Flexible polyamide film

By using units composed of aliphatic dicarboxylic acids and diamines with more than 18 carbon atoms in the polyamide film, a high melting point and soft polyamide film is formed, which solves the problem of the performance degradation of polyamide films at high temperatures in the prior art. problem, achieving both softness and heat resistance.

CN114729119BActive Publication Date: 2024-10-15UNITIKA LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080080528.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-27
Filing Date
2020-11-10
Publication Date
2024-10-15
Estimated Expiration
2040-11-10

AI Technical Summary

Technical Problem

During the polymerization process at high temperatures, the existing heat-resistant polyamide film decomposes the soft segments due to hydrolysis reaction and shortens the segment length, resulting in insufficient performance, low melting point and low heat resistance, making it difficult to meet the softness and heat resistance requirements. balance.

Method used

Use units composed of aliphatic dicarboxylic acids and diamines with more than 18 carbon atoms to form a polyamide film of 10 to 92% by mass, avoid the use of polyether and polyester components that are easily decomposed, and optimize hard segments and soft chains The phase separation structure of segments improves softness and melting point.

Benefits of technology

A polyamide film with excellent flexibility and a melting point higher than 240°C has been realized, which improves the heat resistance and mechanical properties of the film, reduces water absorption and dielectric loss, and is suitable for a variety of electronic and packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003654487000000131
    Figure BDA0003654487000000131
  • Figure BDA0003654487000000161
    Figure BDA0003654487000000161
  • Figure BDA0003654487000000171
    Figure BDA0003654487000000171
Patent Text Reader

Abstract

A flexible polyamide film, characterized in that it is a film formed by molding polyamide, wherein the polyamide contains units composed of an aliphatic dicarboxylic acid (A1) having more than 18 carbon atoms and / or units composed of an aliphatic diamine (B1) having more than 18 carbon atoms, the total content of the units composed of (A1) and the content of the units composed of (B1) in the polyamide is 10 to 92% by mass, and the melting point of the film is above 240°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyamide film having both heat resistance and flexibility. Background Art

[0002] Polyamide films are excellent in heat resistance and mechanical properties, so research is developing towards the electrical and electronic fields, and in recent years, applications to flexible or foldable devices are also being studied (e.g., Patent Documents 1 and 2). However, conventional polyamide films with heat resistance do not have sufficient flexibility for use in these devices.

[0003] As a method for improving the flexibility of polyamide, there is a method of forming a structure having both hard segments and soft segments and each segment being phase-separated, which is considered to be an ideal form with high flexibility. In the past, polyamides having hard segments and soft segments were mostly composed of crystalline polyamides such as polyamide 6, polyamide 11, and polyamide 12 in the hard segment, and the soft segment was composed of a block copolymer containing polyether, etc., and the bond between the hard segment and the soft segment was mostly an ester bond.

[0004] However, polyamide having the above structure has problems of low melting point and low heat resistance compared to polyester having a hard segment and a soft segment.

[0005] The production of high melting point polyamide requires polymerization at high temperature. However, if the polymerization temperature is high, the soft segment decomposes due to the moisture generated in the condensation reaction, the amino groups contained in the raw material monomers, and the amino groups generated in the hydrolysis of the polyamide, and the segment length becomes shorter. As a result, the obtained polyamide has a problem of reduced molecular weight and insufficient performance.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent No. 6061814

[0009] Patent Document 2: Japanese Patent Application Publication No. 2000-186141 Summary of the invention

[0010] The present invention aims to solve the above-mentioned problems and has the object of providing a polyamide film which does not contain polyether components and polyester components that are easily decomposed during polymerization, forms a phase-separated structure of soft segments and hard segments that is considered to be an ideal form with high flexibility, has excellent flexibility, and has a high melting point.

[0011] The present inventors have conducted intensive studies to solve such problems and have found that a film of a polyamide containing 10 to 92% by weight of units consisting of an aliphatic dicarboxylic acid having 18 or more carbon atoms and / or units consisting of an aliphatic diamine having 18 or more carbon atoms can achieve the above-mentioned purpose, thereby completing the present invention.

[0012] The flexible polyamide film of the present invention is characterized in that it is a film formed by molding a polyamide, wherein the polyamide contains a unit composed of an aliphatic dicarboxylic acid (A1) having 18 or more carbon atoms and / or a unit composed of an aliphatic diamine (B1) having 18 or more carbon atoms,

[0013] The total content of the unit composed of the aliphatic dicarboxylic acid (A1) having 18 or more carbon atoms and the unit composed of the aliphatic diamine (B1) having 18 or more carbon atoms in the polyamide is 10 to 92% by mass.

[0014] The melting point of the film is 240°C or higher.

[0015] According to the flexible polyamide film of the present invention, the aliphatic dicarboxylic acid (A1) having 18 or more carbon atoms is preferably a dimer acid.

[0016] According to the flexible polyamide film of the present invention, the aliphatic diamine (B1) having 18 or more carbon atoms is preferably a dimer diamine.

[0017] According to the flexible polyamide film of the present invention, the polyamide preferably includes a unit consisting of a dicarboxylic acid (A2) having 12 or less carbon atoms.

[0018] According to the flexible polyamide film of the present invention, the polyamide preferably includes a unit consisting of a diamine (B2) having 12 or less carbon atoms.

