012
    Figure HDA0003378226660000012
  • Figure HDA0003378226660000021
    Figure HDA0003378226660000021
Patent Text Reader

Abstract

The present invention relates to the field of catalyst preparation, and discloses a high-nitrogen content non-precious metal single-atom catalyst and its preparation method and application, comprising the following preparation steps: adding a nitrogen source, a carbon source, a non-precious metal salt and a salt template to deionized water in a certain proportion and mixing them evenly; then performing oil bath and freeze drying treatment in sequence to obtain a precursor powder; performing gradient pyrolysis on the precursor powder under the protection of an inert atmosphere, then acid washing the obtained product to remove metal element particles to obtain a black powder; finally, performing secondary pyrolysis on the black powder under an inert atmosphere to obtain a high-nitrogen content non-precious metal single-atom catalyst, which is applied to electrocatalytic oxygen reduction reaction, fuel cells and metal-air batteries. The preparation scheme of the present invention is simple and green, and the obtained product has a hierarchical pore structure and the single-atom metal active sites are evenly dispersed, thereby improving the catalytic activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalyst preparation, and in particular to a high-nitrogen-content non-precious metal single-atom catalyst and a preparation method and application thereof. Background Art

[0002] The increasing prominence of environmental pollution and energy shortages has stimulated the vigorous development of sustainable energy conversion and storage technologies, such as fuel cells and metal-air batteries. However, the slow kinetics of the cathode oxygen reduction reaction seriously affects the overall energy conversion efficiency of such devices. Although platinum group noble metals have excellent oxygen reduction reaction activity, these materials have disadvantages such as high price, scarce reserves and poor stability, which hinder their industrial production and application. In recent studies, it was found that transition metal composite carbon-doped materials not only exhibit good electrocatalytic oxygen reduction reaction activity, but also have low cost, good conductivity and adjustable electronic structure, which have attracted widespread attention and are considered to be one of the most promising substitutes for noble metal catalysts. Transition metal single atom catalysts have unique geometric and electronic structures, which maximize the utilization of metal atoms and have the advantages of high stability and high stability. Therefore, non-noble metal single atom catalysts are studied to improve the performance of fuel cells and metal-air batteries.

[0003] Transition metal composite nitrogen-doped carbon materials not only show good electrocatalytic oxygen reduction reaction activity, but also have low cost, good conductivity and controllable electronic structure, which have attracted widespread attention and are considered to be one of the most promising substitutes for precious metal catalysts. Such materials are usually prepared by pyrolysis of nitrogen source, carbon source and transition metal salt. However, since metal atoms are easy to migrate during pyrolysis, the metals in the prepared catalysts are mainly nanoparticles and nanoclusters. Studies have shown that the activity of the catalyst is determined by the density of active sites and their intrinsic activity, and transition metals are important components of the active sites in this type of catalyst. Therefore, the formation of particles and nanoclusters leads to a decrease in the utilization rate of metal atoms, which in turn affects the ORR activity of the catalyst. Compared with metal nanoparticles and nanocluster catalysts, single-atom catalysts have unique geometric and electronic structures, which maximize the utilization rate of atoms and have the advantages of high stability and high activity. Therefore, it is of great research value to develop non-precious metal single-atom catalysts to improve the utilization rate of non-precious metal atoms.

[0004] Existing technologies such as patent CN109841854A disclose a method of preparing a single atom catalyst by anchoring transition metals with organic ligands in metal organic framework materials; patent CN110993968A discloses a method of preparing a single metal atom catalyst by using aerogel as a precursor and silicon dioxide as a pore-forming agent.

