Composite material and method for manufacturing the same

By attaching curved-shaped CNTs to the fiber surface to form a network structure, the problem of difficulty in improving the mechanical properties of CNTs in fibers with larger diameters is solved, and the mechanical strength and electrical conductivity of composite materials are significantly improved.

CN114729499BActive Publication Date: 2024-10-29NITTA CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202080079115.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-20
Publication Date
2024-10-29
Estimated Expiration
2040-11-20

AI Technical Summary

Technical Problem

It is difficult to improve the mechanical properties of fibers with larger diameters in existing composite materials through carbon nanotubes (CNTs), and the number of CNTs attached is insufficient, which affects the electrical conductivity, thermal conductivity and mechanical strength of the materials.

Method used

CNTs with a curved shape are dispersed and attached to the fiber surface through an ultrasonic process to form a network structure, which increases the number of CNTs attached and the thickness of the structure, thereby improving the mechanical properties of the material.

Benefits of technology

By increasing the number of CNTs attached and the thickness of the structure, the mechanical strength, electrical conductivity and thermal conductivity of the composite material are significantly improved, making it suitable for fiber-reinforced moldings in various fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114729499B_ABST
    Figure CN114729499B_ABST
Patent Text Reader

Abstract

The present invention provides a composite material and a method for manufacturing the same that can further improve the properties of carbon nanotubes attached to fibers. A composite material (10) has a structure (12) composed of a plurality of carbon nanotubes (14) formed on the surface of a fiber (11) constituting the composite material (10). The carbon nanotubes (14) have a curved shape. The carbon nanotubes (14) are attached to the surface of the fiber (11) as a curved surface in various postures, and other carbon nanotubes (14) enter the space (gap) formed between the carbon nanotubes (14) and the surface of the fiber (11) or between the attached carbon nanotubes (14), thereby forming a structure (12) composed of more carbon nanotubes (14).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composite material and a method for making the same. Background Art

[0002] A composite material having a structure composed of fibers and a plurality of carbon nanotubes (hereinafter referred to as CNTs) attached to the surface of the fibers has been proposed (for example, Patent Document 1). The structure of the composite material forms a network structure formed by a plurality of CNTs connected to each other and attached to the surface of the fibers. A fiber-reinforced molded body obtained by reinforcing a resin using such a composite material as a reinforcing fiber can obtain higher strength and rigidity than a resin monomer by containing fibers, and at the same time, due to the effect of CNTs, electrical conductivity, thermal conductivity and mechanical properties are improved.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2013-76198 Summary of the invention

[0006] Problems to be solved by the invention

[0007] As described above, the use of fiber-reinforced molded bodies is expanding in various fields, and the requirements for fiber-reinforced molded bodies are becoming higher. On the other hand, fibers with smaller diameters are more likely to obtain the improvement effect of mechanical properties, etc. from CNTs, while fibers with larger diameters are less likely to obtain the improvement effect of mechanical properties, etc. from CNTs, so it is desired to further improve the properties from CNTs.

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a composite material capable of further improving the properties derived from CNTs attached to fibers, and a method for producing the same.

[0009] Means for solving problems

[0010] The composite material of the present invention comprises: fibers; and a structure, wherein the structure is composed of a plurality of carbon nanotubes, forming a network structure in which the carbon nanotubes are in direct contact with each other, and the carbon nanotubes attached to the surface of the fibers are directly attached to the surface of the fibers, wherein the carbon nanotubes are in a curved shape with a curved portion.

[0011] The method for manufacturing the composite material of the present invention includes: an ultrasonic process, applying ultrasonic vibration to a dispersion liquid in which a plurality of carbon nanotubes having a curved shape with a curved portion are dispersed; and an attachment process, immersing continuous fibers in the dispersion liquid to which the ultrasonic vibration is applied, so that the plurality of carbon nanotubes are attached to the fibers to form a structure on the surface of the fibers.

[0012] Effects of the Invention

[0013] According to the present invention, since the carbon nanotubes attached to the fibers have a bent shape having a bent portion, the number of carbon nanotubes attached to the fibers is greater, and the properties derived from the carbon nanotubes can be further improved.

[0014] According to the present invention, since the composite material is manufactured by attaching carbon nanotubes with curved shapes having curved portions to the surface of the fibers in a structure woven like fibers of a non-woven fabric, the number of carbon nanotubes attached to the fibers can be increased, and a composite material can be manufactured in which the properties derived from the carbon nanotubes are further improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 It is an explanatory diagram showing the structure of the composite material according to the first embodiment.

[0016] Figure 2 This is an explanatory diagram showing a multifilament yarn having a composite material as a single yarn.

[0017] Figure 3 This is an explanatory diagram schematically showing the adhesion state of CNTs on the fiber surface.

[0018] Figure 4 This is an explanatory diagram showing the arrangement of an attachment device for attaching CNTs to fibers.

[0019] Figure 5 This is an explanatory diagram showing a fiber bundle in a state of being opened on a guide roller.

[0020] Figure 6 It is an explanatory diagram showing the passing position of the fiber in the dispersion.

[0021] Figure 7 This is a SEM photograph showing an example of a bent state of a CNT material.

[0022] Figure 8 It is an explanatory diagram showing the structure of a composite material provided with a fixing resin portion according to the second embodiment.

[0023] Fig. 9 It is an explanatory diagram showing a state where the carbon nanotubes are fixed by the fixing resin portion.

[0024] Fig.10 This is a perspective view showing an example of a flat belt using a composite material.

[0025] Fig.11 This is a perspective view showing an example of a V-belt using a composite material.

[0026] Fig.12This is a perspective view showing an example of a timing belt using a composite material.

[0027] Fig.13 This is a graph showing the cut fiber length measured by the fragmentation method when glass fibers are used.

[0028] Fig.14 This is a SEM photograph showing a structure formed on glass fiber. DETAILED DESCRIPTION

[0029] [First embodiment]

[0030] [Composite Materials]

[0031] exist Figure 1 In the embodiment, the composite material 10 includes a fiber 11 and a structure 12 formed on the surface of the fiber 11. The structure 12 is formed by a plurality of carbon nanotubes (hereinafter referred to as CNT) 14 entangled with each other. The composite material 10 is, for example, a fiber impregnated with a resin or the like in the structure 12 (hereinafter referred to as a resin-impregnated fiber), or a reinforcing fiber for constituting a monofilament or a fiber-reinforced molded body. The composite material 10 and the resin-impregnated fiber, multifilament or fiber-reinforced molded body, etc. (hereinafter referred to as secondary products) made using such a composite material 10 improve mechanical properties, etc. by providing the surface of the fiber 11 with a structure 12. That is, the mechanical properties, etc. from the CNT 14 attached to the surface of the fiber 11 are improved.