[0019] According to the flexible polyamide film of the present invention, the dicarboxylic acid (A2) having 12 or less carbon atoms is preferably terephthalic acid.

[0020] According to the flexible polyamide film of the present invention, the diamine (B2) having 12 or less carbon atoms is preferably 1,10-decanediamine.

[0021] According to the flexible polyamide film of the present invention, the polyamide preferably does not contain a segment consisting of polyether or polyester.

[0022] According to the present invention, by using a polyamide which does not contain easily decomposed polyether components and polyester components during polymerization and contains a specific amount of units composed of aliphatic dicarboxylic acids having 18 or more carbon atoms and / or units composed of aliphatic diamines having 18 or more carbon atoms, it is possible to provide a polyamide film having excellent flexibility and a high melting point. DETAILED DESCRIPTION

[0023] The flexible polyamide film of the present invention is a film formed by molding a polyamide containing units consisting of an aliphatic dicarboxylic acid (A1) having 18 or more carbon atoms and / or units consisting of an aliphatic diamine (B1) having 18 or more carbon atoms.

[0024] <Polyamide>

[0025] The polyamide constituting the flexible polyamide film of the present invention must contain units consisting of an aliphatic dicarboxylic acid (A1) having at least 18 carbon atoms and / or units consisting of an aliphatic diamine (B1) having at least 18 carbon atoms. In the polyamide constituting the film of the present invention, the units consisting of (A1) and / or the units consisting of (B1) form a soft segment.

[0026] In the present invention, the total content of the unit composed of (A1) and the unit composed of (B1) in the polyamide is required to be 10 to 92% by mass, preferably 15 to 80% by mass, more preferably 30 to 80% by mass, and further preferably 40 to 75% by mass from the viewpoint of the balance between flexibility and heat resistance. If the total content of the polyamide is less than 10% by mass, the flexibility decreases, while if the total content exceeds 92% by mass, the obtained film may have a decreased heat resistance or break during stretching or heat setting.

[0027] In the present invention, from the viewpoint of flexibility and stretchability, the polyamide preferably contains both units consisting of an aliphatic dicarboxylic acid (A1) having 18 or more carbon atoms and units consisting of an aliphatic diamine (B1) having 18 or more carbon atoms, and the mass ratio (units consisting of (A1) / units consisting of (B1)) is preferably 90 / 10 to 10 / 90, more preferably 70 / 30 to 10 / 90, and further preferably 50 / 50 to 10 / 90.

[0028] From the viewpoint of flexibility and heat resistance, it is more preferable to contain a unit consisting of an aliphatic diamine (B1) having 18 or more carbon atoms alone rather than a unit consisting of an aliphatic dicarboxylic acid having 18 or more carbon atoms (A1) alone.

[0029] The aliphatic dicarboxylic acid (A1) having 18 or more carbon atoms preferably consists entirely of hydrocarbons except for the carboxyl group, and examples thereof include hexadecanedicarboxylic acid (having 18 carbon atoms), octadecanedicarboxylic acid (having 20 carbon atoms), and dimer acid (having 36 carbon atoms).

[0030] Among them, from the perspective of obtaining a polyamide with high flexibility, (A1) is more preferably an aliphatic dicarboxylic acid having 20 or more carbon atoms, and is further preferably a dimer acid. The dimer acid may have an unsaturated bond, but from the perspective of being less likely to be colored, it is preferably hydrogenated so that all carbon-carbon bonds are saturated.

[0031] The aliphatic diamine (B1) having 18 or more carbon atoms preferably consists entirely of hydrocarbons except for the amino group, and examples thereof include octadecanediamine (having 18 carbon atoms), eicosandiamine (having 20 carbon atoms), and dimerizediamine (having 36 carbon atoms).

[0032] Among them, (B1) is preferably dimer diamine from the perspective of obtaining a polyamide with high flexibility even if the content is small. Dimer diamine can be produced by reacting a dimer acid with ammonia, followed by dehydration, nitrilation, and reduction. Dimer diamine may have unsaturated bonds, but from the perspective of being less prone to coloration, it is preferably hydrogenated so that all bonds are saturated bonds.

[0033] In the present invention, units other than the units composed of the aliphatic dicarboxylic acid (A1) having 18 or more carbon atoms and the units composed of the aliphatic diamine (B1) having 18 or more carbon atoms in the polyamide mainly form hard segments.

[0034] The unit constituting the hard segment is not particularly limited, but is preferably a unit consisting of a dicarboxylic acid (A2) having 12 or less carbon atoms or a unit consisting of a diamine (B2) having 12 or less carbon atoms.

[0035] Examples of the dicarboxylic acid (A2) having a carbon number of 12 or less include sebacic acid (carbon number 10), azelaic acid (carbon number 9), adipic acid (carbon number 6), terephthalic acid (carbon number 8), isophthalic acid (carbon number 8), and phthalic acid (carbon number 8). Among them, from the viewpoint of improving flexibility, it is preferred to contain a dicarboxylic acid having a carbon number of 8 or more.

[0036] Examples of the diamine (B2) having a carbon number of 12 or less include dodecanediamine (carbon number 12), undecanediamine (carbon number 11), decanediamine (carbon number 10), nonanediamine (carbon number 9), octanediamine (carbon number 8), hexamethylenediamine (carbon number 6), and butanediamine (carbon number 4). Among these, from the viewpoint of improving flexibility, it is preferred to contain a diamine having a carbon number of 5 or more, and it is more preferred to contain a diamine having a carbon number of 8 or more.