[0005] Patent CN109841854A uses metal organic framework materials to prepare single atom catalysts with mainly micropores, which affects the transmission of electrolytes during the reaction. Moreover, the preparation and use costs of organic ligands in this preparation method are high, which is not conducive to large-scale production. Patent CN110993968A uses silicon dioxide as a pore-forming agent, and toxic acid and alkali reagents are needed to remove the silicon template in subsequent experiments, which causes great environmental pollution. Summary of the invention

[0006] In order to solve the shortcomings of the prior art, such as the complicated preparation and high cost of precursor raw materials, the complicated treatment of pore-forming agents, and the pollution and harmfulness, the present invention provides a high-nitrogen-content non-precious metal single-atom catalyst and its preparation method and application. The present invention uses green, easily available, low-cost materials (urea, glucose, sodium chloride, etc.) to prepare metal single-atom catalysts, and the pore-forming agent used in the experiment is sodium chloride, which can be removed by direct water washing and filtration, and the sodium chloride can also be recycled and reused, which has the advantages of low cost and environmental friendliness.

[0007] The specific technical scheme of the present invention is: a method for preparing a high nitrogen content non-precious metal single atom catalyst, which mainly comprises the following steps:

[0008] (1) Add a nitrogen source, a carbon source and a non-precious metal salt to a solvent and dissolve them evenly, then add an excess salt template to obtain a mixed solution; blend the precursor with the salt so that the sodium chloride and the precursor are repeatedly mixed evenly. The mass ratio of the nitrogen source to the carbon source is 1:0.1-0.4; the mass ratio of the nitrogen source to the non-precious metal salt is 1:0.025-0.25; in the present invention, the mass ratio of the nitrogen source, the carbon source, the non-precious metal salt and the sodium chloride should be well controlled. When a certain content is too much or too little, it will affect the carbon-based structure, pore structure, metal atom distribution and the formation of doped nitrogen of the catalyst.

[0009] (2) The mixed solution is heated at 90-150° C. for 4-6 h. During this process, the glucose dehydration product in the precursor reacts with urea to form a Schiff base to form a stable cobalt ligand, which inhibits the decomposition of urea during the thermal decomposition process and inhibits the aggregation of cobalt.

[0010] (3) Freezing the precursor solution at -60 to -50°C and then freeze-drying; the freeze-drying process inhibits the decomposition of the precursor due to heat, thereby affecting the product structure;

[0011] (4) Preliminary gradient pyrolysis of the precursor powder in an inert gas to obtain a primary pyrolysis product. The design of the intermediate step of pyrolysis is conducive to the thermal polymerization of urea molecules in the precursor, improving the thermal stability of the precursor, thereby retaining more single atoms, which is beneficial to increasing the nitrogen content in the catalyst on the one hand, and providing more sites for the anchoring of cobalt atoms on the other hand. Based on this design, a metal single atom-loaded nitrogen-doped carbon catalyst is obtained;

[0012] (5) The primary pyrolysis product is placed in an oil bath in a dilute sulfuric acid environment to remove unstable metal nanoparticles, filtered, and dried to obtain a powder; during the pyrolysis process, the surface energy of the metal atoms is too high, and some metal nanoparticles are still produced, encapsulating some ORR active (MN x ) metal sites, so it is necessary to use acid to remove the metal nanoparticles, which is beneficial to the exposure of the metal active sites, and the acid solution will corrode the carbon layer and produce some defects. After comparing the effects of other acidic solutions in removing unstable cobalt compounds, it is found that dilute sulfuric acid is the best.

[0013] (6) The powder obtained in step (5) is subjected to secondary pyrolysis in an inert gas to remove the cobalt oxidized during the acid washing process and the excess oxygen-containing functional groups in the carbon carrier, thereby increasing the conductivity of the catalyst and obtaining a high nitrogen content non-precious metal single atom catalyst.

[0014] In the process of preparing the catalyst of the present invention, firstly, cobalt salt, nitrogen source and carbon source are added to a certain amount of deionized water in a certain proportion and mixed evenly, and then an excess salt template is added thereto to obtain a preliminary mixed solution, and then an oil bath reflux is performed. The purpose of oil bath reflux is to allow the raw materials to be evenly mixed and coated on the surface of the salt template. Adding salt template sodium chloride to the mixed solution not only provides a template, but also plays a structural guiding role. Since metal single atoms have higher surface energy during pyrolysis, isolated atoms tend to aggregate into metal nanoparticles that are more thermodynamically stable. Adding the salt template allows the precursor to be adsorbed on the salt template, which plays a spatial confinement role, inhibits the movement of metal atoms, and reduces the generation of metal nanoparticles. In addition, the salt template can serve as a protective layer during the pyrolysis process to reduce the evaporation of doping element nitrogen.

