Modified conjugated diene polymer, preparation method thereof and rubber composition containing the same
By using modified conjugated diene polymers containing N aromatic hydrocarbon compounds and S-containing aromatic hydrocarbon compounds or S-containing heterocyclic compounds in tire rubber materials, the difficulty in balancing productivity, processing performance and physical properties in the existing technology is solved. problem, achieving excellent processing performance and mechanical properties.
Patent Information
- Application Number
- CN202180006682.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-08-05
- Filing Date
- 2021-07-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-07-14
AI Technical Summary
It is difficult to improve productivity, processing performance and physical properties at the same time when preparing rubber materials for tires with the existing technology. SBR or BR polymers produced by solution polymerization have problems with wide molecular weight distribution and poor physical properties.
Modified conjugated diene polymers containing derived units from N-containing aromatic hydrocarbon compounds and S-containing aromatic hydrocarbon compounds or S-containing heterocyclic compounds are prepared through a two-step polymerization reaction, and the molecular weight distribution is controlled to be above 1.0 and less than 3.0 , increasing the contents of S, Si and N to form a rubber composition with excellent processing properties, tensile strength and viscoelastic properties.
A rubber material with narrow molecular weight distribution, excellent mechanical properties and good viscoelastic properties has been achieved, which improves the tire's wet skid resistance and rolling resistance properties and balances physical properties and productivity.
Smart Images

Figure FDA0004895931020000011 
Figure FDA0004895931020000021 
Figure FDA0004895931020000022
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority based on Korean Patent Application No. 10-2020-0098086 filed on August 5, 2020, which is incorporated herein by reference in its entirety. Technical Field
[0004] The present invention relates to a modified conjugated diene polymer having excellent processability and good tensile strength and viscoelastic properties, a preparation method thereof and a rubber composition containing the same. Background Art
[0005] According to recent demands for automobiles with low fuel consumption rates, conjugated diene-based polymers having modulation stability represented by wet skid resistance and low rolling resistance as well as excellent wear resistance and tensile properties are required as rubber materials for tires.
[0006] In order to reduce the rolling resistance of the tire, there is a method of reducing the hysteresis loss of the vulcanized rubber, and the rebound resilience, tanδ, Goodrich heat generation, etc. at 50°C to 80°C are used as evaluation indicators of the vulcanized rubber. That is, it is desirable to use a rubber material having high rebound resilience or low tanδ value or Goodrich heat generation at the above temperature.
[0007] Natural rubber, polyisoprene rubber or polybutadiene rubber are known as rubber materials with low hysteresis loss, but these rubbers have the limitation of low wet skid resistance. Therefore, recently, conjugated diene polymers or copolymers such as styrene-butadiene rubber (hereinafter referred to as "SBR") and butadiene rubber (hereinafter referred to as "BR") are prepared by emulsion polymerization or solution polymerization to be used as tire rubber. Among these polymerization methods, the biggest advantage of solution polymerization compared with emulsion polymerization is that the vinyl structure content and styrene content that specify the physical properties of the rubber can be arbitrarily adjusted, and its molecular weight and physical properties can be controlled by coupling or modification. Therefore, SBR prepared by solution polymerization is widely used as a rubber material for tires because it is easy to change the structure of the SBR or BR finally prepared, and the movement of the chain end can be reduced, and the coupling force with fillers such as silica and carbon black can be increased by coupling or modification of the chain end.
[0008] If solution-polymerized SBR is used as a rubber material for tires, since the glass transition temperature of the rubber is increased by increasing the vinyl content in the SBR, the physical properties such as the running resistance and braking force required by the tire can be controlled, and the fuel consumption can be reduced by appropriately adjusting the glass transition temperature. The solution-polymerized SBR is prepared by using an anionic polymerization initiator and is used by coupling or modifying the chain ends of the polymers thus formed using various modifiers. For example, U.S. Patent No. 4,397,994 discloses a method for coupling active anions at the ends of polymer chains, wherein the active anions at the ends of the polymer chains are obtained by polymerizing styrene-butadiene using an alkyl lithium as a monofunctional initiator in a non-polar solvent using a coupling agent such as a tin compound.
[0009] Meanwhile, the polymerization of SBR or BR can be carried out by batch or continuous polymerization. According to batch polymerization, the polymer thus prepared has narrow molecular weight distribution and the advantage from the perspective of improving physical properties, but there is the problem of low productivity and deterioration of processing properties. According to continuous polymerization, polymerization is continuously carried out, and there is the advantage of excellent productivity and improved processing properties, but there is the problem of wide molecular weight distribution and poor physical properties. Therefore, the research of improving productivity, processing properties and physical properties simultaneously in the preparation of SBR or BR is constantly needed.
[0010] Prior art literature
[0011] (Patent Document 1) US4397994A Summary of the invention
[0012] Technical issues
[0013] The present invention is designed to solve the above-mentioned problems of the prior art. The purpose of the present invention is to provide a modified conjugated diene polymer, which has excellent processing performance, good mechanical properties such as tensile strength and excellent viscoelastic properties by including derivative units from N-containing aromatic hydrocarbon compounds and derivative units from S-containing aromatic hydrocarbon compounds or derivative units from S-containing heterocyclic compounds in the molecule.
[0014] In addition, another object of the present invention is to provide a method for preparing the modified conjugated diene polymer.
[0015] Furthermore, another object of the present invention is to provide a rubber composition having excellent processability, wear resistance and rolling resistance by including the modified conjugated diene-based polymer.
[0016] Technical Solution
[0017] In order to solve the above-mentioned tasks, according to one embodiment of the present invention, the present invention provides a modified conjugated diene polymer, which comprises: repeating units derived from conjugated diene monomers; derivative units derived from N-containing aromatic hydrocarbon compounds; and derivative units derived from S-containing aromatic hydrocarbon compounds or S-containing heterocyclic compounds, and satisfies the following conditions (i) and (ii): (i) molecular weight distribution (PDI; MWD): greater than 1.0 and less than 3.0; and (ii) S content: greater than 25 ppm based on the total weight of the polymer.
[0018] In addition, the present invention provides a method for preparing the modified conjugated diene polymer, which comprises: a first polymerization reaction step, which is used to carry out a first polymerization of a first monomer and a second monomer in a hydrocarbon solvent in the presence of a polymerization initiator to prepare a first active polymer (S1); and a second polymerization reaction step, which is used to carry out a second polymerization of the first active polymer and a third monomer (S2), wherein the first monomer is a conjugated diene monomer, or a conjugated diene monomer and an aromatic vinyl monomer, the second monomer is an N-containing aromatic hydrocarbon compound, and the third monomer is an S-containing aromatic hydrocarbon compound or an S-containing heterocyclic compound.
[0019] In addition, the present invention provides a rubber composition comprising a modified conjugated diene polymer and a filler.
[0020] Beneficial Effects
[0021] The modified conjugated diene-based polymer according to the present invention contains N atoms, S atoms and Si atoms in a specific content or more in the molecule, and has the effects of showing excellent processability, good mechanical properties such as tensile properties and excellent viscoelastic properties.
[0022] In addition, the method for preparing the modified conjugated diene polymer according to the present invention includes a two-step polymerization reaction, including first polymerization of a first monomer and a second monomer, and second polymerization by adding a third monomer, to advantageously prepare a highly modified conjugated diene polymer.
[0023] Furthermore, the rubber composition according to the present invention includes the modified conjugated diene-based polymer and exhibits excellent effects of processability, wear resistance, and rolling resistance. DETAILED DESCRIPTION
[0024] Hereinafter, the present invention will be described in more detail to help understanding of the present invention.
[0025] It should be understood that the words or terms used in the description and claims of the present invention should not be interpreted as the meanings defined in commonly used dictionaries. It should also be understood that these words or terms should be interpreted as having meanings consistent with their meanings in the technical ideas of the present invention based on the inventors' ability to appropriately define the meanings of the words or terms to best illustrate the principles of the present invention.
[0026] Definition of terms
[0027] In the present invention, the term "polymer" refers to a polymer compound prepared by polymerizing monomers (whether of the same or different types). Likewise, the general term polymer includes the term homopolymer, which is usually used to refer to polymers prepared from only one type of monomer, and the term copolymer.
[0028] In the present invention, the term "monovalent hydrocarbon group" may refer to a monovalent atomic group obtained by bonding carbon and hydrogen in a monovalent alkyl group, an alkenyl group, an alkynyl group, a cycloalkyl group, a cycloalkyl group including one or more unsaturated bonds, and an aryl group, and the minimum number of carbon atoms of the substituent represented by the monovalent hydrocarbon may be determined according to the type of each substituent.
[0029] In the present invention, the term "divalent hydrocarbon group" may refer to a divalent atomic group obtained by bonding carbon and hydrogen in a divalent alkylene group, an alkenylene group, an alkynylene group, a cycloalkylene group, a cycloalkylene group including one or more unsaturated bonds, and an arylene group, and the minimum number of carbon atoms of the substituent represented by the divalent hydrocarbon may be determined according to the type of each substituent.
[0030] In the present invention, the term "alkyl" may refer to a monovalent aliphatic saturated hydrocarbon and may include straight chain alkyl groups such as methyl, ethyl, propyl and butyl, and branched chain alkyl groups such as isopropyl, sec-butyl, tert-butyl and neopentyl.
[0031] In the present invention, the term "alkenyl" may refer to a monovalent aliphatic unsaturated hydrocarbon including one or two or more double bonds.
[0032] In the present invention, the term "alkynyl" may refer to a monovalent aliphatic unsaturated hydrocarbon including one or two or more triple bonds.
[0033] In the present invention, the term "alkylene group" may refer to a divalent aliphatic saturated hydrocarbon such as methylene, ethylene, propylene and butylene.
[0034] In the present invention, the term "aryl group" may refer to a cyclic aromatic hydrocarbon and may include a monocyclic aromatic hydrocarbon in which one ring is formed and a polycyclic aromatic hydrocarbon in which two or more rings are combined.
[0035] In the present invention, the term "heterocyclic group" is obtained by substituting one or more heteroatoms for carbon atoms in a cycloalkyl or aryl group, and may refer to both heterocycloalkyl and heteroaryl groups. The heteroatom may be N, O, S or Si.
[0036] The terms "including" and "having" and their derivatives in the present invention, although these terms are specifically disclosed or not specifically disclosed, are not intended to exclude the presence of optional additional components, steps or processes. In order to avoid any uncertainty, all compositions claimed by using the term "comprising" may include optional additional additives, adjuvants or compounds, including polymers or any other materials, unless otherwise specified to the contrary. In contrast, the term "essentially consisting of" excludes those that are not necessary for operation, and excludes optional other components, steps or processes from the scope of the optional continuous description. The term "consisting of" excludes optional components, steps or processes that are not specifically described or illustrated.