[0032] like Figure 2 As shown in an example of a multifilament 15 using a composite material 10, the multifilament 15 has a plurality of composite materials 10 and a matrix resin 16. Figure 2 In the figure, a multifilament 15 composed of six composite materials 10 is depicted, but the number of composite materials 10 is not particularly limited, and for example, several thousand to several hundred thousand composite materials 10 may constitute the multifilament 15. In addition, a plurality of composite materials 10 may be twisted into one multifilament 15.

[0033] For example, a resin such as polyurethane or an elastomer such as synthetic rubber can be used as the matrix resin 16. The matrix resin 16 is interposed between the composite materials 10 to bond the composite materials 10 to each other. The matrix resin is impregnated into the structure 12 of each composite material 10 and cured.

[0034] The fiber 11 is not particularly limited, and resin fibers such as nylon, polyester, vinylon, and acrylic fiber, or glass fibers and mineral fibers can be cited. In addition, the diameter of the fiber 11 is not particularly limited, and it is preferred to use fibers with a diameter in the range of 5 μm to 100 μm, and more preferably to use fibers with a diameter in the range of 5 μm to 30 μm. The fiber 11 uses a long fiber, and its length is preferably 50 m or more, more preferably in the range of 100 m or more and 100,000 m or less, and further preferably in the range of 100 m or more and 10,000 m or less. In addition, for example, the fiber 11 can be shortened after the structure 12 is formed.

[0035] The CNTs 14 constituting the structure 12 are uniformly dispersed and entangled with each other in the substantially entire surface of the fiber 11, thereby forming a network structure in which a plurality of CNTs 14 are connected in an entangled state. The connection mentioned here includes physical connection (simple contact) and chemical connection. The CNTs 14 are in direct contact with each other, and there are no inclusions such as dispersants such as surfactants or adhesives between them.

[0036] like Figure 3 As schematically shown, a portion of CNT14 constituting the structure 12 is directly attached and fixed on the surface of the fiber 11. Thus, the structure 12 is directly attached to the surface of the fiber 11. The so-called direct attachment of CNT14 to the surface of the fiber 11 means that there is no dispersant such as a surfactant or an adhesive between the surface of the CNT14 and the fiber 11, and the CNT14 is directly attached to the fiber 11, and its attachment (fixation) is combined by van der Waals force. Since a portion of CNT14 constituting the structure 12 is directly attached to the surface of the fiber 11, the structure 12 is in direct contact with the surface of the fiber 11 without the aid of a dispersant or an adhesive.

[0037] As CNT14, a bent CNT14 is used. Therefore, among the CNT14 constituting the structure 12, some CNT14 is not in direct contact with the surface of the fiber 11, but is fixed to the fiber 11 by being entangled with other CNT14. In addition, some CNT14 is fixed to the fiber 11 by being directly attached to the surface of the fiber 11 and entangled with other CNT14. Hereinafter, the fixation of CNT14 to these fibers 11 will be collectively referred to as attachment to the fiber 11. In addition, the state in which CNT14 is entangled or tangled includes the state in which a part of CNT14 is pressed against other CNT14.

[0038] In addition to the CNTs 14 that are directly attached to the surface of the fiber 11 as described above, there are also CNTs 14 that are not in direct contact with the surface of the fiber 11 but are fixed to the fiber 11 by entanglement with other CNTs 14. Therefore, the structure 12 of this example is composed of more CNTs 14 than a structure composed only of CNTs directly attached to the fiber surface, such as a structure of an existing composite material. That is, the number of CNTs 14 attached to the fiber 11 is greater than the number of attached roots in the existing structure, and the thickness of the structure 12 is also greater than that of the existing structure.

[0039] As described above, since a plurality of CNTs 14 are connected to each other on the surface without inclusions to form a structure 12, the composite material 10 exerts the electrical conductivity and thermal conductivity of the CNTs. In addition, since the CNTs 14 are not attached to the surface of the fibers 11 via inclusions, the CNTs 14 constituting the structure 12 are not easily peeled off from the surface of the fibers 11, and the mechanical strength of the composite material 10 and the secondary product containing the composite material 10 is improved. Moreover, since the thickness of the structure 12 is large, the above-mentioned mechanical strength is further improved. Therefore, even with fibers 11 having a larger diameter, a composite material 10 and a secondary product having improved mechanical strength can be obtained. In addition, although the case of a fiber-reinforced molded body as a secondary product is described below, the same is true for resin-impregnated fibers or multifilaments.

[0040] For example, in a fiber-reinforced molded body, a fiber bundle consisting of a plurality of composite materials 10 having a structure 12 is impregnated with a matrix resin and cured. Since the matrix resin of the fiber-reinforced molded body is impregnated with the structure 12 and cured, the structure 12 of each composite material 10 is fixed to the matrix resin together with the surface of the fiber 11. As a result, each fiber 11 is firmly bonded to the matrix resin, and the peel strength between the composite material 10 and the matrix resin is improved. In addition, by bonding the composite material 10 with the matrix resin in this way, the fiber reinforcement effect is obtained in the entire fiber-reinforced molded body.

[0041] As described above, around each fiber 11 in the fiber-reinforced molded body, there is a region (hereinafter referred to as a composite region) formed by impregnating the CNT 14 constituting the structure 12 with a matrix resin and curing it. Since there are CNTs 14 floating from the surface of the structure 12, the concentration (density) of CNTs 14 in the composite region decreases as it moves away from the composite material 10. In such a composite region, the high strength and flexibility of CNTs 14 are obtained by the composite of CNTs 14 and matrix resin. In addition, through such a composite region, the effect of relieving stress concentration, the restraining effect of suppressing the displacement of the composite material 10, the effect of effectively absorbing mechanical energy from the outside, etc. can be obtained.

[0042] For example, when energy such as vibration is transmitted between the fibers 11, the energy of the transmitted vibration is absorbed and attenuated via the friction of the composite region around each fiber 11. As a result, the fiber-reinforced molded body, for example, has improved vibration attenuation properties (vibration damping properties). In addition, when an external force is applied to the fiber-reinforced molded body and displacement occurs inside it, the fibers 11 inside the fiber-reinforced molded body are displaced. Due to the displacement of the fibers 11, the structure 12 in the composite region is stretched, and a restraint effect can be obtained through the network structure of the CNT 14. As a result, the characteristics of the CNT 14 can be brought into play and the elastic modulus of the fiber-reinforced molded body can be improved.

[0043] The properties of the fiber-reinforced molded body derived from CNT14 are manifested by the properties of the composite region and the effects of the composite region as described above. Since the structure 12 increases the number of CNT14 attached to the fiber 11 as described above and is a structure in which CNT14 is woven like fibers of a non-woven fabric, the properties of CNT derived from the fiber-reinforced molded body are higher than those of a composite material that does not have a structure such as the structure 12.