[0015] The precursor solution after the oil bath is placed in a freeze dryer to remove water molecules and obtain powder. Compared with the direct drying method by heating, freeze drying can protect the morphology and structure of the precursor. Gradient heat treatment is carried out under an inert atmosphere. The pyrolysis heating rate will affect the pore structure size of the catalyst. The low temperature stage is to allow the nitrogen source to generate graphite-like carbon nitride, and the high temperature stage is the decomposition of graphite-like carbon nitride, providing some anchoring points for better loading of non-precious metal atoms on the carbon base.

[0016] The purpose of acid washing the primary pyrolysis product is to remove some unstable metal nanoparticles and prevent some useful ORR active sites from being wrapped by metal and losing their activity. However, some defects will be produced after acid washing, which will affect the conductivity of the catalyst. Therefore, the acid washed sample is subjected to secondary pyrolysis to increase the graphitization degree of the catalyst, thereby improving the ORR performance.

[0017] Preferably, in step (1), the salt template is sodium chloride, and the solvent is deionized water; the concentration of the salt template sodium chloride is 0.2 to 0.5 g·mL -1 ; The carbon source is one or more of glucose, starch and cellulose; the nitrogen source is one or more of urea, dicyandiamide and melamine; the non-precious metal salt is one of cobalt salt, iron salt, manganese salt, nickel salt and copper salt.

[0018] In the present invention, the salt template mainly uses sodium chloride or potassium chloride. Compared with other hard templates (such as porous silicon and silicon dioxide, etc.), the removal of the salt template only requires water washing and filtration, and there is no need to use toxic hydrofluoric acid or sodium hydroxide and other complex template removal methods to remove the silicon template; while the preparation process of the soft template itself is complicated and the structural stability of the template is poor. Another important reason for using salt template sodium chloride or potassium chloride is that it can be recycled and reused.

[0019] Preferably, in step (2), the heating method is oil bath heating; in step (2), the inert gas is nitrogen or argon; in step (6), the inert gas is nitrogen or argon.

[0020] The oil bath temperature will affect the degree of precursor prepolymerization. If the temperature is too low, the carbon source cannot be dehydrated to form carbonyl groups, and the carbon source and nitrogen source cannot be prepolymerized. If the temperature is too high, the carbon source will be dehydrated and carbonized, and the nitrogen source will be unstable and volatilize, which will affect the formation of nitrogen-doped carbon materials in subsequent experiments.

[0021] Preferably, in step (4), the preliminary gradient pyrolysis step comprises: heating at 2-10°C·min -1 The heating rate is raised to 350-550℃, kept at this temperature for 0.5-2h, and then heated at 2-10℃·min -1 The heating rate is raised to 700-900°C and kept at this temperature for 1-3 hours; in step (6), the secondary pyrolysis step comprises: heating at a rate of 2-10°C·min -1 The heating rate is increased to 700-900°C and kept warm for 0.5-2h.

[0022] During the low-temperature pyrolysis of the precursor powder, the nitrogen source is mainly converted into graphite-phase carbon nitride, which produces some defects that can be used for metal single atom anchoring. During the high-temperature pyrolysis process, the heating temperature is raised to 700-900 ℃ The graphite carbon nitride produced in the previous stage decomposes, and the metal ions are reduced to metal atoms by the carbon source and adsorbed on the doped nitrogen, generating a precursor of a uniform mixture of transition metal and carbon. The secondary pyrolysis increases the graphitization degree of the carbon matrix, which is more conducive to the adsorption of oxygen and electron transport in the ORR reaction.

[0023] The present invention also provides a high nitrogen content non-precious metal single-atom catalyst prepared by the preparation method of any of the above-mentioned high nitrogen content non-precious metal single-atom catalysts, characterized in that the metal element in the high nitrogen content non-precious metal single-atom catalyst is anchored on the carbon carrier in the form of a single atom; the nitrogen content is 9.5-10.0at%.