[0037] Measurement methods and conditions
[0038] In the present invention, "weight average molecular weight (Mw)" and "number average molecular weight (Mn)" are measured by gel permeation chromatography (GPC) analysis. Molecular weight distribution (PDI, MWD, Mw / Mn) is calculated from each measured molecular weight. In particular, GPC uses two PLgel Olexis (Polymer Laboratories) columns and one PLgel mixed-C (Polymer Laboratories) column in combination, polystyrene (PS) is used as a GPC standard substance for calculating molecular weight, and tetrahydrofuran mixed with 2 wt% of an amine compound is used as a GPC measurement solvent.
[0039] In the present invention, inductively coupled plasma optical emission spectrometry (ICP-OES; Optima 7300DV) is used as an ICP analysis method to measure "Si content". If inductively coupled plasma optical emission spectrometry is used, the measurement is performed by adding about 0.7 g of the sample to a platinum (Pt) crucible, adding about 1 mL of concentrated sulfuric acid (98 wt %, electronic grade) thereto, heating at 300° C. for 3 hours, and incinerating the sample in an electric furnace (Thermo Scientific, Lindberg Blue M) according to the procedure of steps 1 to 3 below:
[0040] 1) Step 1: initial temperature 0°C, rate (temperature / hour) 180°C / hour, temperature (holding time) 180°C (1 hour);
[0041] 2) Step 2: initial temperature 180°C, rate (temperature / hour) 85°C / hour, temperature (holding time) 370°C (2 hours); and
[0042] 3) Step 3: initial temperature 370°C, rate (temperature / hour) 47°C / hour, temperature (holding time) 510°C (3 hours),
[0043] Add 1 mL of concentrated nitric acid (48 wt %) and 20 μl of concentrated hydrofluoric acid (50 wt %) to the residue, seal the platinum crucible and shake for more than 30 minutes, add 1 mL of boric acid to the sample, store at 0°C for more than 2 hours, dilute in 30 ml of ultrapure water, and incinerate.
[0044] In the present invention, "N content" can be obtained by measuring N content by NSX analysis, and NSX analysis can be measured using a trace nitrogen quantitative analyzer (NSX-2100H). For example, when using a trace nitrogen quantitative analyzer, turn on the trace nitrogen quantitative analyzer (autosampler, horizontal furnace, PMT & Nitrogen detector), set the carrier gas flow rate to 250ml / min for Ar, 350ml / min for O2, and 300ml / min for the ozone generator, set the heater to 800°C, and place the analyzer for about 3 hours to stabilize. After stabilizing the analyzer, use a nitrogen standard (AccuStandard S-22750-01 to 5ml) to make a calibration curve with a calibration curve range of 5ppm, 10ppm, 50ppm, 100ppm and 500ppm, and obtain the area corresponding to each concentration. Then, a straight line is drawn by using the ratio of concentration to area. After that, a ceramic boat containing 20mg of sample is placed in the autosampler of the analyzer and measured to obtain the area. By using the sample area thus obtained and the calibration curve, the N content is calculated. In this case, the sample is a modified conjugated diene-based polymer from which the solvent is removed by placing the sample in hot water heated by steam and stirring, and may be a sample from which residual monomers, residual modifiers, and oil are removed.
[0045] In the present invention, "S content" is measured by a combustion ion chromatography (C-IC) analysis method, and the combustion ion chromatography analysis is measured using ICS2100 / AQF-2100H. Specifically, the combustion ion chromatography uses IonPac AS18 (4×250 mm) as a column and a suppressed conductivity detector as a detector, the supply current is set to 76 mA, and the solvent is set so that 30.05 mM KOH is injected at a flow rate of 1 ml / min. The combustion temperature is set so that the inlet is 900°C, the outlet is 1,000°C, and the carrier gas flow rate is 200 ml / min for Ar gas and 400 ml / min for O2 gas. After stabilizing the analyzer, the standard material (ERM-EC680K or ERM-EC681M) is analyzed to make a calibration curve. After that, the boat containing 50 mg of the sample was burned and passed through an aqueous solution containing an absorbent (H2O2 900 mg / kg) to dilute to a final volume of 10 ml, 100 μl of the diluted sample was collected and passed through the analyzer, and the S content was calculated using the calibration curve of the standard substance.
[0046] Modified conjugated diene polymers
[0047] The invention provides a modified conjugated diene polymer, which has excellent processing performance and excellent tensile properties and viscoelastic properties.
[0048] The modified conjugated diene polymer according to one embodiment of the present invention is characterized in that it comprises: a repeating unit derived from a conjugated diene monomer; a derivative unit derived from an N-containing aromatic hydrocarbon compound; and a derivative unit derived from an S-containing aromatic hydrocarbon compound or an S-containing heterocyclic compound, and satisfies the following conditions (i) and (ii):
[0049] (i) molecular weight distribution (PDI; MWD): 1.0 or more and less than 3.0; and
[0050] (ii) S content: 25 ppm or more based on the total weight of the polymer.
[0051] According to one embodiment of the present invention, the modified conjugated diene polymer includes repeating units derived from conjugated diene monomers, derivative units from N-containing aromatic hydrocarbon compounds and derivative units from S-containing aromatic hydrocarbon compounds or derivative units from S-containing heterocyclic compounds, wherein the repeating units derived from conjugated diene monomers may refer to repeating units formed by conjugated diene monomers during the polymerization process.
[0052] In addition, each of the N-containing aromatic hydrocarbon compound, the S-containing aromatic hydrocarbon compound and the S-containing heterocyclic compound may be a modified monomer, which may be polymerized together with the conjugated diene monomer to form a polymer chain and introduce a functional group into the polymer chain, and each of the derivative unit from the N-containing aromatic hydrocarbon compound, the derivative unit from the S-containing aromatic hydrocarbon compound and the derivative unit from the S-containing heterocyclic compound may refer to a functional group derived from each compound present in the polymer chain during the polymerization of each compound.
[0053] In another embodiment, the unit derived from the N-containing aromatic hydrocarbon compound may exist in the polymer chain including the repeating unit derived from the conjugated diene-based monomer, or may exist in at least one terminal of the polymer chain.
[0054] Furthermore, a unit derived from a S-containing aromatic hydrocarbon compound or a unit derived from a S-containing heterocyclic compound may be present in the polymer chain including the repeating unit derived from the conjugated diene-based monomer, or at one terminal thereof.
[0055] In another embodiment, the modified conjugated diene polymer may further include a functional group derived from an aminoalkoxysilane modifier, and in this case, the modified conjugated diene polymer includes repeating units derived from a conjugated diene monomer, a derivative unit from an N-containing aromatic hydrocarbon compound, a derivative unit from an S-containing aromatic hydrocarbon compound, or a derivative unit from an S-containing heterocyclic compound, and may also include a functional group derived from an aminoalkoxysilane modifier.
[0056] In addition, in the case where the modified conjugated diene polymer includes a functional group derived from a modifier, the derivative unit from the N-containing aromatic compound may be present in the polymer chain comprising the repeating unit derived from the conjugated diene monomer or at one end thereof, the derivative unit from the S-containing aromatic compound or the derivative unit from the S-containing heterocyclic compound may be present in the polymer chain, and the functional group derived from the modifier may be present at the other end of the polymer chain. That is, the modified conjugated diene polymer according to an embodiment of the present invention may be a double-terminal modified conjugated diene polymer with both ends modified. In this case, the modified conjugated diene polymer according to an embodiment of the present invention includes N atoms with better affinity to the filler at both ends, and the affinity to the filler can be further improved, and as a result, the effect of better processing performance, mechanical properties and viscoelastic properties can be shown.
[0057] In addition, according to another embodiment of the present invention, the modified conjugated diene polymer may also include repeating units derived from aromatic vinyl monomers, and in this case, the modified conjugated diene polymer may include repeating units derived from conjugated diene monomers, repeating units derived from aromatic vinyl monomers, derived units from N-containing aromatic hydrocarbon compounds, and derived units from S-containing aromatic hydrocarbon compounds or S-containing heterocyclic compounds, and further include functional groups derived from modifiers as needed. Here, the repeating units derived from aromatic vinyl monomers refer to repeating units formed by aromatic vinyl monomers during polymerization.
[0058] According to one embodiment of the present invention, the conjugated diene monomer may be one or more selected from the group consisting of 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, piperylene, 3-butyl-1,3-octadiene, isoprene, 2-phenyl-1,3-butadiene and 2-halogeno-1,3-butadiene (halogen refers to a halogen atom).
[0059] As the aromatic vinyl monomer, for example, one or more selected from the group consisting of styrene, α-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 1-vinylnaphthalene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene, 1-vinyl-5-hexylnaphthalene, 3-(2-pyrrolidinylethyl)styrene, 4-(2-pyrrolidinylethyl)styrene and 3-(2-pyrrolidinyl-1-methylethyl)-α-methylstyrene.
[0060] In another embodiment, the modified conjugated diene polymer can be a copolymer, which further includes a repeating unit derived from a diene monomer having 1 to 10 carbon atoms and a repeating unit derived from a conjugated diene monomer. The repeating unit derived from the diene monomer can be a repeating unit derived from a diene monomer different from the conjugated diene monomer, and the diene monomer different from the conjugated diene monomer can be, for example, 1,2-butadiene. If the modified conjugated diene polymer is a copolymer further including a diene monomer, the modified conjugated diene polymer can include more than 0 wt % to 1 wt %, more than 0 wt % to 0.1 wt %, more than 0 wt % to 0.01 wt %, or more than 0 wt % to 0.001 wt % of the repeating unit derived from the diene monomer, and within this range, the effect of preventing gel formation can be achieved.
[0061] According to one embodiment of the present invention, the copolymer may be a random copolymer, and in this case, an excellent balance effect between physical properties may be exhibited. The random copolymer may refer to that repeating units forming the copolymer are arranged in a disordered manner.
[0062] The modified conjugated diene polymer according to one embodiment of the present invention may satisfy a molecular weight distribution (PDI; MWD) of 1.0 or more and less than 3.0, particularly 1.1 or more and less than 2.0, or 1.1 or more and 1.7 or less. Within this range, an excellent rolling resistance and wet skid resistance and a balanced effect between physical properties can be achieved.