[0037] In the present invention, the hard segment is preferably composed of units constituting a highly crystalline polyamide. The highly crystalline polyamide is preferably a semi-crystalline polyamide composed of an aromatic dicarboxylic acid and an aliphatic diamine, for example, polyamide 4T, polyamide 9T, polyamide 10T, polyamide 12T, among which polyamide 10T is preferred from the perspective of a good balance between heat resistance and crystallinity. Therefore, (A2) constituting the hard segment is preferably terephthalic acid, and (B2) is preferably butanediamine, nonanediamine, decanediamine, dodecanediamine, and more preferably 1,10-decanediamine.

[0038] By making the units constituting the hard segment units constituting highly crystalline polyamide, the heat resistance of the obtained polyamide is improved, and the formation of a phase separation structure between the hard segment and the soft segment is promoted, thereby improving the flexibility.

[0039] If the soft segment comprising a unit consisting of an aliphatic dicarboxylic acid (A1) having more than 18 carbon atoms and / or a unit consisting of an aliphatic diamine (B1) having more than 18 carbon atoms is compared with a soft segment consisting of a polyether or a polyester, there is a tendency for the segment length to become shorter. If the segment length of the soft segment becomes shorter, it is sometimes difficult to form a phase separation structure with the hard segment. However, by making the unit constituting the hard segment a unit constituting a highly crystalline polyamide, a phase separation structure can be formed even if the soft segment length is short.

[0040] In the present invention, the polyamide preferably does not contain a segment composed of a polyether or polyester that is easily decomposed during polymerization. Examples of the polyether include polyoxyethylene glycol, polyoxypropylene glycol, polyoxybutylene glycol, and polyoxyethylene-polyoxypropylene glycol, and examples of the polyester include polyethylene adipate, polybutylene adipate, and polyethylene sebacate. If the polymerization temperature of the polyamide containing a segment composed of a polyether or polyester is high, it may decompose.

[0041] In the present invention, the polyamide may contain an end-capping agent in order to adjust the degree of polymerization, inhibit decomposition of the product, inhibit coloration, etc. As the end-capping agent, for example, monocarboxylic acids such as acetic acid, lauric acid, benzoic acid, and stearic acid, and monoamines such as octylamine, cyclohexylamine, aniline, and stearylamine can be cited. The end-capping agent can be used alone or in combination. The content of the end-capping agent is not particularly limited, and is generally 0 to 10 mol% relative to the total molar amount of the dicarboxylic acid and the diamine.

[0042] <Polyamide film>

[0043] The flexible polyamide film of the present invention is obtained by molding the above-mentioned polyamide.

[0044] The flexible polyamide film of the present invention has excellent heat resistance, and the melting point, which is an index of heat resistance, needs to be 240°C or higher, preferably 250°C or higher, more preferably 270°C or higher, and further preferably 300°C or higher.

[0045] The flexible polyamide film of the present invention is excellent in flexibility, and its elastic modulus, which is an index of flexibility, is preferably 2500 MPa or less, more preferably 2000 MPa or less, and further preferably 1500 MPa or less.

[0046] The flexible polyamide film of the present invention has low water absorption, and small dimensional changes or mechanical property changes due to water absorption. The water absorption is preferably 2.5% or less, preferably 2.0% or less, more preferably 1.5% or less, and further preferably 1.0% or less.

[0047] Furthermore, the flexible polyamide film of the present invention has low dielectric loss tangent and dielectric constant, is excellent in dielectric properties, and is also excellent in insulation properties.

[0048] <Manufacturing of polyamide>

[0049] In the present invention, the method for producing polyamide is not particularly limited, and the polyamide can be produced by a conventional polyamide polymerization method. For example, there can be mentioned a method of using a pressure vessel equipped with a stirrer or a continuous polymerization apparatus to heat the raw monomers while discharging condensation water to the outside of the system to carry out polymerization.

[0050] In the manufacture of polyamide, a catalyst may be used as required. As the catalyst, for example, phosphoric acid, phosphorous acid, hypophosphorous acid or salts thereof may be cited. The content of the catalyst is not particularly limited, but is generally 2 mol% or less relative to the total molar amount of the dicarboxylic acid and the diamine.

[0051] In the production of polyamide, an organic solvent or water may be added as necessary.

[0052] In the manufacture of polyamide, polymerization can be carried out in a closed system or at normal pressure. When carried out in a closed system, pressure sometimes rises due to the volatilization of monomers, the generation of condensation water, etc., so it is preferred to appropriately control the pressure. On the other hand, when the boiling point of the monomers used is high, even if pressurized, the monomers will not flow out of the system, and polymerization can be carried out at normal pressure. For example, when the raw monomers are a combination of dimer acid, dimer diamine, terephthalic acid, and decanediamine, polymerization can be carried out at normal pressure.

[0053] In the production of polyamide, polymerization is preferably performed under a nitrogen atmosphere or under vacuum in order to prevent oxidative degradation.