[0024] Preferably, the high nitrogen content non-precious metal single atom catalyst is a porous structure with a specific surface area of ​​620-630m 2 -1g.

[0025] The catalytic activity of the high nitrogen content catalyst is better than that of the low nitrogen content catalyst of the same structure. The nitrogen content of the high nitrogen content catalyst prepared by the present invention is as high as 9.0-10.0 at.%. The single atom catalyst realizes the maximum utilization of transition metal atoms, because transition metals are the catalytic active sites of this type of catalyst, and reducing the size of transition metal particles can maximize the metal utilization rate, and has a higher specific activity under the same metal loading conditions; the hierarchical pore structure provides a channel for the diffusion of reactants and products, and improves the catalyst surface reaction kinetics. In order to achieve the above advantages, sodium chloride is used as a soluble template, which, on the one hand, inhibits the agglomeration of carbon layers during pyrolysis; in addition, since the precursor is coated on the surface of sodium chloride crystals after freeze-drying, the presence of sodium chloride inhibits the agglomeration of cobalt and the decomposition of nitrogen during pyrolysis, thereby ensuring the synthesis of the catalyst.

[0026] The present invention also provides a method for preparing the above-mentioned high-nitrogen-content non-precious metal single-atom catalyst. The prepared high-nitrogen-content non-precious metal single-atom catalyst is applied to electrocatalytic oxygen reduction reaction, fuel cell and metal-air battery.

[0027] The present invention dopes the carbon matrix with nitrogen atoms, and forms a porous carbon material with a high nitrogen content after pyrolysis. The doping of nitrogen atoms changes the electronic and spin structure of the carbon material, optimizes the adsorption of oxygen molecules during the oxygen reduction process, reduces the overpotential of the oxygen reduction reaction, and solves the problem of low catalytic activity. At the same time, due to the confinement effect and structural guidance of the salt template, the prepared catalyst has a hierarchical pore structure and the single-atom metal active sites are evenly dispersed, which together improve the oxygen reduction reaction activity of the catalyst.

[0028] Compared with the prior art, the beneficial effects of the present invention are:

[0029] (1) The present invention solves the problem of low catalytic activity. The prepared catalyst has a hierarchical pore structure and uniformly dispersed single-atom metal active sites, which together improve the catalyst's oxygen reduction reaction activity.

[0030] (2) The raw materials required by the present invention are cheap and easily available, and the salt template can be reused; the metal elements in the catalyst are mainly anchored on the carbon carrier in the form of single atoms, which greatly improves the utilization rate of the metal elements; the preparation process is simple and the operation is simple, which is a low-cost green preparation method.

[0031] (3) The present invention uses sodium chloride as a pore-forming agent, and the decomposition and evaporation of urea during the pyrolysis process make the catalyst have a rich pore structure and a large specific surface area. The pore size exhibits a graded pore structure, which is not only conducive to the formation of a large number of active sites, but also conducive to the diffusion of reactants / products in the electrolyte, thereby improving the catalyst activity. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a scanning electron microscope image of the catalyst prepared in Example 1 of the present invention;

[0033] Figure 2 This is a scanning electron microscope image of the catalyst prepared in Example 2 of the present invention;

[0034] Figure 3 This is a scanning electron microscope image of the catalyst prepared in Example 3 of the present invention;

[0035] Figure 4 This is the X-ray diffraction pattern of the catalyst prepared in Example 1 of the present invention;

[0036] Figure 5 This is a transmission electron microscopy image of the catalyst prepared in Example 1 of the present invention;

[0037] Figure 6 A high-resolution transmission electron microscopy image of the catalyst prepared in Example 1 of the present invention and a distribution map of its Co, N and C elements;

[0038] Figure 7 This is a graph showing the oxygen reduction activity of the catalysts prepared in Examples 1-3 of the present invention and a commercial Pt / C catalyst. DETAILED DESCRIPTION

[0039] The present invention is further described below in conjunction with the examples. The devices, reagents and methods involved in the present invention are all known in the art unless otherwise specified.