[0044] The structures 12 formed on the plurality of composite materials 10 are independent structures, and the structures 12 of one composite material 10 and the structures 12 of other composite materials 10 do not share the same CNTs 14. In other words, the CNTs 14 included in the structure 12 provided on one fiber 11 are not included in the structures 12 provided on other fibers 11.

[0045] For example, a sizing agent (not shown) is fixed on the surface of the CNT 14 constituting the structure 12. The sizing agent is composed of a cured or uncured product of a reaction-curable resin, a thermosetting resin, or a thermoplastic resin. The sizing agent is formed by a sizing treatment.

[0046] The sizing agent covers the surface of CNT14, and forms a containing portion covering the contact portion at the contact portion where CNT14 contacts each other. The containing portion makes the contact state of CNT14 more firm, making it more difficult for structure 12 to collapse. In the containing portion, the sizing agent is fixed to each CNT14 without entering between the contacting CNT14, so that the CNT14 in the contact portion are in direct contact with each other.

[0047] In addition, in the structure 12, a void portion (grid) surrounded by multiple CNTs 14 is formed, but in order not to hinder the impregnation of the matrix resin into the structure 12, it is preferred that the sizing agent does not fill the void portion. In order not to fill the void portion, the volume of the sizing agent is preferably less than 30% of the volume of the CNTs 14 of the structure 12. In addition, the above-mentioned sizing agent is formed on the surface of the CNTs 14, which is different from the fixed resin portion described later that enters the interior of the structure 12 and fixes the CNTs 14 on the fibers 11. In addition, the structure 12 may not be given a sizing agent.

[0048] As described above, the CNT14 attached to the fiber 11 has a curved shape. The curved shape of the CNT14 is a shape formed by a curved portion (curved portion) due to the presence of a five-membered ring and a seven-membered ring in the graphite structure of the CNT14, and is a shape that can be evaluated as a curved, bent, etc. CNT14 when observed by SEM. For example, the curved shape of the CNT14 refers to a curved portion having at least one or more places per average length of the utilization range of the CNT14 described later. Even in the case of its long length, the CNT14 of this curved shape is attached to the surface of the fiber 11 as a curved surface in various postures. In addition, the CNT14 of the curved shape is easy to form a space (gap) between the surface of the fiber 11 to which the CNT14 is attached or between the attached CNT14, and other CNT14 enters the space. Therefore, by using the CNT14 of the curved shape, compared with the case of using the CNT of a shape with higher linearity, the number of CNT14 attached to the fiber 11 (the number of CNT14 forming the structure 12) increases.

[0049] The length of CNT14 is preferably within the range of 0.1 μm or more and 10 μm or less. If the length of CNT14 is 0.1 μm or more, it is possible to more reliably form a structure 12 in which CNT14 are entangled with each other and directly contact or directly connected, and as described above, it is possible to more reliably form a space for other CNT14 to enter. In addition, if the length of CNT14 is 10 μm or less, CNT14 will not be attached across the fibers 11. That is, as described above, the CNT14 contained in the structure 12 provided on one fiber 11 will not be included in the structure 12 provided on other fibers 11.

[0050] The length of CNT14 is more preferably within the range of 0.2 μm or more and 5 μm or less. If the length of CNT14 is 0.2 μm or more, the number of attached CNT14 can be increased to thicken the structure 12. If the length of CNT14 is 5 μm or less, when CNT14 is attached to the fiber 11, CNT14 is not easy to aggregate and is easier to be evenly dispersed. As a result, CNT14 is more evenly attached to the fiber 11.

[0051] In addition, the CNTs attached to the fiber 11 may be mixed with CNTs with higher linearity or CNTs outside the length range described above. Even if there is a mixed presence, for example, CNTs with higher linearity may enter the space formed by CNT 14, thereby increasing the number of CNTs attached to the fiber 11.

[0052] The average diameter of CNT14 is preferably in the range of 1 nm to 15 nm, more preferably in the range of 3 nm to 10 nm. If the diameter of CNT14 is 15 nm or less, it is flexible and easy to adhere along the surface of fiber 11. It is also easy to entangle with other CNT14 and fix on fiber 11, so that the formation of structure 12 is more reliable. In addition, if the diameter of CNT14 is 10 nm or less, the bonding between CNT14 constituting structure 12 becomes firm. In addition, the diameter of CNT14 is a value measured using a transmission electron microscope (TEM: Transmission Electron Microscope) photograph. CNT14 can be a single layer or a multilayer, but preferably a multilayer.

[0053] As described above, by making CNT14 into a curved shape, the number of CNT14 attached to the fiber 11 can be increased compared to the case of using CNT with higher linearity, the thickness of the structure 12 can be increased, and the structure 12 in which CNT14 is woven like the fiber of a non-woven fabric can be formed. As a result, not only the mechanical strength is further improved, but also when an external force is applied to the secondary product to displace the fiber 11, the restraining effect of the structure 12 is increased, and the elastic modulus is further improved. In addition, the absorption effect of the composite area around the fiber 11 on mechanical energy is also increased, and the vibration attenuation characteristics of the secondary product are further improved.

[0054] As one of the improved mechanical strengths of the secondary product, the improvement in durability against repeated bending can be cited. As described above, in a fiber-reinforced molded body using a composite material 10 having CNT14 attached to the surface of the fiber 11, the durability against repeated bending can be improved by the improvement in peel strength brought about by the intervention of the structure 12 and the absorption effect of mechanical energy brought about by the composite region. As the number of CNT14 attached to the surface of the fiber 11 increases, the improvement in peel strength and the absorption effect of mechanical energy are further improved, thereby further improving the durability against repeated bending. The composite material 10 having such characteristics is preferably used as a spring material such as a coil spring or a leaf spring to which a load is repeatedly applied, and the secondary product containing the composite material 10 can be applied to various springs such as a coil spring or a leaf spring.

[0055] In addition, in a secondary product using the composite material 10, such as a fiber-reinforced molded body, the composite regions that are solidified by impregnating the matrix resin in the structure 12 are fixed to each other, thereby generating a cross-linked structure in which the fibers 11 are cross-linked to each other. The composite region obtained by solidifying the impregnated matrix resin has a higher hardness than the solidified matrix resin monomer, and at the same time has a large elastic limit, that is, it has high elasticity. In addition, the wear resistance of the composite region is higher than that of the matrix resin. Through the combination of such composite regions, the combination of the composite materials 10 becomes firm, and the durability of the fiber-reinforced molded body using the composite material 10 to repeated bending is improved. Since a cross-linked structure is formed when the distance between the composite materials 10 is close to the degree of contact between the structures 12, the greater the thickness of the structure 12, the more cross-linking is more advantageous. In addition, when the composite material 10 is made into a fabric or bundled like a multifilament, the cross-linked parts obtained by the composite regions being fixed to each other increase, and the effect brought by the cross-linked structure increases.