[0054] The polymerization temperature is not particularly limited and is generally 150 to 300°C. In order to suppress the decomposition and deterioration reactions of the obtained polyamide, it is preferably carried out at a temperature not exceeding 300°C, preferably at a temperature below the melting point of the polyamide. If the polymerization is carried out at a temperature below the melting point of the polyamide, the hard segment component is in a precipitated state, but the soft segment component is in a molten state, so the reactant has fluidity as a whole. Therefore, the polymerization can be carried out using the existing equipment and process for melt polymerization of polyamide. It should be noted that at this time, the polymerization of the hard segment is carried out in the form of solid phase polymerization. The method of polymerizing at a temperature below the melting point is particularly effective in the polymerization of high melting point polyamides above 280°C, which have a high polymerization temperature and are easily decomposed.

[0055] The polymerized polyamide can be extruded into tows and made into pellets, or can be cut thermally or underwater to make pellets.

[0056] In the manufacturing method of polyamide, solid phase polymerization can be performed to further increase the molecular weight. Solid phase polymerization is particularly effective for situations where the viscosity during polymerization is high and the operation is difficult. Solid phase polymerization is preferably performed by heating at a temperature lower than the melting point of the resin for more than 30 minutes under the circulation of an inert gas or under reduced pressure, and more preferably by heating for more than 1 hour.

[0057] <Manufacturing of polyamide film>

[0058] The flexible polyamide film of the present invention can be manufactured by the following method: after the polyamide is melted at 240 to 340° C. for 3 to 15 minutes, it is extruded into a sheet through a T-die, and the extrudate is closely attached to a roller whose temperature is adjusted to -10 to 80° C. for cooling. The polyamide film of the present invention can also use the obtained unstretched film in an unstretched state, but it is usually used after stretching. Stretching is preferably uniaxial or biaxial stretching, more preferably biaxial stretching. It is preferred that the polyamide in the film is oriented and crystallized by stretching. As stretching methods, simultaneous stretching method and sequential stretching method can be cited.

[0059] As an example of the simultaneous biaxial stretching method, there can be cited a method of simultaneously biaxially stretching an unstretched film and then subjecting it to a heat fixation treatment. The stretching is preferably performed at 30 to 150°C at a ratio of 1.5 to 5 times in both the width direction (hereinafter sometimes referred to as "TD") and the longitudinal direction (hereinafter sometimes referred to as "MD"). The heat fixation treatment is preferably performed at 150 to 300°C for a few seconds with the relaxation of TD being set to several %. Before the simultaneous biaxial stretching, the film may be subjected to a preliminary longitudinal stretching of about 1 to 1.2 times.

[0060] As an example of the sequential biaxial stretching method, there can be cited a method in which the unstretched film is subjected to a heat treatment such as roller heating or infrared heating, and then stretched in the longitudinal direction, and then continuously subjected to transverse stretching and heat fixing treatment. The longitudinal stretching is preferably carried out at a ratio of 1.5 to 5 times at 30 to 150° C. The transverse stretching is preferably carried out at 30 to 150° C. in the same manner as the longitudinal stretching. The ratio of the transverse stretching is preferably 2 times or more, and more preferably 3 times or more. The heat fixing treatment is preferably carried out at 150 to 300° C. for a few seconds with the relaxation of TD being several %.

[0061] As a method for stretching a polyamide film, for example, a flat film type sequential biaxial stretching method, a flat film type simultaneous biaxial stretching method, and a tubular film method can be cited. Among them, from the viewpoint of being able to improve the thickness accuracy of the film and make the physical properties of the MD of the film uniform, it is preferred to adopt a flat film type simultaneous biaxial stretching method. As a stretching device for adopting the flat film type simultaneous biaxial stretching method, for example, a spiral tenter, a pantograph tenter, and a linear motor driven clamp-type tenter can be cited.

[0062] As a heat treatment method after stretching, for example, there are known methods such as a method of blowing hot air, a method of irradiating infrared rays, and a method of irradiating microwaves. Among them, the method of blowing hot air is preferred because it can heat uniformly and accurately.

[0063] The obtained flexible polyamide film can be a single sheet or can be wound on a winding roller to form a film roll. From the perspective of productivity when used for various purposes, the film roll is preferably in the form of a film roll. When made into a film roll, it can be divided into a desired width.

[0064] It should be noted that in the manufacturing device of the polyamide film, in order to prevent the polyamide from being retained on the surface of the barrel, the melting part of the barrel, the metering part, the single tube, the filter, the T-die, etc., it is preferred to perform a roughness reduction treatment on the surface thereof. As a method for reducing the surface roughness, for example, a method of modifying with a substance with low polarity can be cited, and another method of vapor-depositing silicon nitride or diamond-like carbon on the surface thereof can be cited.

[0065] <Additives>

[0066] In order to improve the thermal stability during film formation, prevent the deterioration of the strength and elongation of the film, and prevent the deterioration of the film caused by oxidation, decomposition, etc. during use, the flexible polyamide film of the present invention preferably contains a thermal stabilizer. Examples of the thermal stabilizer include hindered phenol-based thermal stabilizers, hindered amine-based thermal stabilizers, phosphorus-based thermal stabilizers, sulfur-based thermal stabilizers, and bifunctional thermal stabilizers.

[0067] Examples of hindered phenol-based heat stabilizers include Irganox 1010 (registered trademark) (manufactured by BASF Japan, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]), Irganox 1076 (registered trademark) (manufactured by BASF Japan, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), Cyanox 1790 (registered trademark) (manufactured by Solvay, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid), Irganox 1098 (registered trademark) (manufactured by BASF JAPAN Co., Ltd., N,N'-(hexane-1,6-diyl)bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], Sumilizer GA-80 (registered trademark) (Sumitomo Chemical Co., Ltd., 3,9-bis[2-{3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane).