[0063] In addition, the modified conjugated diene-based polymer may have a number average molecular weight (Mn) of 1,000 g / mol to 2,000,000 g / mol, 10,000 g / mol to 1,000,000 g / mol, or 100,000 g / mol to 800,000 g / mol, a weight average molecular weight (Mw) of 1,000 g / mol to 3,000,000 g / mol, 10,000 g / mol to 2,000,000 g / mol, or 100,000 g / mol to 2,000,000 g / mol, and a peak average molecular weight (Mp) of 1,000 g / mol to 3,000,000 g / mol, 10,000 g / mol to 2,000,000 g / mol, or 100,000 g / mol to 2,000,000 g / mol.
[0064] In another embodiment, the modified conjugated diene polymer can satisfy the molecular weight distribution curve of unimodal shape by gel permeation chromatography (GPC). This is the molecular weight distribution curve shown in the polymer polymerized by continuous polymerization, and may mean that the modified conjugated diene polymer has uniform performance. That is, the modified conjugated diene polymer according to the embodiment of the present invention can be prepared by continuous polymerization and can have the molecular weight distribution curve of unimodal shape and the molecular weight distribution of more than 1.0 and less than 3.0.
[0065] In addition, the modified conjugated diene polymer satisfies an S content of 25 ppm or more, 25 ppm to 2,000 ppm, or 100 ppm to 1,000 ppm based on the total weight of the polymer, and within this range, the mechanical properties of the modified conjugated diene polymer, such as tensile properties, may be even better. Meanwhile, the S content in the polymer refers to the content of S atoms, and the S atoms and their content may be derived from S-containing aromatic hydrocarbon compounds or S-containing heterocyclic compounds.
[0066] In another embodiment, based on the total weight of the polymer, the Si content and N content of the modified conjugated diene polymer can be 50ppm or more, 100ppm or more, 100ppm to 500ppm or 100ppm to 300ppm, respectively, and within this range, the excellent effect of mechanical properties (such as tensile properties and viscoelastic properties) of the rubber composition including the modified conjugated diene polymer can be achieved. At the same time, the Si content and N content in the polymer refer to the content of Si atoms and N atoms present in the polymer, respectively, and the Si atoms and their content can be derived from the modifier, and the N atoms and their content can be derived from the N-containing aromatic hydrocarbon compound and the modifier.
[0067] In another embodiment, the modified conjugated diene-based polymer may have a measured Mooney stress relaxation rate of 0.5 or more, 0.5 to 3.0, 0.5 to 2.5, or 0.5 to 2.0.
[0068] Here, the Mooney stress relaxation rate represents the stress change shown as a response to the same amount of strain, and can be measured using a Mooney viscometer. Specifically, the Mooney stress relaxation rate is obtained by using Monsanto's MV2000E using a Large Rotor at a rotor speed of 2±0.02rpm at 100°C. The polymer used is placed at room temperature (23±5°C) for more than 30 minutes, 27±3g of the sample is taken out, placed in the mold cavity, the platen is operated, and then, the Mooney viscosity is measured while applying torque. Then, the slope value of the Mooney viscosity change shown when the torque is released is measured, and the Mooney stress relaxation rate is obtained.
[0069] Meanwhile, the Mooney stress relaxation rate can be used as an indicator of the branched structure of the corresponding polymer, and can be used as an indicator of the degree of branching because, for example, if polymers having the same Mooney viscosity are compared, the Mooney relaxation rate decreases as the branching increases.
[0070] In addition, the Mooney viscosity of the modified conjugated diene-based polymer at 100° C. may be 30 or more, 40 to 150, or 40 to 140, and within this range, the effects of excellent processability and productivity may be achieved.
[0071] In addition, the modified conjugated diene polymer may have a vinyl content of 5% by weight or more, 10% by weight or more, or 10% by weight to 60% by weight. Here, the vinyl content may refer to the content of the conjugated diene monomer that is not 1,4-added but 1,2-added based on 100% by weight of the conjugated diene copolymer composed of the monomer having the vinyl group and the aromatic vinyl monomer.
[0072] Meanwhile, the N-containing aromatic hydrocarbon compound according to an embodiment of the present invention may be a compound represented by the following Formula 1, and may be polymerized with a monomer to introduce a functional group into a polymer chain when the polymer chain is formed.
[0073] [Formula 1]
[0074]
[0075] In formula 1,
[0076] R 1a To R 1c each independently represents a hydrogen atom; an alkyl group of 1 to 20 carbon atoms; an alkenyl group of 2 to 20 carbon atoms; an alkynyl group of 2 to 20 carbon atoms; a heteroalkyl group of 1 to 20 carbon atoms, a heteroalkenyl group of 2 to 20 carbon atoms; a heteroalkynyl group of 2 to 20 carbon atoms; a cycloalkyl group of 5 to 20 carbon atoms; an aryl group of 6 to 20 carbon atoms; or a heterocyclyl group of 3 to 20 carbon atoms,
[0077] R 1d is a single bond, an alkylene group of 1 to 20 carbon atoms which may be substituted or unsubstituted; a cycloalkylene group of 5 to 20 carbon atoms which may be substituted or unsubstituted; or an arylene group of 6 to 20 carbon atoms which may be substituted or unsubstituted, wherein the substituent is an alkyl group of 1 to 10 carbon atoms, a cycloalkyl group of 5 to 10 carbon atoms, or an aryl group of 6 to 20 carbon atoms, and
[0078] R 1e is an alkyl group of 1 to 20 carbon atoms; an alkenyl group of 2 to 20 carbon atoms; an alkynyl group of 2 to 20 carbon atoms; a heteroalkyl group of 1 to 20 carbon atoms; a heteroalkenyl group of 2 to 20 carbon atoms; a heteroalkynyl group of 2 to 20 carbon atoms; a cycloalkyl group of 5 to 20 carbon atoms; an aryl group of 6 to 20 carbon atoms; a heterocyclic group of 3 to 20 carbon atoms; or a substituent represented by the following formula 1a:
[0079] [Formula 1a]
[0080]
[0081] In formula 1a,
[0082] R 1f is a single bond, an alkylene group of 1 to 20 carbon atoms which may be substituted or unsubstituted; a cycloalkylene group of 5 to 20 carbon atoms which may be substituted or unsubstituted; or an arylene group of 6 to 20 carbon atoms which may be substituted or unsubstituted, wherein the substituent is an alkyl group of 1 to 10 carbon atoms, a cycloalkyl group of 5 to 10 carbon atoms, or an aryl group of 6 to 20 carbon atoms, and
[0083] R1g and R 1h each independently represents an alkyl group of 1 to 20 carbon atoms; an alkenyl group of 2 to 20 carbon atoms; an alkynyl group of 2 to 20 carbon atoms; a heteroalkyl group of 1 to 20 carbon atoms; a heteroalkenyl group of 2 to 20 carbon atoms; a heteroalkynyl group of 2 to 20 carbon atoms; a cycloalkyl group of 5 to 20 carbon atoms; an aryl group of 6 to 20 carbon atoms; a heterocyclyl group of 3 to 20 carbon atoms; or a mono-, di- or tri-substituted alkylsilyl group substituted with an alkyl group of 1 to 10 carbon atoms, or R 1g and R 1h They are connected to each other to form, together with N, a heterocyclic group of 2 to 10 carbon atoms substituted with an alkyl group of 1 to 10 carbon atoms or having no substituent.
[0084] In particular, in Formula 1, R 1a To R 1c R may be each independently a hydrogen atom; an alkyl group of 1 to 10 carbon atoms; an alkenyl group of 2 to 10 carbon atoms; an alkynyl group of 2 to 10 carbon atoms; a heteroalkyl group of 1 to 10 carbon atoms, a heteroalkenyl group of 2 to 10 carbon atoms; a heteroalkynyl group of 2 to 10 carbon atoms; a cycloalkyl group of 5 to 10 carbon atoms; an aryl group of 6 to 10 carbon atoms; or a heterocyclic group of 3 to 10 carbon atoms, R 1d It may be a single bond or an unsubstituted alkylene group of 1 to 10 carbon atoms, R 1e It may be an alkyl group of 1 to 10 carbon atoms; an alkenyl group of 2 to 10 carbon atoms; an alkynyl group of 2 to 10 carbon atoms; a heteroalkyl group of 1 to 10 carbon atoms; a heteroalkenyl group of 2 to 10 carbon atoms; a heteroalkynyl group of 2 to 10 carbon atoms; a cycloalkyl group of 5 to 10 carbon atoms; an aryl group of 6 to 10 carbon atoms; a heterocyclic group of 3 to 10 carbon atoms; or a substituent represented by Formula 1a. In Formula 1a, R 1f It may be a single bond or an unsubstituted alkylene group of 1 to 10 carbon atoms, R 1g and R 1h Each of the above may be independently an alkyl group having 1 to 10 carbon atoms; an alkenyl group having 2 to 10 carbon atoms; an alkynyl group having 2 to 10 carbon atoms; a heteroalkyl group having 1 to 10 carbon atoms; a heteroalkenyl group having 2 to 10 carbon atoms; a heteroalkynyl group having 2 to 10 carbon atoms; a cycloalkyl group having 5 to 10 carbon atoms; an aryl group having 6 to 10 carbon atoms; a heterocyclyl group having 3 to 10 carbon atoms; or a mono-, di- or tri-substituted alkylsilyl group substituted with an alkyl group having 1 to 6 carbon atoms, or R 1g and R 1h They may be linked to each other to form, together with N, a heterocyclic group of 2 to 10 carbon atoms substituted with an alkyl group of 1 to 6 carbon atoms or having no substituent.
[0085] In another embodiment, in Formula 1, R 1a To R1c can be each independently a hydrogen atom; an alkyl group of 1 to 6 carbon atoms; R 1d It may be a single bond, an unsubstituted alkylene group of 1 to 6 carbon atoms; R 1e It may be an alkyl group having 1 to 10 carbon atoms, or a substituent represented by Formula 1a. In Formula 1a, R 1f It may be a single bond or an unsubstituted alkylene group of 1 to 6 carbon atoms, R 1g and R 1h may each independently be an alkyl group having 1 to 10 carbon atoms or a trialkylsilyl group substituted by an alkyl group having 1 to 6 carbon atoms; or R 1g and R 1h They may be linked to each other to form, together with N, a heterocyclic group of 2 to 6 carbon atoms substituted with an alkyl group of 1 to 3 carbon atoms or having no substituent.
[0086] More specifically, the compound represented by Formula 1 may be one or more selected from the group consisting of compounds represented by the following Formulas 1-1 to 1-3.