[0040] General Example: A method for preparing a high nitrogen content non-precious metal single atom catalyst using a salt template, comprising the following preparation steps:

[0041] (1) Add a nitrogen source, a carbon source and a non-precious metal salt into deionized water and dissolve them evenly, then add an excess salt template to obtain a mixed solution; the carbon source includes one or more of glucose, starch and cellulose; the nitrogen source includes one or more of urea, dicyandiamide and melamine; the non-precious metal salt includes one of cobalt salt, iron salt, manganese salt, nickel salt and copper salt; the salt template is sodium chloride. The mass ratio of the nitrogen source to the carbon source is 1:0.1-0.4; the mass ratio of the nitrogen source to the non-precious metal salt is 1:0.025-0.25; the concentration of the salt template sodium chloride is 0.2-0.5 g·mL-1;

[0042] (2) placing the mixed solution in an oil bath at 90-150° C. for 4-6 hours to obtain a precursor solution;

[0043] (3) freezing the precursor solution at -60 to -50°C and freeze-drying it under vacuum to obtain a precursor powder;

[0044] (4) The precursor powder is subjected to a preliminary gradient pyrolysis in a tube furnace with a nitrogen or argon atmosphere at a temperature of 2 to 10 °C min -1 The heating rate is from room temperature to 350-550℃, kept at this temperature for 0.5-2h, and then heated at 2-10℃·min -1 The heating rate is raised to 700-900°C and kept at this temperature for 1-3 hours. A metal single atom-supported nitrogen-doped carbon catalyst is obtained;

[0045] (5) removing metal nanoparticles from the primary pyrolysis product in an oil bath under a dilute sulfuric acid environment, filtering, and drying to obtain a black powder;

[0046] (6) The black powder is subjected to secondary pyrolysis in a tubular furnace with a nitrogen or argon atmosphere at a temperature of 2 to 10 °C min -1 The heating rate is increased from room temperature to 700-900°C and kept warm for 0.5-2h to obtain a non-precious metal single atom catalyst.

[0047] Embodiment 1:

[0048] 0.25g of cobalt chloride hexahydrate, 2g of urea and 0.5g of glucose were added to deionized water and stirred to dissolve evenly. Then, an excess of sodium chloride was added and stirred evenly. Then, an oil bath reflux reaction was carried out at 150°C for 5h. After cooling to room temperature, the oil bath product was freeze-dried. After freeze-drying, the product was subjected to gradient pyrolysis in a tube furnace with an argon atmosphere. The product was first heated at 5°C·min -1 The heating rate was from room temperature to 500°C, and the temperature was kept for 1 h; then the temperature was increased at 2°C·min -1The heating rate was raised to 800 °C and kept at this temperature for 1 h. The primary pyrolysis product was washed with deionized water, filtered three times, and then dried to remove the sodium chloride salt template. The metal nanoparticles were washed with 0.5 M dilute sulfuric acid in an 80 °C oil bath environment, filtered, washed to neutrality, and dried. Finally, a secondary pyrolysis treatment was carried out in a tubular furnace with an argon atmosphere at 5 °C min -1 The heating rate was increased to 800°C and kept at that temperature for 1 hour to prepare a nitrogen-doped carbon-based metal single atom catalyst.

[0049] Embodiment 2:

[0050] The specific steps are the same as those in Example 1, except that the initial pyrolysis condition is reduced to 2°C·min -1 The heating rate was increased to 500°C.

[0051] Embodiment 3:

[0052] The specific steps are the same as those in Example 1, except that the initial pyrolysis condition is increased to 10 °C·min -1 The heating rate was increased to 500°C.

[0053] Embodiment 4:

[0054] The specific steps are the same as those in Example 1, except that the oil bath temperature is 90°C.

[0055] Embodiment 5:

[0056] The specific steps are the same as those in Example 1, except that the oil bath temperature is 120°C.

[0057] Embodiment 6:

[0058] The specific steps are the same as those in Example 1, except that the amount of cobalt salt added is 0.15 g.

[0059] Embodiment 7:

[0060] The specific steps are the same as those in Example 1, except that the amount of cobalt salt added is 0.35 g.