[0068] Examples of hindered amine heat stabilizers include Nylostab S-EED (registered trademark) (manufactured by Clariant Japan Co., Ltd., N,N′-bis-2,2,6,6-tetramethyl-4-piperidinyl-1,3-benzenedicarbamide).

[0069] Examples of phosphorus-based heat stabilizers include Irgafos 168 (registered trademark) (manufactured by BASF Japan, tris(2,4-di-tert-butylphenyl)phosphite), Irgafos 12 (registered trademark) (manufactured by BASF Japan, 6,6',6"-[nitrilotri(ethyleneoxy)]tris(2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]diphenylphosphite), and Phosphophan)), Irgafos38 (registered trademark) (manufactured by BASF Japan, bis(2,4-di-tert-butyl)-6-methylphenyl)ethyl phosphite), ADKSTAB329K (registered trademark) (manufactured by ADEKA, tris(monodinonylphenyl)phosphite), ADKSTAB PEP36 (registered trademark) (manufactured by ADEKA, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite), Hostanox P-EPQ (registered trademark) (manufactured by Clarion, tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenyl bisphosphonite), GSY-P101 (registered trademark) (manufactured by Sakai Chemical Industry Co., Ltd., tetrakis(2,4-di-tert-butyl-5-methylphenyl)-4,4'-biphenyl bisphosphonite), Sumilizer GP (registered trademark) (manufactured by Sumitomo Chemical Co., Ltd., 6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]-di phosphine).

[0070] Examples of the sulfur-based heat stabilizer include DSTP "Yoshitomi" (registered trademark) (manufactured by Mitsubishi Chemical Corporation, distearyl thiodipropionate) and Seenox 412S (registered trademark) (manufactured by SHIPRO KASEI Co., Ltd., pentaerythritol tetrakis (3-dodecylthiopropionate)).

[0071] Examples of the bifunctional heat stabilizer include Sumilizer GM (registered trademark) (manufactured by Sumitomo Chemical Co., Ltd., 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate) and Sumilizer GS (registered trademark) (manufactured by Sumitomo Chemical Co., Ltd., 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate).

[0072] From the viewpoint of preventing the deterioration of film strength, hindered phenol-based heat stabilizers are preferred. The thermal decomposition temperature of the hindered phenol-based heat stabilizer is preferably above 320°C, and more preferably above 350°C. Sumilizer GA-80 can be cited as a hindered phenol-based heat stabilizer having a thermal decomposition temperature of above 320°C. In addition, if the hindered phenol-based heat stabilizer has an amide bond, the deterioration of film strength can be prevented. As a hindered phenol-based heat stabilizer having an amide bond, for example, Irganox 1098 can be cited. In addition, by using a hindered phenol-based heat stabilizer in combination with a difunctional heat stabilizer, the deterioration of film strength can be further reduced.

[0073] These heat stabilizers can be used alone or in combination of two or more. For example, if a hindered phenol heat stabilizer and a phosphorus heat stabilizer are used in combination, the pressure increase of the filter for filtering the raw materials during the film-making of the film can be prevented, and the deterioration of the film strength can be prevented. In addition, if a hindered phenol heat stabilizer, a phosphorus heat stabilizer and a bifunctional heat stabilizer are used in combination, the pressure increase of the filter for filtering the raw materials during the film-making of the film can be prevented, and the deterioration of the film strength can be further reduced.

[0074] As a combination of a hindered phenolic heat stabilizer and a phosphorus-based heat stabilizer, a combination of Sumilizer GA-80 or Irganox 1098 and Hostanox P-EPQ or GSY-P101 is preferred. As a combination of a hindered phenolic heat stabilizer, a phosphorus-based heat stabilizer and a bifunctional heat stabilizer, a combination of Sumilizer GA-80 or Irganox 1098 and Hostanox P-EPQ or GSY-P101 and Sumilizer GS is preferred, and a combination of Sumilizer GA-80 and GSY-P101 and Sumilizer GS is more preferred.

[0075] The content of the above-mentioned heat stabilizer in the flexible polyamide film of the present invention is preferably 0.01 to 2 parts by mass, and more preferably 0.05 to 1 part by mass, relative to 100 parts by mass of polyamide. By setting the content of the heat stabilizer to 0.01 to 2 parts by mass, thermal decomposition can be more effectively suppressed. It should be noted that when two or more heat stabilizers are used in combination, it is preferred that the content of each heat stabilizer and the total content of the heat stabilizers fall within the above range.

[0076] In order to improve the sliding property, the flexible polyamide film of the present invention may contain lubricant particles. Examples of lubricant particles include inorganic particles such as silicon dioxide, aluminum oxide, titanium dioxide, calcium carbonate, kaolin, and barium sulfate, and organic particles such as acrylic resin particles, melamine resin particles, silicone resin particles, and cross-linked polystyrene particles.