[0056] The thickness of each part of the structure 12 (the radial length of the fiber 11) can be obtained by, for example, sticking a part of the structure 12 on the surface of the fiber 11 to a transparent tape or the like to peel it off, and measuring the cross section of the structure 12 remaining on the surface of the fiber 11 by SEM or the like. In a manner that the measurement range of the specified length of the fiber 11 along the fiber axis direction is roughly evenly covered, the average value of the values ​​obtained by measuring the thickness of the structure 12 at 10 points in the measurement range is taken as the thickness of the structure 12. The length of the measurement range is, for example, 5 times the upper limit of the length range of the above-mentioned CNT14. The number of CNT14 attached to the fiber 11 can be evaluated by the thickness of the structure 12.

[0057] The thickness (average) of the structure 12 obtained as described above is in the range of 10 nm to 300 nm, preferably in the range of 15 nm to 200 nm, and more preferably in the range of 50 nm to 200 nm. If the thickness of the structure 12 is 200 nm or less, the impregnation of the resin between the fibers 11 is better.

[0058] [Method for producing composite material]

[0059] Next, the production of the composite material 10 is described. In this example, a fiber bundle 20 (see Figure 4 ) is used to illustrate the case where the composite material 10 is manufactured, but the composite material 10 can also be manufactured in the same manner by using the fiber 11 alone instead of the fiber bundle 20.

[0060] The fibers 11 constituting the fiber bundle 20 are not substantially entangled with each other, and the fiber axis directions of the fibers 11 are consistent. The fiber axis direction is the axial direction (extension direction) of the fiber 11. In this example, the fiber bundle 20 is composed of a plurality of fibers 11. The number of fibers 11 constituting the fiber bundle 20 is not particularly limited, and may be, for example, in the range of 100 or more and 10 million or less.

[0061] The entanglement of the fibers 11 in the fiber bundle 20 can be evaluated based on the degree of disorder of the fibers 11. For example, the fiber bundle 20 is observed at a certain magnification using a scanning electron microscope (SEM), and the lengths of a predetermined number of fibers 11 (e.g., 10 fibers) in the observed range (the range of the predetermined length of the fiber bundle 20) are measured. The degree of disorder of the fibers 11 can be evaluated based on the length deviation, the difference between the maximum and minimum values, and the standard deviation of the predetermined number of fibers 11 obtained from the measurement results. In addition, in the case where the fibers 11 are not substantially entangled with each other, for example, the degree of intertwining can be measured and judged according to the method for measuring the degree of intertwining of JIS L1013:2010 "Test Methods for Artificial Filament Yarns". The smaller the measured degree of intertwining, the less the fibers 11 in the fiber bundle 20 are entangled with each other.

[0062] The fiber bundle 20 in which the fibers 11 are substantially not entangled with each other or are less entangled with each other makes it easy to evenly open the fibers 11. This makes it easy to evenly attach the CNTs 14 to each fiber 11, and the resin is evenly impregnated in the fiber bundle 20, so that the composite material 10 contributes to the strength.

[0063] In order to attach CNT14 to each fiber 11 of the fiber bundle 20 and form a structure 12, the fiber bundle 20 is immersed in a CNT separation dispersion (hereinafter referred to as dispersion) in which CNT14 is separated and dispersed, and mechanical energy is given to the dispersion. Separation dispersion refers to the state in which CNT14 is physically separated one by one and dispersed in the dispersion medium without being entangled with each other, and refers to the state in which the proportion of aggregates of two or more CNT14 aggregated into bundles is less than 10%. Here, if the proportion of aggregates is more than 10%, the coagulation of CNT14 in the dispersion medium is promoted and the attachment of CNT14 to the fiber 11 is hindered.

[0064] like Figure 4 As shown in the example of , the attachment device 21 is composed of a CNT attachment tank 22, guide rollers 23 to 26, an ultrasonic generator 27, and a moving mechanism (not shown) for moving the fiber bundle 20 at a certain speed. A dispersion 28 is contained in the CNT attachment tank 22. The ultrasonic generator 27 irradiates ultrasonic waves to the dispersion 28 in the CNT attachment tank 22 from the lower side of the CNT attachment tank 22.

[0065] A fiber bundle 20 of a long length (e.g., about 100 m) without forming a structure 12 is continuously supplied to an attaching device 21. The supplied fiber bundle 20 is sequentially wound on guide rollers 23 to 26 and moved at a constant speed by a moving mechanism. The fiber bundle 20 without sizing agent attached to each fiber 11 is supplied to the attaching device 21. The sizing agent mentioned here is a slurry attached to the surface of the fiber 11 in order to prevent the fiber 11 from being entangled, etc., and is different from the above-mentioned sizing agent and fixing resin part.

[0066] The fiber bundle 20 is wound around the guide rollers 23 to 26 in an open state. The fiber bundle 20 wound around the guide rollers 23 to 26 can reduce the possibility of the fibers 11 being entangled with each other by applying appropriate tension. It is preferred to wind the fiber bundle 20 around the guide rollers 24 to 26 at a smaller winding angle (90° or less).

[0067] The guide rollers 23 to 26 are all flat rollers. Figure 5 As shown, the roller length (length in the axial direction) L1 of the guide roller 23 is sufficiently larger than the width WL of the fiber bundle 20 after fiber opening. The guide rollers 24 to 26 are also similar to the guide roller 23, and their roller lengths are sufficiently larger than the width WL of the fiber bundle 20 after fiber opening. For example, all the guide rollers 23 to 26 have the same size. In the fiber bundle 20 after fiber opening, a plurality of fibers 11 are arranged in the thickness direction (radial direction of the guide roller).

[0068] The guide rollers 24 and 25 among the guide rollers 23 to 26 are arranged in the CNT attachment tank 22. Thus, between the guide rollers 24 and 25, the fiber bundle 20 moves linearly in the dispersion 28 at a constant depth.

[0069] The moving speed of the fiber bundle 20 is preferably within the range of 0.5 m / min to 10000 m / min. The higher the moving speed of the fiber bundle 20, the higher the productivity, and the lower the moving speed, the more effectively and evenly the CNT14 can be attached, and the entanglement of the fibers 11 can be effectively suppressed. In addition, the less the entanglement of the fibers 11, the more the uniformity of the attachment of CNT14 to the fibers 11 can be improved. If the moving speed of the fiber bundle 20 is 100 m / min or less, the entanglement of the fibers 11 can be more effectively suppressed, and the uniformity of the attachment of CNT14 can be further improved. In addition, the moving speed of the fiber bundle 20 is more preferably within the range of 5 m / min to 50 m / min.