[0087] [Formula 1-1]
[0088]
[0089] [Formula 1-2]
[0090]
[0091] [Formula 1-3]
[0092]
[0093] In Formula 1-3, Me is a methyl group.
[0094] In addition, the S-containing aromatic hydrocarbon compound may be a compound represented by Formula 2 below.
[0095] [Formula 2]
[0096]
[0097] In formula 2,
[0098] R5 is a hydrogen atom; an alkyl group of 1 to 30 carbon atoms; an alkenyl group of 2 to 30 carbon atoms; an alkynyl group of 2 to 30 carbon atoms; a heteroalkyl group of 1 to 30 carbon atoms, a heteroalkenyl group of 2 to 30 carbon atoms; a heteroalkynyl group of 2 to 30 carbon atoms; a cycloalkyl group of 5 to 30 carbon atoms; an aryl group of 5 to 30 carbon atoms; or a heterocyclic group of 3 to 30 carbon atoms,
[0099] R6 is a single bond; or an alkylene group of 1 to 20 carbon atoms, and
[0100] R7 is an alkenyl group of 2 to 30 carbon atoms.
[0101] In particular, in Formula 2, R5 can be a hydrogen atom; an alkyl group of 1 to 10 carbon atoms; or a heteroalkyl group of 1 to 10 carbon atoms, R6 can be a single bond; or an alkylene group of 1 to 10 carbon atoms, and R7 can be an alkenyl group of 2 to 10 carbon atoms.
[0102] More specifically, the compound represented by Formula 2 may be a compound represented by the following Formula 2-1.
[0103] [Formula 2-1]
[0104]
[0105] In addition, the S-containing heterocyclic compound may be a compound represented by Formula 3 below.
[0106] [Formula 3]
[0107]
[0108] In Formula 3, R8 is a hydrogen atom, an alkyl group having 1 to 20 carbon atoms which is substituted by or has no substituent, a cycloalkyl group having 1 to 20 carbon atoms which is substituted by or has no substituent, or an aryl group having 6 to 30 carbon atoms which is substituted by or has no substituent, R9 is an alkylene group having 1 to 5 carbon atoms which is substituted by or has no substituent, the substituent X is selected from the group consisting of a hydroxyl group (—OH), a halogen group, a primary amino group (—NH2) and a secondary amino group (—NHR′), and in the case where X is a secondary amino group, R′ is an alkyl group having 1 to 10 carbon atoms.
[0109] In particular, in Formula 3, R8 may be an unsubstituted alkyl group of 1 to 10 carbon atoms, an unsubstituted cycloalkyl group of 1 to 10 carbon atoms, or an unsubstituted aryl group of 6 to 12 carbon atoms, and R9 may be an unsubstituted alkylene group of 1 to 3 carbon atoms.
[0110] More specifically, the compound represented by Formula 3 may be a compound represented by the following Formula 3-1.
[0111] [Formula 3-1]
[0112]
[0113] In addition, the modifier according to the present invention may be a modifier for modifying at least one terminal of a conjugated diene-based polymer, particularly a modifier having an affinity for silica. The modifier having an affinity for silica may refer to a modifier containing a functional group having an affinity for silica in a compound used as a modifier, and the functional group having an affinity for silica may have excellent affinity with a filler, particularly a silica-based filler, and may mean a functional group capable of interacting between a silica-based filler and a functional group derived from the modifier.
[0114] In particular, according to one embodiment of the present invention, the aminoalkoxysilyl modifier may be a compound represented by Formula 4 below.
[0115] [Formula 4]
[0116]
[0117] In formula 4, R 20 is a single bond, or an alkylene group of 1 to 10 carbon atoms, R 21 and R 22 are each independently an alkyl group having 1 to 10 carbon atoms, R 23 is a single bond or an alkylene group of 1 to 10 carbon atoms, R 24 is hydrogen, an alkyl group of 1 to 10 carbon atoms, or an alkylsilyl group di-substituted or tri-substituted by an alkyl group of 1 to 10 carbon atoms, a is an integer of 2 or 3, c is an integer of 1 to 3, and b is an integer of 0 to 2, wherein b+c=3 may be satisfied.
[0118] In one embodiment, in Formula 4, R 20 It can be a single bond, or an alkylene group of 1 to 5 carbon atoms, R 21 and R 22 can be independently an alkyl group of 1 to 5 carbon atoms, R 23 It can be a single bond or an alkylene group of 1 to 5 carbon atoms, R 24 It can be hydrogen, an alkyl group of 1 to 5 carbon atoms, or a trialkylsilyl group substituted by an alkyl group of 1 to 5 carbon atoms, a can be an integer of 2 or 3, c can be an integer of 1 to 3, and b can be an integer of 0 to 2, wherein b+c=3 can be satisfied.
[0119] In a more specific embodiment, the compound represented by Formula 4 can be one selected from the group consisting of: N,N-bis(3-(dimethoxy(methyl)silyl)propyl)-methyl-1-amine, N,N-bis(3-(diethoxy(methyl)silyl)propyl)-methyl-1-amine, N,N-bis(3-(trimethoxysilyl)propyl)-methyl-1-amine, N,N-bis(3-(triethoxysilyl)propyl)-methyl-1-amine, N,N-dimethyl-3- (Trimethoxysilyl)propane-1-amine, N,N-diethyl-3-(trimethoxysilyl)propane-1-amine, N,N-diethyl-3-(triethoxysilyl)propane-1-amine, tris(trimethoxysilyl)amine, tris(3-(trimethoxysilyl)propyl)amine, N,N-bis(3-(diethoxy(methyl)silyl)propyl)-1,1,1-trimethylsilaneamine and 3-(dimethoxy(methyl)silyl)-N,N-diethylpropane-1-amine.
[0120] Method for preparing modified conjugated diene polymer
[0121] In addition, the present invention provides a method for preparing the modified conjugated diene polymer.
[0122] The modified conjugated diene polymer according to an embodiment of the present invention is prepared by the following preparation method, and can have a narrow molecular weight distribution of greater than 1.0 and less than 3.0, an S content, a Si content and a N content in the molecule within the above range, and thus has good tensile properties and viscoelastic properties in a balanced manner as well as excellent processing properties.
[0123] The method for preparing a modified conjugated diene polymer according to an embodiment of the present invention is characterized in that it includes: a first polymerization reaction step, which is used to carry out a first polymerization of a first monomer and a second monomer in the presence of a polymerization initiator to prepare a first active polymer (S1); and a second polymerization reaction step, which is used to carry out a second polymerization of the first active polymer and a third monomer (S2), wherein the first monomer is a conjugated diene monomer, or a conjugated diene monomer and an aromatic vinyl monomer, the second monomer is an N-containing aromatic hydrocarbon compound, and the third monomer is an S-containing aromatic hydrocarbon compound or an S-containing heterocyclic compound.
[0124] In addition, the preparation method may further include the step of adding an aminoalkoxysilane-based modifier and performing a modification reaction after step (S2).
[0125] The conjugated diene monomers, aromatic vinyl monomers, N-containing aromatic hydrocarbon compounds, S-containing aromatic hydrocarbon compounds, S-containing heterocyclic compounds and aminoalkoxysilyl modifiers used in the preparation method are the same as those described above, and explanation thereof will be omitted.
[0126] The hydrocarbon solvent is not particularly limited, and may be, for example, one or more selected from the group consisting of n-pentane, n-hexane, n-heptane, isooctane, cyclohexane, toluene, benzene, and xylene.
[0127] The polymerization initiator is not particularly limited, and may be, for example, one or more selected from the group consisting of methyllithium, ethyllithium, propyllithium, isopropyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, hexyllithium, n-decyllithium, tert-octyllithium, phenyllithium, 1-naphthyllithium, n-eicosyllithium, 4-butylphenyllithium, 4-tolyllithium, cyclohexyllithium, 3,5-di-n-heptylcyclohexyllithium, cyclopentyllithium, sodium naphthyl, potassium naphthyl, lithium alkoxide, sodium alkoxide, potassium alkoxide, lithium sulfonate, sodium sulfonate, potassium sulfonate, lithium amide, sodium amide, potassium amide and isopropyl lithium amide.
[0128] According to one embodiment of the present invention, based on a total of 100g of monomers, the polymerization initiator can be used with 0.01mmol to 10mmol, 0.05mmol to 5mmol, 0.1mmol to 2mmol, 0.1mmol to 1mmol or 0.15mmol to 0.8mmol. Here, a total of 100g of monomers can represent the total amount of the first monomer, the second monomer and the third monomer.
[0129] In addition, according to an embodiment of the present invention, based on 100g of the first monomer, each of the second monomer and the third monomer can be used in an amount of 0.01g to 10g, or 0.1g to 1g. In this case, the S content in the prepared polymer can be easily controlled within the above range, and a polymer with even better tensile properties can be prepared.
[0130] Meanwhile, in the case where the compound represented by Formula 3 is used as the third monomer, the compound represented by Formula 3 may participate in a polymerization reaction (Corey-Seebach reaction) after being lithiated in the following Exemplary Reaction 1.
[0131] [Reaction 1]
[0132]
[0133] In Reaction 1, R8 and R9 are the same as described above.
[0134] The first polymerization reaction and the second polymerization reaction in step (S1) and step (S2) can be, for example, anionic polymerization, and in a specific embodiment, it is an active anionic polymerization that forms an anionic active part at the polymerization end by anion extension polymerization reaction. In addition, the first polymerization reaction and the second polymerization reaction of step (S1) and step (S2) can be heating polymerization, isothermal polymerization or constant temperature polymerization (adiabatic polymerization). Constant temperature polymerization refers to a polymerization method including a step of polymerization without arbitrarily applying heat and using the reaction heat generated by itself after injecting a polymerization initiator, and heating polymerization refers to a polymerization method including injecting a polymerization initiator and then raising the temperature by arbitrarily heating. Isothermal polymerization may refer to a polymerization method by which the temperature of the polymer is kept constant by applying heat or heating to increase the heat after adding a polymerization initiator.
[0135] In addition, according to an embodiment of the present invention, the first polymerization reaction of step (S1) can be carried out by a diene compound having 1 to 10 carbon atoms in addition to the conjugated diene monomer, and in this case, the effect of preventing the formation of gel on the reactor wall during long-term operation can be achieved. The diene compound can include, for example, 1,2-butadiene.
[0136] Each of the first polymerization reaction and the second polymerization reaction of step (S1) and step (S2) can be carried out in a temperature range of 100° C. or less, -20° C. to 90° C., 0° C. to 80° C., 0° C. to 70° C., or 10° C. to 70° C. Within this range, the molecular weight distribution of the polymer is controlled to be narrow, and an excellent effect of improving physical properties is achieved.