[0077] In the scope of not damaging the effect of the present invention, the soft polyamide film of the present invention can also contain various additives on the basis of the above-mentioned heat stabilizer and lubricant particles as needed. As additives, for example, colorants such as pigments and dyes, anti-colorants, antioxidants different from the above-mentioned heat stabilizers, weathering improvers, flame retardants, plasticizers, release agents, reinforcing agents, modifiers, antistatic agents, ultraviolet absorbers, antifogging agents, and various polymers can be cited. As pigments, titanium oxides, etc. can be cited. As weathering improvers, benzotriazole compounds, etc. can be cited. As flame retardants, bromine flame retardants, phosphorus flame retardants, etc. can be cited. As reinforcing agents, talc, etc. can be cited. It should be noted that the above-mentioned various additives can be added at any stage when manufacturing the film.

[0078] <Film processing>

[0079] The flexible polyamide film of the present invention may be subjected to treatment for improving the adhesiveness of its surface as required. Examples of methods for improving the adhesiveness include corona treatment, plasma treatment, acid treatment, and flame treatment.

[0080] In order to impart functions such as good adhesion, antistatic properties, mold release properties, and gas barrier properties to the surface of the flexible polyamide film of the present invention, various coating agents may be applied.

[0081] The flexible polyamide film of the present invention may be laminated with inorganic substances such as metals or their oxides, other types of polymers, paper, woven fabrics, nonwoven fabrics, wood, and the like.

[0082] <Application of membrane>

[0083] The flexible polyamide film of the present invention has excellent heat resistance and flexibility. Therefore, the stretched flexible polyamide film of the present invention can be suitably used as: packaging materials for pharmaceuticals; packaging materials for foods such as retort foods; packaging materials for electronic components such as semiconductor packages; electrical insulating materials for motors, transformers, cables, etc.; dielectric materials for capacitors, etc.; materials for tapes such as cassette tapes, data storage tapes for digital data storage, and video tapes; solar cell substrates, liquid crystal panels, conductive films, and protective plates for display devices, etc.; electronic substrate materials such as LED mounting substrates, flexible printed wiring boards, and flexible flat cables; heat-resistant adhesive tapes such as cover films for flexible printed wiring, heat-resistant masking tapes, and industrial engineering tapes; heat-resistant barcode labels; heat-resistant reflectors; various release films; heat-resistant adhesive base films; photo films; molding materials; agricultural materials; medical materials; civil engineering and construction materials; household and industrial materials such as filtration membranes; and films for fiber materials.

[0084] Example

[0085] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples.

[0086] A. Evaluation Method

[0087] The physical properties of polyamide and polyamide film were measured by the following methods.

[0088] (1) Composition

[0089] The obtained polyamide and polyamide film were subjected to high-resolution nuclear magnetic resonance (ECA-500NMR manufactured by JEOL Ltd.). 1 The resin composition was determined from the peak intensity of each copolymer component by H-NMR analysis (resolution: 500 MHz, solvent: a mixed solvent of deuterated trifluoroacetic acid and deuterated chloroform in a volume ratio of 4 / 5, temperature: 23°C).

[0090] (2) Melting point

[0091] Several milligrams of the obtained polyamide film were cut out and the temperature was raised to 350°C at a heating rate of 20°C / min using a differential scanning calorimeter DSC-7 (manufactured by PerkinElmer), then maintained at 350°C for 5 minutes, cooled to 25°C at a cooling rate of 20°C / min, and further maintained at 25°C for 5 minutes. The apex of the endothermic peak when the temperature was again raised at a heating rate of 20°C / min was taken as the melting point.

[0092] (3) Tensile breaking strength, tensile breaking elongation and tensile elastic modulus of stretched films

[0093] The measurement was performed in an environment of a temperature of 20° C. and a humidity of 65% according to JIS K 7127. The size of the sample was 10 mm×150 mm, the initial distance between the chucks was 100 mm, and the tensile speed was 500 mm / min.

[0094] (4) Water absorption

[0095] The obtained polyamide film was subjected to water absorption treatment in pure water at 23° C. for 2 days, and then the surface water was wiped off. The water absorption rate was determined by measuring the weight change before and after the water absorption treatment.

[0096] B. Raw materials

[0097] The following materials were used as raw materials.

[0098] Dimer acid: Pripol 1009 manufactured by Croda

[0099] Dimer diamine: Priamine 1075 manufactured by Croda

[0100] Heat stabilizer: Sumitomo Chemical Co., Ltd. Sumilizer GA-80

[0101] Manufacturing example

[0102] Polyamide P1

[0103] In a reaction container equipped with a heating mechanism and a stirring mechanism, 4.7 parts by mass of dimer acid, 4.5 parts by mass of dimer diamine, 44.5 parts by mass of terephthalic acid, 46.2 parts by mass of 1,10-decanediamine, and 0.1 parts by mass of sodium hypophosphite monohydrate were charged.

[0104] Thereafter, the system was heated to 260° C. while stirring, and polymerization was carried out for 5 hours at 260° C. under a nitrogen stream and normal pressure while discharging condensation water out of the system. During the polymerization, the system was in a suspended state.

[0105] After the polymerization was completed, the product was discharged and cut to obtain polyamide P1.

[0106] Polyamide P2~P8

[0107] Polyamides P2 to P8 were obtained by carrying out the same operation as for polyamide P1 except that the monomers charged into the reaction container were changed as shown in Table 1.

[0108] Polyamide P9

[0109] 24.8 parts by mass of 1,4-butanediamine, 17.6 parts by mass of dimer diamine, and 18 parts by mass of dimer acid were charged into an autoclave to generate a salt.