[0061] Comparative Example 1:

[0062] The specific steps are the same as those in Example 1, except that the heating in the oil bath for 5 h is replaced by magnetic stirring at room temperature for 5 h.

[0063] Comparative Example 2:

[0064] The specific steps are the same as those in Example 1, except that the salt template sodium chloride is not added.

[0065] The catalysts prepared in the examples and comparative examples were tested for performance, morphology and oxygen reduction activity. The morphology of the catalysts was mainly characterized by scanning electron microscopy and transmission electron microscopy; the oxygen reduction activity test method was as follows: a three-electrode system (graphite rod as counter electrode, saturated calomel as counter electrode and catalyst slurry coated on the surface of a rotating disk electrode as a working electrode) was used, and the catalyst oxygen reduction activity curve was measured in an oxygen-saturated 0.1M KOH solution, with the rotating disk electrode speed set to 1600rpm and the scanning rate set to 5mV·s-1.

[0066] Figure 1 This is a scanning electron microscope image of the catalyst prepared in Example 1. It can be seen from the image that the catalyst exhibits a porous flocculent structure. Figure 2 This is a scanning electron microscope image of the catalyst prepared in Example 2. It can be seen from the image that the catalyst presents a wrinkled structure with smaller pores.

[0067] Figure 3 This is a scanning electron microscope image of the catalyst prepared in Example 3. It can be seen from the image that the catalyst presents a relatively large block structure.

[0068] Figure 4 This is the X-ray diffraction diagram of the catalyst prepared in Example 1. It can be seen from the diagram that the diffraction peak of the metal Co used in the example is basically undetectable in the prepared catalyst.

[0069] Figure 5 This is a transmission electron microscopy image of the catalyst prepared in Example 1. It can be seen from the image that no metal particles are detected.

[0070] Figure 6 The high-resolution transmission electron micrograph of the catalyst prepared in Example 1 of the present invention and the distribution diagram of its CO, N and C elements are shown. The high-nitrogen-content non-precious metal single-atom catalyst prepared using a salt template in Example 1 contains cobalt, nitrogen and carbon elements, and each element is evenly distributed in the entire material.

[0071] Figure 7 This is a graph showing the oxygen reduction activity of the catalysts prepared in Examples 1-3 and a commercial Pt / C catalyst (JM, 20%). It can be seen from the graph that the oxygen reduction activity of the catalyst prepared in Example 1 is comparable to that of the commercial Pt / C catalyst.

[0072] Depend on Figure 2 , 4 From the characterization test results obtained in , 5, and 6, it can be seen that the catalyst prepared using this method is a metal single atom catalyst.

[0073] The catalysts prepared in Examples 1 and 3 were subjected to X-ray photoelectron spectroscopy analysis, and the results are shown in Table 1:

[0074] Table 1

[0075] project C (at.%) N (at.%) O(at.%) Co(at.%) Example 1 83.7 10.2 5.3 0.8 Example 3 85.2 10.0 4.0 0.8

[0076] The surface element analysis results of the samples prepared in Examples 1 and 3 indicate that the non-precious metal single-atom catalyst prepared by the template method has a high content of nitrogen (the nitrogen atom content reaches more than 10 at.%), and the metal content supported by the carbon matrix is ​​also relatively high.

[0077] The catalysts prepared in the examples and comparative examples were tested for half-wave potential, and the results are shown in Table 2.

[0078] Table 2

[0079] project Half-wave potential (V vs. RHE) Limiting diffusion current density (mA·cm-2) Example 1 0.84 -6.1 Example 2 0.81 -5.6 Example 3 0.85 -4.3 Example 4 0.85 -5.0 Example 5 0.83 -4.9 Example 6 0.80 -5.3 Example 7 0.79 -5.6 Comparative Example 1 0.85 -4.5 Comparative Example 2 0.77 -3.7

[0080] The catalyst prepared in the embodiment of the present invention has good half-wave potential and good catalytic activity.

[0081] Comparative Example 1 adopts the room temperature stirring method and does not adopt the oil bath method to prepare the catalyst. The prepared catalyst presents a very obvious block particle structure, and the limiting diffusion current in the tested oxygen reduction performance is poor, so its catalytic activity is not compared and studied.