[0137] In addition, the first polymerization reaction and the second polymerization reaction of step (S1) and step (S2) can be carried out by batch polymerization or continuous polymerization, or batch polymerization and continuous polymerization can be combined as needed so that the first polymerization reaction is carried out by batch polymerization and the second polymerization reaction is carried out by continuous polymerization.
[0138] In addition, regardless of whether the first polymerization reaction and the second polymerization reaction of step (S1) and step (S2) are carried out by intermittent polymerization or continuous polymerization, the modified conjugated diene polymer according to the present invention can be prepared by polymerizing the first monomer and the second monomer once, and then performing a secondary polymerization after adding the third monomer.
[0139] For example, if step (S1) and step (S2) are performed by batch polymerization, a hydrocarbon solvent, a polymerization initiator, a first monomer, and a second monomer can be injected into a polymerization reactor, a first polymerization can be performed to prepare a first active polymer, and then, a third monomer can be injected therein, and a second polymerization can be performed.
[0140] In another embodiment, if step (S1) and step (S2) are performed by continuous polymerization using two or more polymerization reactors, the first monomer and the second monomer may be injected into the first reactor of the polymerization reactor, the first polymerization reaction may be performed, the third monomer may be injected into the second reactor, and the second polymerization reaction may be performed. That is, in the preparation method, after the polymerization reaction of the first monomer and the second monomer is performed for a certain period of time, the third monomer may be injected to participate in the polymerization.
[0141] In the preparation method according to the present invention, the positions of the first monomer, the second monomer and the third monomer in the formed polymer chain can be controlled by the time difference of the monomers participating in the polymerization. For example, the polymerization of the second monomer can be carried out together with the first polymer from the polymerization starting point, and the derivative unit from the second monomer can be located at one end portion of the polymer chain. The derivative unit from the third monomer derived from the polymerization of the third monomer injected after and participating in the polymerization can be located at the other end portion of the polymer chain. At the same time, since a small amount of the second monomer is used for polymerization, according to the progress of polymerization, the derivative unit from the second monomer can be located at one end portion of the polymer chain, for example, the part formed when the polymerization is initiated. Afterwards, according to the progress of continuous polymerization, a polymer chain in which only the derivative unit from the first monomer is formed can be prepared.
[0142] In addition, if the preparation method includes a modification reaction, by performing a modification reaction after the above-mentioned first polymerization reaction and second polymerization reaction, a modified conjugated diene polymer having the following structure can be prepared, in which a derivative unit from the second monomer is included at one end of the polymer chain and a derivative unit from the third monomer is included at the other end of the polymer chain, and a functional group derived from a modifier is included at the terminal portion where the derivative unit from the third monomer exists; and since the modified conjugated diene polymer has this structure, the balance between tensile properties and viscoelastic properties can become excellent.
[0143] In another embodiment, the method for preparing modified conjugated diene polymer can be carried out in multiple reactors including two or more polymerization reactors and modification reactors by continuous polymerization method. For example, step (S1) and step (S2) can be carried out continuously in two or more polymerization reactors including the first reactor, and the number of polymerization reactors can be flexibly determined according to reaction conditions and environment. Continuous polymerization method can refer to the reaction process in which reactants are continuously supplied to the reactor and the reaction product produced thereby is continuously discharged. By continuous polymerization method, excellent productivity and processability can be had, and the effect of excellent uniformity of the polymer thus prepared can be achieved.
[0144] In addition, according to one embodiment of the present invention, if the active polymer is continuously prepared in the polymerization reactor, the polymerization conversion rate in the first reactor can be 50% or less, 10% to 50% or 20% to 50%, within which range, the side reaction generated when the polymer is formed after the polymerization reaction is initiated can be suppressed, and the polymer having a linear structure can be induced during the polymerization process. Therefore, the molecular weight distribution of the polymer can be controlled to be narrow, and the excellent improvement effect of physical properties can be achieved.
[0145] In this case, the polymerization conversion rate can be controlled according to the reaction temperature, the residence time in the reactor, and the like.
[0146] The polymerization conversion rate can be determined, for example, by measuring the solid concentration in the polymer solution phase containing the polymer during the polymerization of the polymer. In a specific embodiment, in order to ensure the safety of the polymer solution, a cylindrical container is installed at the outlet of each polymerization reactor to fill a certain amount of polymer solution in the cylindrical container. Then, the cylindrical container is separated from the reactor, the weight (A) of the cylinder filled with the polymer solution is measured, the polymer solution filled in the cylindrical container is transported to an aluminum container, such as an aluminum pan, the weight (B) of the cylindrical container from which the polymer solution is removed is measured, the aluminum container containing the polymer solution is dried in an oven at 140°C for 30 minutes, the weight (C) of the dried polymer is measured, and calculated according to the following mathematical formula 1.
[0147] [Mathematical formula 1]
[0148]
[0149] In Mathematical Formula 1, the total solid content is the total solid (monomer) content in the polymerization solution separated from each reactor, and is the weight percentage of the solid relative to 100% of the polymer solution. For example, if the total solid content is 20% by weight, and if it is applied to Mathematical Formula 1, 20 / 100, i.e., 0.2, can be used instead for calculation.
[0150] At the same time, the polymerization reactants polymerized in the first reactor can be sequentially transported to the polymerization reactor before the modification reactor, and polymerization can be performed until the final polymerization conversion becomes 95% or more. After polymerization in the first reactor, the polymerization conversion of each reactor from the second reactor to the polymerization reactor before the modification reactor can be appropriately controlled to control the molecular weight distribution.
[0151] At the same time, in step (S1), during the preparation of the active polymer, the residence time of the polymerization reactant in the first reactor can be 1 minute to 40 minutes, 1 minute to 30 minutes or 5 minutes to 30 minutes, and within this range, the polymerization conversion rate is easy to control, so the molecular weight distribution of the polymer can be controlled to be narrower, and excellent physical property improvement effect can be obtained.
[0152] The term "polymerization reactant" used in the present invention may refer to a polymer-type intermediate, which is polymerized in each reactor, or may refer to a polymer having a polymerization conversion rate of less than 95% when polymerized in a reactor.
[0153] According to one embodiment of the present invention, the molecular weight distribution (PDI, polydispersity index; MWD, Mw / Mn) of the active polymer prepared in step (S1) can be less than 2.0, 1.0 to less than 1.7, or 1.1 to less than 1.6, and within this range, the molecular weight distribution of the modified conjugated diene polymer prepared by modification reaction or coupling with a modifier is narrow, and the physical property improvement effect can be excellent.
[0154] Meanwhile, the polymerization of step (S1) can be carried out by including a polar additive, and based on a total of 100 g of monomer, the polar additive can be added in a ratio of 0.001 g to 50 g, 0.001 g to 10 g, or 0.005 g to 0.1 g. In another embodiment, based on a total of 1 mmol of the polymerization initiator, the polar additive can be added in a ratio of 0.001 g to 10 g, 0.005 g to 5 g, or 0.005 g to 4 g.
[0155] The polar additive may be, for example, one or more selected from the following compositions: tetrahydrofuran, 2,2-bis(2-tetrahydrofuranyl)propane, diethyl ether, cyclopentyl ether, dipropyl ether, vinyl methyl ether, vinyl dimethyl ether, diethylene glycol, dimethyl ether, tert-butoxyethoxyethane, bis(3-dimethylaminoethyl)ether, (dimethylaminoethyl)ethyl ether, trimethylamine, triethylamine, tripropylamine, N,N,N',N'-tetramethylethylenediamine, sodium menthol and 2-ethyltetrahydrofurfuryl ether, and may preferably be 2,2-bis(2-tetrahydrofurfuryl)propane, triethylamine, tetramethylethylenediamine, sodium menthol or 2-ethyltetrahydrofurfuryl ether. If the polar additive is included, and if the conjugated diene monomer and the aromatic vinyl monomer are copolymerized, their reaction rate differences may be compensated, and the effect of inducing easy formation of random copolymers may be achieved.
[0156] According to one embodiment of the present invention, the reaction or coupling of step (S2) can be carried out in a modified reactor, and in this case, based on a total of 100g of monomer, the amount of the modifier can be 0.01mmol to 10mmol. In another embodiment, based on 1mol of the polymerization initiator of step (S1), the amount of the modifier can be 0.1mol to 10mol, 0.1mol to 5mol, or 0.1mol to 3mol.
[0157] In addition, according to one embodiment of the present invention, the modifier may be injected into the modification reactor, and step (S2) may be performed in the modification reactor. In another embodiment, the modifier may be injected into a delivery section for delivering the active polymer prepared in step (S1) to the modification reactor for performing step (S2), and the active polymer and the modifier may be mixed in the delivery section for reaction or coupling.
[0158] The method for preparing the modified conjugated diene polymer according to the embodiment of the present invention is a method for satisfying the performance of the modified conjugated diene polymer. If the above performance is satisfied as described above, the effect intended to be achieved by the present invention can be achieved, but at least in the preparation method, the polymerization conversion rate during the transportation from the first reactor to the second reactor under the continuous process needs to be satisfied, and by controlling other polymerization conditions differently, the physical properties of the modified conjugated diene polymer of the present invention can be achieved.
[0159] Furthermore, the present invention provides a rubber composition comprising the modified conjugated diene-based polymer.
[0160] The rubber composition may include the modified conjugated diene polymer in an amount of 10 wt % or more, 10 wt % to 100 wt %, or 20 wt % to 90 wt %, and within this range, mechanical properties such as tensile strength and wear resistance are excellent, and an excellent balance between physical properties can be achieved.
[0161] In addition, as required, in addition to the modified conjugated diene polymer, the rubber composition may also include other rubber components, and in this case, the content of the rubber component may be 90 wt % or less based on the total weight of the rubber composition. In a specific embodiment, the content of the rubber component may be 1 to 900 parts by weight based on 100 parts by weight of the modified conjugated diene polymer.