[0110] Next, 39.6 parts by mass of adipic acid was added. The mixture was heated from 37°C and 0 barg to 11 barg and 204°C over 35 minutes. Next, the mixture was maintained at 205°C for 42 minutes, and the pressure was raised to 13.6 barg. Next, the reaction mixture was released into an atmosphere inactivation container to obtain a polyamide in the form of a solid powder. Next, the prepolymer thus obtained was crushed into particles of a size between 1 and 20 mm, and then heated at 230°C under N for 24 hours. 2 / H 2 Post-condensation was carried out in a flow of O (1800 / 700 g / hour) to obtain polyamide P9.

[0111] Polyamide P10

[0112] 49.0 parts by mass of terephthalic acid and 0.1 parts by mass of sodium hypophosphite monohydrate were added to a powder stirring device equipped with a heating mechanism. 50.9 parts by mass of 1,10-decanediamine were added in small portions over 3 hours while being heated at 170°C and stirred to obtain a salt. Thereafter, the salt was heated to 250°C while being stirred, and the condensation water was discharged to the outside of the system, and polymerization was carried out at 250°C under a nitrogen flow, normal pressure, and for 7 hours. After the polymerization was completed, the mixture was discharged to obtain polyamide P10.

[0113] Polyamide P11

[0114] 51.3 parts by mass of dimer acid, 48.6 parts by mass of dimer diamine, and 0.1 parts by mass of sodium hypophosphite monohydrate were placed in a reaction container equipped with a heating mechanism and a stirring mechanism.

[0115] Then, the mixture was heated to 260°C while stirring and condensation water was discharged from the system, and polymerization was carried out for 5 hours at 260°C under a nitrogen stream and normal pressure. During the polymerization, the system was in a uniform molten state. After the polymerization was completed, the mixture was discharged and cut to obtain polyamide P11.

[0116] Polyamide P12

[0117] 51.0 parts by mass of polyoxybutylene glycol (PTMG1000) with a number average molecular weight of 1000 having amino groups instead of hydroxyl groups at both terminals, 28.3 parts by mass of terephthalic acid, 20.6 parts by mass of 1,10-decanediamine, and 0.1 parts by mass of sodium hypophosphite monohydrate were added to a reaction vessel equipped with a heating mechanism and a stirring mechanism, and the mixture was heated to 250° C. while stirring, and the generated water vapor was released, and polymerization was performed at 250° C. under a nitrogen flow, normal pressure, and for 5 hours. During the polymerization, the system was in a state of a suspended solution.

[0118] After the polymerization is completed, it is discharged and cut, but polyamide P12 is brittle and not suitable for practical use.

[0119] Table 1 shows the input composition of the obtained polyamide.

[0120]

[0121] Example 1 (simultaneous biaxially stretched film)

[0122] 100 parts by mass of polyamide P1 and 0.4 parts by mass of Sumilizer GA-80 were dry-blended and fed into a twin-screw extruder with a barrel temperature of 330° C. and a screw diameter of 26 mm for melt kneading. The mixture was extruded into a filament bundle, cooled, and cut to obtain pellets.

[0123] The obtained pellets are put into a single-screw extruder with a barrel temperature of 330°C and a screw diameter of 50 mm for melting. The molten polymer is filtered using a metal fiber sintered filter (manufactured by Nippon Seisen Co., Ltd., "NF-13", absolute filter diameter: 60 μm), and then extruded into a film from a T-die at 330°C. The film is cooled by electrostatic application by fitting it tightly onto a cooling roller at 10°C to obtain an essentially non-oriented unstretched polyamide film.

[0124] The resin composition of the polyamide component of the obtained unstretched film was determined to be the same as the resin composition of the polyamide used.

[0125] The obtained unstretched polyamide film was biaxially stretched using a flat film type simultaneous biaxial stretching machine while holding both ends of the film with a clamp. The stretching conditions were as follows: the temperature of the preheating section was 80°C, the temperature of the stretching section was 80°C, the stretching deformation rate in MD was 2400% / min, the stretching deformation rate in TD was 2400% / min, the stretching ratio in MD was 2.3 times, and the stretching ratio in TD was 2.3 times. After stretching, the film was continuously heat-fixed at 250°C in the same tenter of the biaxial stretching machine, and a relaxation treatment of 6% was performed in the width direction of the film to obtain a biaxially stretched polyamide film.

[0126] The resin composition of the polyamide component of the obtained stretched film was determined to be the same as the resin composition of the polyamide used or the resin composition of the polyamide component of the unstretched film.

[0127] Examples 2, 4 to 7, 9 to 14, and Comparative Example 1 (simultaneous biaxially stretched film)

[0128] Except that the type of polyamide used and the production conditions were changed as shown in Tables 2 and 3, the same operation as in Example 1 was carried out to obtain a biaxially stretched polyamide film.

[0129] Example 3 (unstretched film)

[0130] Using polyamide P3, the same operation as in Example 1 was carried out to obtain a substantially non-oriented unstretched polyamide film, which was evaluated as a flexible polyamide film.

[0131] The resin composition of the polyamide component of the obtained unstretched film was determined to be the same as the resin composition of the polyamide used.

[0132] Example 8 (Sequentially Biaxially Stretched Film)

[0133] The unstretched polyamide film obtained in Example 3 was biaxially stretched using a flat film type sequential axis stretching machine.