[0082] Comparative Example 2 is a catalyst prepared without adding salt template NaCl. The nitrogen content is lower than that of the salt template, which is 9.8% in Example 1 and 7.2% in the comparative example. Moreover, it is not single atom and has poor ORR performance.

[0083] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a high nitrogen content non-precious metal single atom catalyst, comprising the steps of: (1) Add nitrogen source, carbon source and non-precious metal salt in a mass ratio of 1:0.1-0.4:0.025-0.25 into deionized water as solvent and dissolve evenly, and add excess salt template 0.2-0.5 g / mL sodium chloride to prepare a mixed solution; (2) heating the mixed solution at 90-150°C for 4-6 hours to obtain a precursor solution; (3) The precursor solution is frozen at -60 to -50°C, and then freeze-dried to obtain a precursor powder; (4) Preliminary gradient pyrolysis of the precursor powder in an inert gas: 2~10℃ / min to 350~550℃, keep warm for 0.5~2h, then 2~10℃ / min to 700~900℃, keep warm for 1~3h; obtain the primary pyrolysis product; (5) The primary pyrolysis product is placed in an oil bath under dilute sulfuric acid to remove metal nanoparticles, and then filtered and dried to obtain a powder; (6) The powder is subjected to secondary pyrolysis in an inert gas: the temperature is raised to 700-900°C at 2-10°C / min and kept at this temperature for 0.5-2h to obtain a non-precious metal single-atom catalyst with a high nitrogen content.

2. The method for preparing the high nitrogen content non-precious metal single atom catalyst according to claim 1, It is characterized in that In step (1), the carbon source is one or more of glucose, starch and cellulose.

3. The method for preparing the high nitrogen content non-noble metal single atom catalyst according to claim 1, It is characterized in that In step (1), the nitrogen source is one or more of urea, dicyandiamide and melamine.

4. The method for preparing the high nitrogen content non-precious metal single atom catalyst according to claim 1, It is characterized in that In step (1), the non-precious metal salt is one of cobalt salt, iron salt, manganese salt, nickel salt and copper salt.

5. The method for preparing the high nitrogen content non-noble metal single atom catalyst according to claim 1, It is characterized in that In step (2), the heating method is oil bath heating.

6. The method for preparing the high nitrogen content non-noble metal single atom catalyst according to claim 1, It is characterized in that In step (4), the inert gas is nitrogen or argon.

7. The method for preparing the high nitrogen content non-noble metal single atom catalyst according to claim 1, It is characterized in that In step (6), the inert gas is nitrogen or argon.

8. A high nitrogen content non-precious metal single atom catalyst prepared by the preparation method of high nitrogen content non-precious metal single atom catalyst according to any one of claims 1 to 7, It is characterized in that The metal elements in the high nitrogen content non-precious metal single atom catalyst are anchored on the carbon support in the form of single atoms; the nitrogen content is 9.5-10.0 at%.

9. The high nitrogen content non-noble metal single atom catalyst as claimed in claim 8, It is characterized in that The high nitrogen content non-precious metal single atom catalyst has a porous structure and a specific surface area of ​​620-630 m 2 / g.

10. The high nitrogen content non-precious metal single atom catalyst prepared by the method for preparing the high nitrogen content non-precious metal single atom catalyst as described in any one of claims 1 to 7 is applied to electrocatalytic oxygen reduction reaction, fuel cell and metal air battery.

Citation Information

Patent Citations

  • Nitrogen-doped carbon-supported monoatomic oxygen reduction catalyst and preparation method thereof

    CN109841854A

  • Preparation method and electrocatalytic application of carbon aerogel monometal atom catalyst

    CN110993968A

  • Preparation method and application of hollow non-noble metal oxygen reduction catalyst

    CN111883783A

  • Preparation method and application of carbon tube intercalated nitrogen-doped carbon-coated cobalt particle catalyst

    CN112701303A

  • Porous nitrogen-doped carbon-based transition metal monatomic catalyst as well as preparation method and application thereof

    CN113351236A