[0070] The ultrasonic generator 27 applies ultrasonic vibration as mechanical energy to the dispersion 28. As a result, a reversible reaction state in which the dispersed state of CNT14 and the condensed state of condensation alternately change is formed in the dispersion 28. If the fiber bundle 20 passes through the dispersion 28 in this reversible reaction state, when the dispersion state is transferred to the condensed state, the CNT14 is attached to each fiber 11 by the van der Waals force. The mass of the fiber 11 is more than 100,000 times greater than that of the CNT14, and the energy used to separate the attached CNT14 is greater than the energy of the ultrasonic vibration. Therefore, once the CNT14 is attached to the fiber 11, it will not be peeled off from the fiber 11 even under the action of the ultrasonic vibration after attachment. In addition, since the mass of each CNT14 is extremely small, it is alternately changed to a dispersed state and a condensed state by ultrasonic vibration.

[0071] By repeatedly transferring from a dispersed state to an aggregated state, a plurality of CNTs 14 are attached to each fiber 11 to form a structure 12. As described above, by using a curved CNT 14, other CNTs 14 enter a space formed between the CNT 14 and the surface of the fiber 11 to which the CNT 14 is attached or between the attached CNTs 14, thereby more CNTs 14 are attached to the fiber 11 to form a structure 12.

[0072] The frequency of the ultrasonic vibration applied to the dispersion 28 is preferably 40 kHz or more and 950 kHz or less. If the frequency is 40 kHz or more, the entanglement of the fibers 11 in the fiber bundle 20 is suppressed. In addition, if the frequency is 950 kHz or less, the CNT 14 is well attached to the fiber 11. In order to further reduce the entanglement of the fiber 11, the frequency of the ultrasonic vibration is preferably 100 kHz or more, and more preferably 130 kHz or more. In addition, the frequency of the ultrasonic vibration is more preferably 430 kHz or less.

[0073] In addition, the inventors found that by making the number of transitions of CNT14 from the dispersed state to the coagulated state 65,000 times, the number of CNT14 attached to the fiber 11 is approximately the maximum while ensuring the uniformity of the attachment of CNT14 to the fiber 11. In addition, the maximum number of attached roots varies according to the CNT concentration of the dispersion 28, and the higher the CNT concentration of the dispersion 28, the greater the maximum number of attached roots. However, if the CNT concentration of the dispersion 28 reaches a high concentration at which CNT17 cannot be in a dispersed state when ultrasonic vibration is applied, CNT17 will not attach to the fiber 11.

[0074] Therefore, it is preferable to determine the moving speed of the fiber bundle 20, the distance that the fiber bundle 20 moves in the dispersion 28 (the interval between the guide rollers 24 and 25), and the frequency of the ultrasonic vibration applied to the dispersion 28 so that the length of the period during which the fiber bundle 20 moves in the dispersion 28, that is, the time during which the fiber bundle 20 moves between the guide rollers 24 and 25 (hereinafter referred to as the immersion time) is 65,000 times or more the period of the ultrasonic vibration applied to the dispersion 28. That is, when the frequency of the ultrasonic vibration is fs (Hz) and the immersion time is Ts (seconds), it is preferable to satisfy "Ts ≥ 65,000 / fs". For example, if the frequency of the ultrasonic vibration is 130 kHz and the distance that the fiber bundle 20 moves in the dispersion 28 is 0.1 m, the moving speed of the fiber bundle 20 may be 12 m / min or less. Even when fiber bundle 20 is immersed in dispersion 28 in multiple times, if the total immersion time is 65,000 times or more of the ultrasonic vibration period, the number of attached CNTs 14 can be substantially maximized.

[0075] like Figure 6 As schematically shown, the ultrasonic vibration applied from the ultrasonic generator 27 generates a standing wave determined by the distribution of the sound pressure (amplitude) in the dispersion 28 in the CNT attachment tank 22. In the attachment device 21, the positions of the guide rollers 24 and 25 in the depth direction are adjusted in the dispersion 28 so that the fiber bundle 20 moves at the node of the standing wave of the ultrasonic vibration, that is, the depth at which the sound pressure is extremely low. Therefore, the depth of the fiber bundle 20 from the liquid surface of the dispersion 28 when moving in the dispersion 28 is determined as follows: when the depth is set to D, the wavelength of the standing wave of the ultrasonic vibration generated in the dispersion 28 is set to λ, and n is set to an integer greater than 1, "D=n·(λ / 2)" is satisfied. In addition, the wavelength λ of the standing wave can be obtained based on the sound velocity in the dispersion 28 and the frequency of the ultrasonic vibration applied from the ultrasonic generator 27.

[0076] As described above, by adjusting the depth of the fiber bundle 20 moving in the dispersion 28, the vibration of the fiber 11 caused by the sound pressure can be suppressed, the tangling of the fibers caused by the relaxation of the fibers can be prevented, the friction between the fibers 11 or between the CNTs 14 attached to the surface of each fiber 11 can be suppressed, and a structure 12 with a large thickness can be formed. The larger the diameter of the fiber 11, the greater the influence of the vibration caused by the standing wave. Therefore, by satisfying the depth condition of the fiber bundle 20 moving in the dispersion 28, a significant vibration suppression effect of the fiber 11 can be obtained. In addition, the fiber 11 is not easy to elongate in the fiber axis direction due to the sound pressure of the standing wave, and the plastic deformation of the fiber 11 in the fiber axis direction can be prevented. In addition, the depth of the fiber bundle 20 moving in the dispersion 28 can also deviate from the node of the standing wave to some extent. In this case, it is preferably within the range of n·λ / 2-λ / 8 or more and n·λ / 2+λ / 8 or less (n·λ / 2-λ / 8≤D≤n·λ / 2+λ / 8). Thereby, the yarn disorder of the fiber 11 due to the yarn relaxation can be made within the allowable range.

[0077] The fiber bundle 20 is drawn out from the dispersion 28 and then dried. The dried fiber bundle 20 is sequentially subjected to a sizing treatment and dried, thereby providing the structure 12 with a sizing agent. The sizing treatment can be performed by a general method.

[0078] The sizing agent is not particularly limited, and as mentioned above, various reaction curing resins, thermosetting resins, and thermoplastic resins can be used. For example, as thermosetting resins, epoxy resins, phenolic resins, melamine resins, urea resins (urea-formaldehyde resins), unsaturated polyesters, alkyd resins, thermosetting polyimides, and resins with reactive groups can be listed. In addition, as thermoplastic resins, general-purpose resins such as polyethylene, polypropylene, polystyrene, acrylonitrile / styrene (AS) resins, acrylonitrile / butadiene / styrene (ABS) resins, methacrylic resins (PMMA, etc.), vinyl chloride, polyamides, polyacetals, polyethylene terephthalate, ultra-high molecular weight polyethylene, engineering plastics such as polycarbonate, polyphenylene sulfide, polyetheretherketone, liquid crystal polymers, polytetrafluoroethylene, polyetherimide, polyarylate, super engineering plastics such as polyimide, etc. can be listed. In the sizing treatment, a solution in which a resin serving as a sizing agent is dissolved is preferably used, and the solution may be applied to the fiber bundle 20 , etc., so that the sizing agent can be attached to the CNTs 14 of the structure 12 .