[0134] First, the unstretched film is heated to 80° C. by roll heating or infrared heating, and stretched 3.0 times in MD at a stretching deformation rate of 2400% / min to obtain a longitudinally stretched film.

[0135] Then, the film was continuously stretched in the transverse direction by clamping the two ends of the film with the clamps of the transverse stretching machine. The temperature of the preheating section of the TD stretching was 85°C, the temperature of the stretching section was 85°C, the stretching deformation rate was 2400% / min, and the stretching ratio of TD was 3.0 times. Then, in the same tenter of the transverse stretching machine, heat fixing was performed at 250°C, and a relaxation treatment of 6% was performed in the width direction of the film to obtain a biaxially stretched polyamide film.

[0136] Comparative Example 2 (unstretched film)

[0137] Except that the type of polyamide used and the production conditions were changed as shown in Table 3, the same operation as in Example 3 was carried out to obtain a substantially non-oriented unstretched polyamide film.

[0138] Comparative Example 3 (simultaneous biaxially stretched film)

[0139] The unstretched film obtained in Comparative Example 2 was used to obtain a biaxially stretched polyamide film in the same manner as in Example 1. However, the film was broken during heat fixation, and no biaxially stretched polyamide film could be obtained.

[0140] Tables 2 and 3 show the compositions of the polyamides used, the film production conditions, and the properties of the obtained polyamide films.

[0141]

[0142]

[0143] The polyamide films of Examples 1 to 14 have excellent flexibility, a melting point of 240° C. or higher, and excellent heat resistance because the total content of units composed of aliphatic dicarboxylic acids (A1) with more than 18 carbon atoms and the content of units composed of aliphatic diamines (B1) with more than 18 carbon atoms in the polyamide is 10 to 92% by mass.

[0144] By comparing Examples 1 to 13 with Example 14, it can be seen that the water absorption of the film of the polyamide using a diamine having 5 or more carbon atoms as the diamine having 12 or less carbon atoms (B2) is lower.

[0145] The polyamide film of Comparative Example 1 was inferior in flexibility because it used a polyamide that did not contain the unit composed of (A1) and the unit composed of (B1) and did not have a soft segment.

[0146] The polyamide in Comparative Example 2 has a total content of units consisting of an aliphatic dicarboxylic acid (A1) having more than 18 carbon atoms and a content of units consisting of an aliphatic diamine (B1) having more than 18 carbon atoms exceeding 92% by mass, so the melting point cannot be confirmed, and the film after biaxial stretching breaks during heat setting, and has poor heat resistance.

Claims

1. A flexible polyamide film, characterized in that: A film formed by molding a polyamide, the polyamide comprising a unit composed of an aliphatic dicarboxylic acid A1 having 18 or more carbon atoms and / or a unit composed of an aliphatic diamine B1 having 18 or more carbon atoms, a unit composed of a dicarboxylic acid A2 having 12 or less carbon atoms, and a unit composed of a diamine B2 having 5 to 12 carbon atoms, The dicarboxylic acid A2 having 12 or less carbon atoms is an aromatic dicarboxylic acid, The total content of the unit composed of the aliphatic dicarboxylic acid A1 having 18 or more carbon atoms and the unit composed of the aliphatic diamine B1 having 18 or more carbon atoms in the polyamide is 15 to 92% by mass. The melting point of the film is above 300°C. The tensile elastic modulus of the film is 2000 MPa or less.

2. The flexible polyamide film according to claim 1, characterized in that The aliphatic dicarboxylic acid A1 having 18 or more carbon atoms is a dimer acid.

3. The flexible polyamide film according to claim 1 or 2, characterized in that The aliphatic diamine B1 having 18 or more carbon atoms is a dimerized diamine.

4. The flexible polyamide film according to claim 1 or 2, characterized in that: The dicarboxylic acid A2 having 12 or less carbon atoms is terephthalic acid.

5. The flexible polyamide film according to claim 3, characterized in that: The dicarboxylic acid A2 having 12 or less carbon atoms is terephthalic acid.

6. The flexible polyamide film according to claim 1 or 2, characterized in that: The diamine B2 having 5 to 12 carbon atoms is 1,10-decanediamine.

7. The flexible polyamide film according to claim 3, characterized in that The diamine B2 having 5 to 12 carbon atoms is 1,10-decanediamine.

8. The flexible polyamide film according to claim 4, characterized in that The diamine B2 having 5 to 12 carbon atoms is 1,10-decanediamine.

9. The flexible polyamide film according to claim 5, characterized in that The diamine B2 having 5 to 12 carbon atoms is 1,10-decanediamine.

10. The flexible polyamide film according to claim 1 or 2, characterized in that: Polyamides do not contain segments consisting of polyethers or polyesters.

11. The flexible polyamide film according to claim 3, characterized in that Polyamides do not contain segments consisting of polyethers or polyesters.

12. The flexible polyamide film according to claim 4, characterized in that Polyamides do not contain segments consisting of polyethers or polyesters.

13. The flexible polyamide film according to claim 5, characterized in that Polyamides do not contain segments consisting of polyethers or polyesters.

14. The flexible polyamide film according to claim 6, characterized in that Polyamides do not contain segments consisting of polyethers or polyesters.

15. The flexible polyamide film according to claim 7, characterized in that Polyamides do not contain segments consisting of polyethers or polyesters.

16. The flexible polyamide film according to claim 8, characterized in that Polyamides do not contain segments consisting of polyethers or polyesters.