[0162] The rubber component may be, for example, natural rubber or synthetic rubber, and in particular may be natural rubber (NR) including cis-1,4-polyisoprene; modified natural rubber obtained by modifying or purifying ordinary natural rubber, such as epoxidized natural rubber (ENR), deproteinized natural rubber (DPNR) and hydrogenated natural rubber; and synthetic rubbers such as styrene-butadiene copolymer (SBR), polybutadiene (BR), polyisoprene (IR), butyl rubber (IIR), ethylene-propylene copolymer, copolymerized isobutylene-isoprene, chloroprene rubber, copolymerized (ethylene-propylene), copolymerized (styrene-butadiene), copolymerized (styrene-isoprene), copolymerized (styrene-isoprene-butadiene), copolymerized (isoprene-butadiene), copolymerized (ethylene-propylene-diene), polysulfide rubber, acrylic rubber, polyurethane rubber, silicone rubber, epichlorohydrin rubber, butyl rubber and halogenated butyl rubber, and any one of them or a mixture of two or more thereof may be used.
[0163] Based on 100 weight portions of the modified conjugated diene polymer of the present invention, the rubber composition can include 0.1 weight portion to 200 weight portions, or 10 weight portions to 120 weight portions of filler. The filler can be, for example, a silicon dioxide filler, particularly wet silicon dioxide (hydrated silicate), dry silicon dioxide (anhydrous silicate), calcium silicate, aluminum silicate or colloidal silicon dioxide. Preferably, the filler can be wet silicon dioxide, which has the most significant cracking characteristic improvement effect and wet grip compatibility effect. In addition, if desired, the rubber composition can also include a carbon filler.
[0164] In another embodiment, if silica is used as a filler, a silane coupling agent can be used together to improve reinforcement and low exothermic properties. Specific examples of silane coupling agents may include bis (3-triethoxysilylpropyl) tetrasulfide, bis (3-triethoxysilylpropyl) trisulfide, bis (3-triethoxysilylpropyl) disulfide, bis (2-triethoxysilylethyl) tetrasulfide, bis (3-trimethoxysilylpropyl) tetrasulfide, bis (2-trimethoxysilylethyl) tetrasulfide, 3-mercaptopropyl trimethoxysilane, 3-mercaptopropyl triethoxysilane, 2-mercaptoethyl trimethoxysilane, 2-mercaptoethyl triethoxysilane, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-triethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, Formyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropylbenzothiazolyl tetrasulfide, 3-triethoxysilylpropylbenzothiazolyl tetrasulfide, 3-triethoxysilylpropylmethacrylic acid monosulfide, 3-trimethoxysilylpropylmethacrylic acid monosulfide, bis(3-diethoxymethylsilylpropyl)tetrasulfide, 3-mercaptopropyldimethoxymethylsilane, dimethoxymethylsilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide or dimethoxymethylsilylpropylbenzothiazolyl tetrasulfide, and any one of them or a mixture of two or more thereof can be used. In view of the effect of improving the reinforcing property, bis(3-triethoxysilylpropyl)polysulfide or 3-trimethoxysilylpropylbenzothiazolyl tetrasulfide can be preferably used.
[0165] In addition, in the rubber composition according to one embodiment of the present invention, since a modified conjugated diene polymer having a functional group having a high affinity with silica is introduced in an active part as a rubber component, the mixing amount of the silane coupling agent can be less than that of a normal case. Therefore, the silane coupling agent can be used in an amount of 1 to 20 parts by weight or 5 to 15 parts by weight based on 100 parts by weight of silica. Within the above range, the effect as a coupling agent can be fully exerted, and the effect of preventing the gelation of the rubber component can be achieved.
[0166] The rubber composition according to the embodiment of the present invention can be sulfur cross-linkable, and therefore can further include a vulcanizing agent. The vulcanizing agent can be particularly sulfur powder, and based on 100 parts by weight of the rubber component, can be included with 0.1 parts by weight to 10 parts by weight. Within the above range, the elasticity and strength required for the vulcanized rubber composition can be ensured, and at the same time, excellent low fuel consumption can be achieved.
[0167] The rubber composition according to the embodiment of the present invention may further include various additives used in the general rubber industry in addition to the above-mentioned components, specifically, vulcanization accelerators, processing oils, antioxidants, plasticizers, anti-aging agents, scorch retardants, zinc white, stearic acid, thermosetting resins or thermoplastic resins.
[0168] The vulcanization accelerator may include 0.1 to 5 parts by weight of, for example, a thiazole compound (e.g., 2-mercaptobenzothiazole (M), dibenzothiazole disulfide (DM), and N-cyclohexyl-2-benzothiazolylsulfenamide (CZ)) or a guanidine compound (e.g., diphenylguanidine (DPG)), based on 100 parts by weight of the rubber component.
[0169] Processing oil acts as a softener in the rubber composition and can include, for example, paraffin compounds, cycloparaffin compounds or aromatic compounds. Considering tensile strength and wear resistance, aromatic processing oils can be used, considering hysteresis loss and the characteristics under low temperatures, cycloparaffin or paraffin processing oils can be used. Based on the rubber component of 100 weight portions, the content of processing oil can be below 100 weight portions. Within the above range, the tensile strength of vulcanized rubber and the deterioration of low heat release performance (low fuel consumption rate) can be prevented.
[0170] The antioxidant may include, for example, 2,6-di-tert-butyl-p-cresol, dibutylhydroxytoluene, 2,6-bis((dodecylthio)methyl)-4-nonylphenol or 2-methyl-4,6-bis((octylthio)methyl)phenol, and may be used in an amount of 0.1 to 6 parts by weight based on 100 parts by weight of the rubber component.
[0171] The anti-aging agent may include, for example, N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, or a condensate of diphenylamine and acetone at high temperature, in an amount of 0.1 to 6 parts by weight based on 100 parts by weight of the rubber component.
[0172] The rubber composition according to an embodiment of the present invention can be obtained by mixing using a mixing device such as a Banbury mixer, a roller and an internal mixer according to a mixing formula. The rubber composition with low exothermic performance and good wear resistance can be obtained by a vulcanization process after a molding process.
[0173] Therefore, the rubber composition can be used to manufacture each component of a tire, such as a tire tread, a tread base, a sidewall, a carcass covering rubber, a belt covering rubber, a bead filler, a bead filler, and a bead covering rubber, or to manufacture rubber products in various industries, such as anti-vibration rubber, a belt conveyor, and a hose.
[0174] Furthermore, the present invention provides a tire manufactured using the rubber composition.
[0175] The tire may be a tire or include a tire tread.
[0176] Hereinafter, the present invention will be described in detail with reference to the embodiments. However, the embodiments according to the present invention can be modified into various other types, and the scope of the present invention should not be limited to the embodiments described below. The embodiments of the present invention are provided to explain the present invention more completely to those with general knowledge in the art.
[0177] Example 1
[0178] Into the first reactor of the series of three reactors were injected: a styrene solution in which 60 wt% of styrene was dissolved in n-hexane at a rate of 2.67 kg / h; a 1,3-butadiene solution in which 60 wt% of 1,3-butadiene was dissolved in n-hexane at a rate of 11.2 kg / h; a second monomer solution in which 15 wt% of 1-methyl-4-(4-vinylbenzyl)piperazine (Sigma-Aldrich) was dissolved in n-hexane at a rate of 72.04 g / h; and a 1,3-butadiene solution in which 60 wt% of 1,3-butadiene was dissolved in n-hexane at a rate of 11.2 kg / h. Hexane at a rate of 46.28 kg / h; a solution in which 10 wt% of 2,2-(di(2-tetrahydrofuryl)propane was dissolved in n-hexane as a polar additive at a rate of 35.0 g / h; and an n-butyllithium solution in which 6.6 wt% of n-butyllithium was dissolved in n-hexane at a rate of 90.91 g / h. In this case, the temperature of the first reactor was maintained at 65° C., and at a time point when the polymerization conversion rate reached 45%, the polymerization reactant was transported from the first reactor to the second reactor through a transport pipe.
[0179] Then, into the second reactor, a 1,3-butadiene solution in which 60 wt% of 1,3-butadiene was dissolved in n-hexane was injected at a rate of 2.95 kg / h, and a third monomer solution in which 5 wt% of phenyl (vinyl) sulfide (CAS No. 1822-73-7, Sigma-Aldrich) was dissolved in n-hexane was injected at a rate of 25.52 g / h. In this case, the temperature of the second reactor was maintained at 75° C., and at a time point when the polymerization conversion rate reached 95% or more, the polymerization reactant was transported from the second reactor to the third reactor through a transport pipe.
[0180] The polymer reactant was transported from the second reactor to the third reactor, and a solution in which 20 wt % of N,N-dimethyl-3-(trimethoxysilyl)propane-1-amine was dissolved as a modifier was continuously injected into the third reactor at a rate of 60.0 g / h. The temperature of the third reactor was maintained at 65° C.
[0181] After that, into the polymerization solution discharged from the third reactor, a solution of IR1520 (BASF) in which 30 wt % of an antioxidant was dissolved was injected at a rate of 166.67 g / h and stirred. The polymer thus obtained was injected into hot water heated with steam and stirred to remove the solvent, thereby preparing a modified conjugated diene polymer.
[0182] Example 2
[0183] A modified conjugated diene polymer was prepared by carrying out the same method as in Example 1, except that in Example 1, a solution in which 5 wt % of 2-methyl-1,3-dithiane (CAS No. 6607-26-7, Sigma-Aldrich) was dissolved in n-hexane was continuously supplied to the second reactor at a rate of 25.25 g / h as the third monomer solution.
[0184] Example 3
[0185] A modified conjugated diene-based polymer was prepared by performing the same method as in Example 1, except that in Example 1, the third monomer solution was continuously supplied to the second reactor at a rate of 51.04 g / h.
[0186] Example 4
[0187] A modified conjugated diene polymer was prepared by carrying out the same method as in Example 1, except that in Example 1, a solution in which 15 wt % of 4-ethyl-N,N-bis(trimethylsilyl)aniline was dissolved in n-hexane was continuously supplied to the first reactor as the second monomer solution at a rate of 87.76 g / h.
[0188] Comparative Example 1
[0189] A modified conjugated diene-based polymer was prepared by performing the same method as in Example 1, except that in Example 1, the second monomer solution and the third monomer solution were not supplied to the first reactor.
[0190] Comparative Example 2
[0191] A modified conjugated diene-based polymer was prepared by performing the same method as in Example 1, except that in Example 1, the third monomer solution was not supplied to the second reactor.
[0192] Comparative Example 3
[0193] A modified conjugated diene-based polymer was prepared by performing the same method as in Example 1, except that in Example 1, the second monomer solution was not supplied to the first reactor.
[0194] Comparative Example 4
[0195] A modified conjugated diene-based polymer was prepared by performing the same method as in Example 2, except that in Example 2, the second monomer solution was not supplied to the first reactor.