[0079] [Dispersion liquid]

[0080] The dispersion 28 used when attaching CNT14 to the composite material 10 is prepared by, for example, adding long CNTs (hereinafter referred to as material CNTs) into a dispersion medium, cutting the material CNTs by a homogenizer, shear force, ultrasonic disperser, etc., to form CNT14 of a desired length, while achieving uniform dispersion of CNT14.

[0081] As the dispersion medium, water, alcohols such as ethanol, methanol, and isopropanol, or organic solvents such as toluene, acetone, tetrahydrofuran (THF), methyl ethyl ketone (MEK), hexane, n-hexane, ether, xylene, methyl acetate, and ethyl acetate, and mixtures thereof in any proportions can be used. The dispersion 28 does not contain a dispersant or a binder.

[0082] As described above, the material CNTs that form the basis of the curved CNT 14 are curved. Such material CNTs preferably have the same diameter. An example of a material CNT is Figure 7 The material CNT is preferably a material that can separate and disperse the CNTs even if the length of each CNT generated by cutting is large. Thus, a dispersion 28 in which CNTs 14 satisfying the above-mentioned length condition are separated and dispersed can be easily obtained.

[0083] In the composite material 10 of this example, as described above, since the CNT 14 in a curved shape is attached, other CNTs 14 enter the space formed between the CNT 14 and the surface of the fiber 11 to which the CNT 14 is attached or between the attached CNTs 14. As a result, more CNTs 14 are attached to the fiber 11. In addition, since the CNT 14 is firmly attached to the fiber 11 to form the structure 12, it is more difficult for the CNT 14 to be peeled off from the fiber 11. Moreover, in the fiber-reinforced molded body made using such a composite material 10, the properties derived from the CNTs are further improved.

[0084] The secondary product made of the composite material 10 as described above has improved mechanical properties such as vibration attenuation characteristics (vibration damping properties) and elastic modulus variation characteristics compared to the secondary products using the conventional composite materials. Regarding the elastic modulus variation characteristics, the increase in the elastic modulus of the fiber-reinforced molded body is suppressed relative to the increase in the collision speed with the fiber-reinforced molded body.

[0085] The concentration of CNT 14 in dispersion liquid 28 is preferably in the range of 0.003 wt % to 3 wt %. The concentration of CNT 14 in dispersion liquid 28 is more preferably in the range of 0.005 wt % to 0.5 wt %.

[0086] In the above-mentioned embodiment, the fixation of CNT to the fiber surface is carried out by the combination of the van der Waals force of the fiber and the CNT, but in addition to this, a bonding portion for strengthening the fixation of CNT to the fiber surface can also be provided. The bonding portion is, for example, an epoxy resin obtained by curing in a state of entering the gap formed between the fiber and the surfaces (peripheral surfaces) of the CNT directly attached (contacting) on ​​the fiber. The epoxy resin is dissolved in a solvent such as toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone (MIBK), butanol, ethyl acetate or butyl acetate to form a solution, in which a fiber bundle containing fibers forming a structure is immersed, and then heated. Thus, the uncured epoxy resin enters the gap formed between the fiber and the surfaces of CNT17 and cures.

[0087] In addition, when forming the bonding portion, the solution of the epoxy resin as the material of the bonding portion can also be emulsified and used. For example, emulsifying can be performed by adding emulsifiers such as nonionic emulsifiers to the solution obtained by dissolving the epoxy resin in a solvent. As the bonding portion, except for the epoxy resin, for example, phenolic resin, polyurethane resin, melamine resin, urea-formaldehyde resin, polyimide resin, etc. can also be used. In addition, the adhesive of silane coupling agent or inorganic system can also be used as the bonding portion.

[0088] [Second Embodiment]

[0089] The composite material of the second embodiment has a plurality of fixing resin portions for locally fixing a portion of the plurality of CNTs constituting the structure on the fiber surface. The composite material of the second embodiment is the same as the composite material of the first embodiment except that the fixing resin portion is provided instead of the sizing agent, and therefore substantially the same components are given the same reference numerals and their detailed description is omitted.

[0090] exist Figure 8 In the composite material 10A, a plurality of fixing resin portions 38 are provided for locally fixing a portion of the plurality of CNTs 14 constituting the structure 12 on the surface of the fiber 11. The composite material 10A may be a resin-impregnated fiber or a reinforcing fiber constituting a multifilament or a fiber-reinforced molded body.

[0091] The fixing resin part 38 is a resin solidified into a granular state that reaches the surface of the fiber 11 from the surface of the structure 12. The fixing resin part 38 is fixed to the surface of the fiber 11 attached to the bottom thereof, and is fixed to the CNT 14 of the structure 12 covered by the portion above the bottom. In this way, the fixing resin part 38 is fixed to both the surface of the fiber 11 and a portion of the CNT 14, thereby fixing the CNT 14 to the fiber 11.

[0092] As described above, the fixing resin portion 38 is a component that locally fixes a portion of the plurality of CNTs 14 constituting the structure 12 on the surface of the fiber 11, and is arranged to be dispersed on the surface of the fiber 11, and the CNTs 14 of the structure 12 are fixed at each location. The upper portion of the fixing resin portion 38 dispersed in this way is exposed on the surface of the structure 12, and is also observed to be dispersed on the surface of the structure 12.

[0093] like Fig. 9 As schematically shown, the fixing resin portion 38 is formed in the radial direction of the fiber 11 (the thickness direction of the structure 12) within the range from the surface of the structure 12 to the surface of the fiber 11, and is fixed to the surface of the fiber 11 and to the portion of the CNT 14 contained therein.

[0094] Among the CNTs 14 of the structure 12, there are cases where the portion attached to the surface of the fiber 11, the portion overlapping with other CNTs 14, or the portion clamped is fixed to the fixing resin portion 38. In addition, there are also CNTs 14 whose ends or central portions are fixed to the fixing resin portion 38. In this way, the CNTs 14 fixed to the fixing resin portion 38 are firmly fixed to the fiber 11 by the fixing resin portion 38. As described above, the portion of the CNT 14 not covered by the fixing resin portion 38 is attached to the surface of the fiber 11 by the van der Waals force, and therefore, compared with the portion fixed by the fixing resin portion 38, it can be detached from the surface of the fiber 11 and floated under the action of a weaker force, and can move on the surface of the fiber 11. In addition, on the surface of the structure 12, the portion of the CNT 14 not fixed by the fixing resin portion 38 is in a free state that can be detached from the surface of the structure 12 and floated.

[0095] As described above, by fixing the CNTs 14 of the structure 12 with the fixing resin portion 38, local detachment of the structure 12 is suppressed compared to the case where the CNTs 14 of the structure 12 are not fixed with the fixing resin portion 38. As a result, the properties derived from the CNTs of the fiber-reinforced molded body are further improved. By constraining the CNTs 14 of the fixing resin portion 38 on the surface of the fiber 11, it is easy for the current from the fiber 11 to flow, which can help improve the conductivity of the fiber-reinforced molded body.

[0096] In addition, all CNTs 14 constituting the structure 12 may be fixed to the fibers 11 by the fixing resin portion 38, but it is sufficient to fix only a portion of the CNTs 14. That is, at least a portion of the CNTs 14 constituting the structure 12 may be fixed by the fixing resin portion 38. Since the CNTs 14 form a film as the structure 12 having a non-woven fabric-like structure, the performance can be exerted if at least a portion of the CNTs 14 constituting the structure 12 is fixed.

[0097] The number of fixed resin parts 38 per 5 μm square in the surface (peripheral surface) of the structure 12 when viewed from above, i.e., the number ratio N, is preferably within a range of 27 or more and 130 or less. In addition, on the surface of the structure 12 when viewed from above, the area ratio S of the fixed resin parts 38 is preferably within a range of 6% or more and 45% or less, and more preferably within a range of 7% or more and 30% or less. The area ratio S refers to the ratio of the area of ​​the surface of the structure 12 covered by the plurality of fixed resin parts 38 to the surface area of ​​the structure 12 when viewed from above. Suppose the surface area of ​​the structure 12 within a specified range is S2, and the area of ​​the surface of the structure 12 covered by each fixed resin part 38 within a specified range is S1, then the area ratio S is calculated by "S = S1 / S2×100 (%)". Viewing from above means viewing the peripheral surface of the structure 12 from a direction perpendicular to the fiber axis direction of the fiber 11.

[0098] In addition, since the thickness of the structure 12 is sufficiently small compared to the radius of the fiber 11, the surface of the structure 12 can be regarded as the surface of the fiber 11, and for each fixing resin portion 38, the area of ​​the surface of the structure 12 covered by the fixing resin portion 38 and the area of ​​the surface of the fiber 11 covered can be regarded as being approximately the same. Therefore, the above-mentioned number ratio N can be regarded as the number of fixing resin portions 38 per 5 μm square in the surface (peripheral surface) of the fiber 11 when viewed from above, that is, the number ratio, and the above-mentioned area ratio S can be regarded as the ratio of the area of ​​the surface of the fiber 11 covered by the fixing resin portion 38 to the surface area of ​​the fiber 11 when viewed from above.

[0099] In practice, when counting the number ratio N and finding the area ratio S, for example, the structure 12 formed on the peripheral surface of the fiber 11 is observed from above using an SEM photograph. Then, an observation frame of 5 μm square is set on the top view observation image of the structure 12 in the SEM photograph, and the number of the fixing resin parts 38 in the observation frame is counted, and the number is set as the number ratio N. Similarly, the area of ​​each fixing resin part 38 observed in the observation frame is respectively found, and the sum of the areas of these fixing resin parts 38 is set as the area S1, and the area of ​​the observation frame is set as the surface area S2, and the area ratio S can be calculated. In addition, the observation frame G can be set to have its center of gravity coincident with the radial center of the fiber 11.

[0100] If the number ratio N and the area ratio S are increased, the CNT 14 can be reliably fixed on the surface of the fiber 11, and the local detachment of the structure 12 can be reduced. In addition, if the number ratio N and the area ratio S are reduced, the portion of the CNT 14 not fixed by the fixing resin portion 38 increases, and the degree of freedom of the CNT 14 and thus the degree of freedom of the structure 12 is improved.

[0101] If the above-mentioned number ratio N is 27 or more or the area ratio S is 6% or more, the CNT 14 can be reliably fixed to the fiber 11 by the fixing resin portion 38, and the effect of reducing the local detachment of the structure 12 can be reliably obtained, and the characteristics derived from CNTs of the fiber-reinforced molded body can be further improved. In addition, if the number ratio N is 130 or less or the area ratio S is 45% or less, the CNT 14 covered by the fixing resin portion 38 as a whole can be sufficiently reduced. As a result, the characteristics derived from CNTs of the fiber-reinforced molded body, especially the effect based on the floating of a part of the CNT 14 from the surface of the structure 12, can be reliably obtained. The number ratio N and the area ratio S are preferably both within the above ranges.

[0102] As described later, under certain conditions, the area ratio S can be increased or decreased in proportion to the number ratio N, so that the number ratio N and the area ratio S can satisfy the above conditions at the same time. In addition, when the above area ratio S is satisfied, the total area of ​​the fixing resin portion 38 within a 5 μm square on the surface of the structure 12 when viewed from above is 1.5 μm. 2 ~11.25μm 2 within the range.

[0103] In addition, the substantial area of ​​each fixing resin portion 38 on the surface of the structure 12 is preferably 0.03 μm 2 Above and 1.12μm 2 If the area of ​​each fixing resin portion 38 is 0.03 μm 2 As described above, it is possible to obtain a fixing force that can reliably fix the CNT 14 on the surface of the fiber 11. In this case, the effect of reducing the local detachment of the structure 12 can also be reliably obtained. If the area of ​​each fixing resin portion 38 is 1.12 μm 2 Then, sufficient freedom of CNT 14 can be obtained.

[0104] The area ratio S, number ratio N, and substantial areas of the fixing resin portions 38 in a plan view can be obtained using image analysis software (eg, Winroof 2015 (manufactured by Mitani Corporation)).

[0105] As described above, a fiber-reinforced molded body or the like produced from composite material 10A including structure 12 composed of curved CNTs 14 has improved properties derived from CNTs 14 compared to conventional fiber-reinforced molded bodies.

[0106] Due to the restraining effect for suppressing the displacement of the fiber 11 caused by the composite region, the elastic modulus of the fiber-reinforced molded body using the composite material 10A is improved. In addition, the restraining effect brought by the composite region between the fibers of the fiber-reinforced molded body suppresses the increase in the elastic modulus of the fiber-reinforced molded body relative to the increase in the collision speed to the fiber-reinforced molded body. As a result, the speed dependence of the elastic modulus becomes smaller. Furthermore, the resistance to the development of interlayer delamination cracks can be further increased by fixing the resin portion 38.