[0196] Experimental Example 1
[0197] For each of the modified conjugated diene polymers prepared in the examples and comparative examples, the styrene unit content and 1,2-vinyl content in the polymer were measured, and the weight average molecular weight (Mw, × 10 3 g / mol), number average molecular weight (Mn, ×10 3 g / mol), molecular weight distribution (PDI, MWD), Si content, N content and S content. The results are shown in the following Table 1.
[0198] 1) Styrene unit (SM) content (weight %) and 1,2-vinyl content (weight %)
[0199] The styrene unit (SM) and 1,2-vinyl content in each polymer were measured and analyzed using a Varian VNMRS 500 MHz NMR.
[0200] In measuring NMR, 1,1,2,2-tetrachloroethane was used as a solvent, and the styrene unit and 1,2-vinyl content were calculated by calculating the solvent peak as 5.97 ppm, regarding 7.2-6.9 ppm as a random styrene peak, 6.9-6.2 ppm as a block styrene peak, 5.8-5.1 ppm as 1,4-vinyl and 1,2-vinyl peaks, and 5.1-4.5 ppm as a 1,2-vinyl peak.
[0201] 2) Weight average molecular weight (Mw, × 10 3 g / mol), number average molecular weight (Mn, ×10 3 g / mol) and molecular weight distribution (PDI, MWD)
[0202] By gel permeation chromatography (GPC) analysis, the weight average molecular weight (Mw) and number average molecular weight (Mn) are measured. In addition, molecular weight distribution (PDI, MWD, Mw / Mn) is calculated based on each molecular weight thus measured. Specifically, GPC is performed by combining two PLgel Olexis (Polymer Laboratories) columns and one PLgel mixed-C (Polymer Laboratories) column. In order to calculate the molecular weight, polystyrene (PS) is used as a GPC standard material. The GPC measurement solvent uses a mixture of tetrahydrofuran and 2% by weight of an amine compound.
[0203] 3) Si content
[0204] The Si content was measured by ICP analysis using inductively coupled plasma optical emission spectrometry (ICP-OES; Optima 7300DV). Specifically, about 0.7 g of the sample was added to a platinum (Pt) crucible, and then about 1 mL of concentrated sulfuric acid (98 wt %, electronic grade) was added thereto, heated at 300° C. for 3 hours, and incinerated in an electric furnace (ThermoScientific, Lindberg Blue M) by the following procedures 1 to 3:
[0205] 1) Step 1: Initial temperature 0°C, rate (temperature / hour) 180°C / hour, temperature (holding time) 180°C (1 hour)
[0206] 2) Step 2: Initial temperature 180°C, rate (temperature / hour) 85°C / hour, temperature (holding time) 370°C (2 hours)
[0207] 3) Step 3: initial temperature 370°C, rate (temperature / hour) 47°C / hour, temperature (holding time) 510°C (3 hours),
[0208] Add 1 mL of concentrated nitric acid (48 wt%) and 20 μl of concentrated hydrofluoric acid (50 wt%) to the residue, seal the platinum crucible and shake for more than 30 minutes, add 1 mL of boric acid to the sample, store at 0°C for more than 2 hours, dilute with 30 mL of ultrapure water, and incinerate.
[0209] 4) N content
[0210] The N content is measured by the NSX analysis method using a trace nitrogen quantitative analyzer (NSX-2100H). Specifically, the trace nitrogen quantitative analyzer (autosampler, horizontal furnace, PMT & Nitrogen detector) is turned on, the carrier gas flow is set to 250ml / min for Ar, 350ml / min for O2, 300ml / min for the ozone generator, the heater is set to 800°C, and the analyzer is placed for about 3 hours to stabilize. After stabilizing the analyzer, a calibration curve with a calibration curve range of 5ppm, 10ppm, 50ppm, 100ppm and 500ppm is made using a nitrogen standard (AccuStandard S-22750-01 to 5ml), and the area corresponding to each concentration is obtained. Afterwards, a ceramic boat containing 20mg of sample is placed in the autosampler of the analyzer and measured to obtain the area. By using the sample area and calibration curve thus obtained, the N content is calculated.
[0211] 5) S content
[0212] The measurement was performed by combustion ion chromatography (C-IC) analysis, and the combustion ion chromatography analysis was measured using ICS2100 / AQF-2100H. Specifically, the combustion ion chromatography used IonPac AS18 (4x250mm) as a column and a suppressed conductivity detector as a detector, the supply current was set to 76mA, and the solvent was set so that 30.05mM KOH was injected at a flow rate of 1ml / min. The combustion temperature was set so that the inlet was 900°C, the outlet was 1,000°C, and the carrier gas flow rate was 200ml / min for Ar gas and 400ml / min for O2 gas. After stabilizing the analyzer, the standard material (ERM-EC680K or ERM-EC681M) was analyzed to make a calibration curve. After that, the boat containing 50 mg of the sample was burned and diluted to a final volume of 10 ml by passing through an aqueous solution containing an absorbent (H2O2 900 mg / kg), 100 μl of the diluted sample was collected and passed through the analyzer, and the S content was calculated using a calibration curve of the standard substance.
[0213] [Table 1]
[0214]
[0215] As shown in Table 1, it can be confirmed that the modified conjugated diene polymers of Examples 1 to 4 show a molecular weight distribution of 1.0 or more and less than 3.0, an S content of 25 ppm or more, a Si content of 100 ppm or more, and an N content of 200 ppm or more. Meanwhile, in the case of Comparative Examples 1 and 2, the S content is 0, and compared with Examples 1 to 4, Comparative Examples 1, 3, and 4 show that the value is significantly reduced to half the level of the N content. In this case, Comparative Example 1 corresponds to a polymer prepared without using the N-containing aromatic hydrocarbon compound, the S-containing aromatic hydrocarbon compound, and the S-containing heterocyclic compound proposed by the present invention, Comparative Example 2 corresponds to a polymer prepared without using the S-containing aromatic hydrocarbon compound and the S-containing heterocyclic compound during polymerization, and Comparative Examples 3 and 4 correspond to polymers without using the N-containing aromatic hydrocarbon compound during polymerization. It can be found that the modified conjugated diene polymer according to the present invention includes derivative units from N-containing aromatic hydrocarbon compounds, derivative units from S-containing aromatic hydrocarbon compounds or derivative units from S-containing heterocyclic compounds, and derivative units from modifiers in the polymer chain, and the significant improvement effect of tensile strength, rolling resistance and wear resistance brought about by this difference can be confirmed through the following Experimental Example 2.
[0216] Experimental Example 2
[0217] In order to comparatively analyze the physical properties of the rubber compositions comprising each modified conjugated diene-based copolymer prepared in Examples and Comparative Examples and the molded articles made therefrom, the tensile strength, abrasion resistance and rolling resistance were measured respectively. The results are shown in Table 3 below.
[0218] 1) Preparation of rubber samples
[0219] Using each of the modified conjugated diene-based polymers of Examples and Comparative Examples as a raw material rubber, compounding was performed under the compounding conditions shown in the following Table 2. The raw material amounts in Table 2 are expressed in parts by weight based on 100 parts by weight of the raw material rubber.
[0220] [Table 2]
[0221]
[0222] Specifically, the rubber sample was kneaded by first-stage kneading and second-stage kneading. In the first-stage kneading, the raw rubber, silica (filler), organic silane coupling agent (X50S, Evonik), process oil (TADE oil), zinc oxide (ZnO), stearic acid, antioxidant (TMQ (RD)) (2,2,4-trimethyl-1,2-dihydroquinoline polymer), antioxidant (6PPD ((dimethylbutyl)-N-phenyl-phenylenediamine) and wax (microcrystalline wax) were kneaded using a Banbury mixer equipped with a temperature control device. In this case, the kneading device was set to The initial temperature was controlled at 70°C, and after the mixing was completed, the first compounded mixture was obtained at a discharge temperature of 145°C. In the second stage of mixing, the first compounded mixture was cooled to room temperature, and the first compounded mixture, sulfur, rubber accelerator (DPD (diphenylguanidine)) and vulcanization accelerator (CZ (N-cyclohexyl-2-benzothiazolylsulfenamide)) were added to the mixing device and mixed at a temperature below 100°C to obtain a second compounded mixture. Then, the rubber sample was formed by curing at 160°C for 20 minutes.
[0223] 2) Tensile properties
[0224] Based on the ASTM 412 tensile test method, each sample was manufactured and the tensile strength at break was measured. Specifically, the tensile properties were measured at a rate of 50 cm / min at room temperature using a Universal Test Machin 4204 tensile tester (Instron). In Table 3, the result values are expressed as an index based on the result values of Comparative Example 1, with higher values indicating better results.
[0225] 3) Rolling resistance
[0226] The viscoelastic properties were confirmed by measuring the viscoelastic behavior of thermodynamic deformation at each measurement temperature (-60°C to 60°C) using a dynamic mechanical analyzer (GABO) in film tension mode at a frequency of 10 Hz and ensuring the tanδ value. It can be seen from the result value that if the tanδ value at a high temperature of 60°C is reduced, the hysteresis loss becomes smaller and the rolling resistance (fuel consumption rate) becomes better. However, in Table 3, the result values are shown as indicators based on the result values of Comparative Example 1, and the higher the value, the better the result.
[0227] 4) Wear resistance (DIN wear test)
[0228] For each rubber sample, a DIN wear test was performed based on ASTM D5963 and indicated by a DIN loss index (loss volume index: ARIA (Abrasion Resistance Index, Method A)). In Table 3, the result values are indicated as indices based on the result values of Comparative Example 1, and a higher value indicates a better result.
[0229] [Table 3]
[0230]
[0231] As shown in Table 3, compared with Comparative Examples 1 to 4, Examples 1 to 4 all show the effect of greatly improving tensile strength, rolling resistance and wear resistance. Specifically, compared with Comparative Example 1, Examples 1 to 4 show the effect of significantly improving tensile strength, rolling resistance and wear resistance by more than 10%, and in this case, Comparative Example 1 corresponds to a polymer prepared without using the N-containing aromatic hydrocarbon compound, S-containing aromatic hydrocarbon compound and S-containing heterocyclic compound proposed in the present invention. In addition, compared with Comparative Examples 2 to 4, Examples 1 to 4 show that tensile strength, rolling resistance and wear resistance are significantly improved by at least 5% to at most more than 15%, and in this case, Comparative Examples 2 to 4 correspond to polymers prepared without using the N-containing aromatic hydrocarbon compound, or the S-containing aromatic hydrocarbon compound and the S-containing heterocyclic compound proposed in the present invention.
[0232] It can be confirmed that the modified conjugated diene polymer according to the present invention includes a derivative unit from the N-containing aromatic hydrocarbon compound and a derivative unit from the S-containing aromatic hydrocarbon compound or a derivative unit from the S-containing heterocyclic compound by using an N-containing aromatic hydrocarbon compound and a S-containing aromatic hydrocarbon compound or a S-containing heterocyclic compound during polymerization, and the tensile strength, rolling resistance and wear resistance are significantly improved in a balanced manner.
Claims
1. A modified conjugated diene polymer, comprising: Repeating units derived from conjugated diene monomers; Units derived from N-containing aromatic hydrocarbon compounds; and A unit derived from a S-containing aromatic hydrocarbon compound or a S-containing heterocyclic compound and satisfies the following conditions (i) and (ii): (i) molecular weight distribution (PDI; MWD): 1.0 or more and less than 3.0; and (ii) S content: 25 ppm or more based on the total weight of the polymer, in, The derivative units derived from the N-containing aromatic hydrocarbon compound and the derivative units derived from the S-containing aromatic hydrocarbon compound or from the S-containing heterocyclic compound are present in the polymer chain including the repeating units derived from the conjugated diene monomer, Wherein, based on the total weight of the polymer, the N content is 50 ppm or more, Wherein, the N-containing aromatic hydrocarbon compound is a compound represented by the following formula 1: [Formula 1] In formula 1, R 1a To R 1c each independently represents a hydrogen atom; an alkyl group of 1 to 20 carbon atoms; an alkenyl group of 2 to 20 carbon atoms; an alkynyl group of 2 to 20 carbon atoms; a heteroalkyl group of 1 to 20 carbon atoms, a heteroalkenyl group of 2 to 20 carbon atoms; a heteroalkynyl group of 2 to 20 carbon atoms; a cycloalkyl group of 5 to 20 carbon atoms; an aryl group of 6 to 20 carbon atoms; or a heterocyclyl group of 3 to 20 carbon atoms, R 1d is a single bond, an alkylene group of 1 to 20 carbon atoms which may be substituted or unsubstituted; a cycloalkylene group of 5 to 20 carbon atoms which may be substituted or unsubstituted; or an arylene group of 6 to 20 carbon atoms which may be substituted or unsubstituted, wherein the substituent is an alkyl group of 1 to 10 carbon atoms, a cycloalkyl group of 5 to 10 carbon atoms, or an aryl group of 6 to 20 carbon atoms, and R 1e is a substituent represented by the following formula 1a: [Formula 1a] In formula 1a, R 1f is a single bond, an alkylene group of 1 to 20 carbon atoms which may be substituted or unsubstituted; a cycloalkylene group of 5 to 20 carbon atoms which may be substituted or unsubstituted; or an arylene group of 6 to 20 carbon atoms which may be substituted or unsubstituted, wherein the substituent is an alkyl group of 1 to 10 carbon atoms, a cycloalkyl group of 5 to 10 carbon atoms, or an aryl group of 6 to 20 carbon atoms, and R 1g and R 1h each independently represents an alkyl group of 1 to 20 carbon atoms; an alkenyl group of 2 to 20 carbon atoms; an alkynyl group of 2 to 20 carbon atoms; a heteroalkyl group of 1 to 20 carbon atoms; a heteroalkenyl group of 2 to 20 carbon atoms; a heteroalkynyl group of 2 to 20 carbon atoms; a cycloalkyl group of 5 to 20 carbon atoms; an aryl group of 6 to 20 carbon atoms; a heterocyclyl group of 3 to 20 carbon atoms; or a mono-, di- or tri-substituted alkylsilyl group substituted with an alkyl group of 1 to 10 carbon atoms, or R 1g and R 1h are connected to each other to form, together with N, a heterocyclic group of 2 to 10 carbon atoms substituted with an alkyl group of 1 to 10 carbon atoms or having no substituent, Wherein, the S-containing aromatic compound is a compound represented by the following formula 2: [Formula 2] In formula 2, R5 is a hydrogen atom; an alkyl group of 1 to 30 carbon atoms; an alkenyl group of 2 to 30 carbon atoms; an alkynyl group of 2 to 30 carbon atoms; a heteroalkyl group of 1 to 30 carbon atoms, a heteroalkenyl group of 2 to 30 carbon atoms; a heteroalkynyl group of 2 to 30 carbon atoms; a cycloalkyl group of 5 to 30 carbon atoms; an aryl group of 5 to 30 carbon atoms; or a heterocyclic group of 3 to 30 carbon atoms, R6 is a single bond; or an alkylene group of 1 to 20 carbon atoms, and R7 is an alkenyl group of 2 to 30 carbon atoms, Wherein, the S-containing heterocyclic compound is a compound represented by the following formula 3: [Formula 3] In formula 3, R8 is a hydrogen atom, an alkyl group having 1 to 20 carbon atoms which may be substituted by a substituent X or not, a cycloalkyl group having 1 to 20 carbon atoms which may be substituted by a substituent X or not, or an aryl group having 6 to 30 carbon atoms which may be substituted by a substituent X or not, R9 is an alkylene group of 1 to 5 carbon atoms which is substituted by a substituent X or has no substituent, and The substituent X is selected from the group consisting of hydroxyl (-OH), halogen groups, primary amino (-NH2) and secondary amino (-NHR') groups, and in the case where X is a secondary amino group, R' is an alkyl group of 1 to 10 carbon atoms.
2. The modified conjugated diene polymer according to claim 1, wherein The Si content is 50 ppm or more based on the total weight of the polymer.
3. The modified conjugated diene polymer according to claim 1, wherein In formula 1, R 1a To R 1c each independently represents a hydrogen atom; an alkyl group of 1 to 10 carbon atoms; an alkenyl group of 2 to 10 carbon atoms; an alkynyl group of 2 to 10 carbon atoms; a heteroalkyl group of 1 to 10 carbon atoms; a heteroalkenyl group of 2 to 10 carbon atoms; a heteroalkynyl group of 2 to 10 carbon atoms; a cycloalkyl group of 5 to 10 carbon atoms; an aryl group of 6 to 10 carbon atoms; or a heterocyclyl group of 3 to 10 carbon atoms, R 1d is a single bond, or an unsubstituted alkylene group of 1 to 10 carbon atoms, R 1e is a substituent represented by formula 1a, In Formula 1a, R 1f is a single bond, or an unsubstituted alkylene group of 1 to 10 carbon atoms, R 1g and R 1h Each of the above may be independently an alkyl group having 1 to 10 carbon atoms; an alkenyl group having 2 to 10 carbon atoms; an alkynyl group having 2 to 10 carbon atoms; a heteroalkyl group having 1 to 10 carbon atoms; a heteroalkenyl group having 2 to 10 carbon atoms; a heteroalkynyl group having 2 to 10 carbon atoms; a cycloalkyl group having 5 to 10 carbon atoms; an aryl group having 6 to 10 carbon atoms; a heterocyclyl group having 3 to 10 carbon atoms; or a mono-, di- or tri-substituted alkylsilyl group substituted with an alkyl group having 1 to 6 carbon atoms, or R 1g and R 1h They are connected to each other to form, together with N, a heterocyclic group of 2 to 10 carbon atoms substituted with an alkyl group of 1 to 6 carbon atoms or having no substituent.
4. The modified conjugated diene polymer according to claim 1, wherein In formula 2, R5 is a hydrogen atom; an alkyl group of 1 to 10 carbon atoms; or a heteroalkyl group of 1 to 10 carbon atoms, R6 is a single bond; or an alkylene group of 1 to 10 carbon atoms, and R7 is an alkenyl group of 2 to 10 carbon atoms.
5. The modified conjugated diene polymer according to claim 1, wherein In formula 3, R8 is an unsubstituted alkyl group of 1 to 10 carbon atoms, an unsubstituted cycloalkyl group of 1 to 10 carbon atoms, or an unsubstituted aryl group of 6 to 12 carbon atoms, and R9 is an alkylene group of 1 to 3 carbon atoms which has no substituent. 6 . The modified conjugated diene-based polymer according to claim 1 , further comprising a functional group derived from an aminoalkoxysilane-based modifier.
7. The modified conjugated diene polymer according to claim 6, wherein the aminoalkoxysilane modifier is a compound represented by the following formula 4: [Formula 4] In formula 4, R 20 is a single bond, or an alkylene group of 1 to 10 carbon atoms, R 21 and R 22 are each independently an alkyl group having 1 to 10 carbon atoms, R 23 is a single bond or an alkylene group of 1 to 10 carbon atoms, R 24 is hydrogen, an alkyl group of 1 to 10 carbon atoms, or an alkylsilyl group di-substituted or tri-substituted by an alkyl group of 1 to 10 carbon atoms, a is an integer of 2 or 3, c is an integer of 1 to 3, and b is an integer of 0 to 2, wherein b+c=3.
8. A method for preparing the modified conjugated diene polymer of claim 1, the method comprising: A first polymerization step S1 is used to perform a first polymerization of a first monomer and a second monomer in a hydrocarbon solvent in the presence of a polymerization initiator to prepare a first living polymer; and The second polymerization step S2 is used to perform a second polymerization of the first living polymer and the third monomer, The first monomer is a conjugated diene monomer, or a conjugated diene monomer and an aromatic vinyl monomer, the second monomer is an N-containing aromatic hydrocarbon compound, and the third monomer is an S-containing aromatic hydrocarbon compound or an S-containing heterocyclic compound.
9. The method for preparing a modified conjugated diene polymer according to claim 8, wherein: The second monomer and the third monomer are each used in an amount of 0.01 to 10 g based on 100 g of the first monomer.
10. The method for preparing a modified conjugated diene polymer according to claim 8, wherein: The polymerization initiator is used in an amount of 0.01 mmol to 10 mmol based on 100 g in total of the first monomer, the second monomer, and the third monomer. 11 . The method for preparing a modified conjugated diene polymer according to claim 8 , further comprising the step of adding an aminoalkoxysilane modifier and performing a modification reaction after step S2 .
12. The method for preparing a modified conjugated diene polymer according to claim 11, wherein: The modifier is used in an amount of 0.1 to 10 mol based on 1 mol of the polymerization initiator. 13 . A rubber composition comprising the modified conjugated diene polymer according to claim 1 and a filler.
14. The rubber composition according to claim 13, wherein The rubber composition includes 0.1 parts by weight to 200 parts by weight of the filler based on 100 parts by weight of the modified conjugated diene-based polymer.
15. The rubber composition according to claim 13, wherein The filler is a silica filler or a carbon black filler.