[0107] The manufacturing process of the composite material 10A is the same as that of the first embodiment except that a fixing resin imparting process for forming the fixing resin portion 38 is performed instead of a sizing process for attaching a sizing agent to the surface of the structure 12. That is, by applying a fixed resin to the surface of the structure 12 from the dispersion 28 (see Figure 2 ) and dried, the fiber bundle 20 is subjected to a fixing resin imparting treatment to form a fixing resin portion 38. The fixing resin imparting treatment may be a treatment corresponding to the material or form of the fixing resin portion 38.

[0108] As a preferred method for the fixing resin imparting treatment, there can be mentioned a method using an emulsion type treatment liquid in which an uncured resin (polymer) to be the fixing resin portion 38 is dispersed in a dispersion medium in the form of droplets. In this method, an adhesion treatment of forming a fiber bundle 20 with a structure 12 formed on each fiber 11 and contacting the fiber bundle 20 with a treatment liquid to adhere the resin to the fiber bundle 20, and a curing treatment of evaporating the dispersion medium after the adhesion treatment and curing the resin to form the fixing resin portion 38 are sequentially performed.

[0109] The resin in the treatment liquid uses a resin with curing properties, that is, a curing resin. As the curing resin, it can be any of a thermosetting resin, a reaction curing resin, etc. In addition, the cured resin obtained by curing the curing resin can also be a thermoplastic resin. Specifically, it can be: epoxy resin or polyurethane resin, urea resin, polyimide resin, vinyl acetate, acrylic resin, olefin resin, vinyl chloride, phenolic resin, melamine resin, rubber, silicone resin or inorganic adhesive, etc., but it is not limited to these.

[0110] In addition, the fixing resin portion 38 preferably has a high affinity with the matrix resin. Therefore, the fixing resin portion 38 and the matrix resin are preferably a combination of polar resins or a combination of non-polar resins, for example.

[0111] As the dispersion medium of the treatment liquid, for example, water, ethanol, acetone, MEK, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, toluene and xylene can be mentioned. These dispersion media can be used alone or in combination of two or more. As the dispersion medium, water is preferred from the perspective of usability and safety. The resin concentration in the diluted treatment liquid is appropriately adjusted to the target adhesion amount of the fixed resin portion 38 (the mass ratio (wt%) of the fixed resin portion 38 relative to the composite material 10A). The adhesion amount of the fixed resin portion 38 on the surface of the fiber 11 after the drying treatment is preferably in the range of 0.1wt% to 5.0wt%, more preferably in the range of 0.3wt% to 3.0wt%.

[0112] The particle size of the resin in the treatment liquid is preferably within the range of 0.05 μm or more and 1 μm or less, and more preferably within the range of 0.1 μm or more and 0.4 μm or less. The particle size of the resin in the treatment liquid can be determined by laser analysis. If the particle size of the resin in the treatment liquid is 0.05 μm or more, the CNT 14 can be reliably fixed on the surface of the fiber 11. If the particle size of the resin in the treatment liquid is 1 μm or less, the resin can reliably enter between the CNTs 14 constituting the structure 12, and can reliably prevent the CNTs 14 from being covered by the resin. In addition, if the particle size of the resin in the treatment liquid is 0.1 μm or more, it is a resin size sufficient to fix the non-woven fabric-like structure 12. If the particle size of the resin in the treatment liquid is 0.4 μm or less, local fixation of the structure 12 can be achieved.

[0113] When an emulsion type treatment liquid containing a resin having a particle size in the range of 0.1 μm or more and 0.4 μm or less is used, it is possible to form a plurality of particles each having an area of ​​0.03 μm 2 Above and 1.12μm 2 When a treatment liquid adjusted so that the adhesion amount of the fixing resin part 38 after the curing treatment is about 0.1 mass % to 5.0 mass % is used, the number ratio N can be within the range of 27 or more and 130 or less.

[0114] The method of the adhesion treatment using the treatment liquid is not particularly limited, and examples thereof include a roll immersion method, a roll contact method, a spray method, etc. In addition, the method of the curing treatment is not particularly limited, and examples thereof include hot air, a hot plate, a heating roller, various infrared heaters, etc.

[0115] Fig.10A flat belt 40 is shown as an example of a product using the composite material 10. The flat belt 40 is used, for example, as a power transmission belt, etc. The flat belt 40 has a structure in which a reinforcing cloth 42 and a surface rubber layer 43 are laminated on both sides of an inner rubber layer 41, and a cord core 45 is buried in the inner rubber layer 41.

[0116] The inner rubber layer 41 is formed of, for example, nitrile rubber, carboxylated nitrile rubber, hydrogenated nitrile rubber, chloroprene rubber, chlorosulfonated polyethylene, polybutadiene rubber, natural rubber, EPM, EPDM, polyurethane rubber, acrylic rubber, etc. The reinforcing cloth 42 is provided to improve the durability of the flat belt 40, and is, for example, a woven or braided cloth made of polyester fiber, nylon fiber, aramid fiber, glass fiber, carbon fiber, cotton, etc. The surface rubber layer 43 is provided to obtain a predetermined frictional force between the flat belt 40 and the conveyed object or power transmission device, and is, for example, formed of nitrile rubber, carboxylated nitrile rubber, hydrogenated nitrile rubber, chloroprene rubber, chlorosulfonated polyethylene, polybutadiene rubber, natural rubber, EPM, EPDM, polyurethane rubber, acrylic rubber, silicone rubber, etc.

[0117] As the cord core 45, the above-mentioned multifilament 15 in which the composite material 10 is bonded to each other by the matrix resin 16 impregnated into the structure 12 and cured is used. The fiber axis direction of the multifilament 15 of the cord core 45 is consistent with the longitudinal direction of the flat belt 40 (the running direction of the flat belt 40, the arrow X direction). In addition, the cord core 45 is arranged at a predetermined pitch in the width direction orthogonal to the longitudinal direction of the flat belt 40. In the case of using twisted multifilaments as the cord core 45, in order to suppress the oblique movement of the belt, it is preferable to alternately arrange S-twisted cord cores and Z-twisted cord cores. In this way, since the flat belt 40 uses the multifilament of the composite material 10 as the cord core 45, the elongation due to tension or compression is small, and the durability against repeated bending is high.

[0118] Although the above description uses a flat belt as an example, composite materials can be used as the cord core of various belts. In particular, composite materials are suitable as the cord core of toothed belts represented by synchronous belts, V-belts, and V-ribbed belts. Fig.11 The example shown is an example of using the multifilament 15 as the cord core 45 of the V-belt 50. Fig.12 The illustrated example is an example in which the multifilament 15 is used as the cord core wire 45 of the timing belt 60 . Fig.11 The V-belt 50 has a structure in which a base fabric 51, a bottom rubber layer 52, an adhesive rubber layer 53, a back rubber layer 54, and a top fabric layer 55 are laminated, and the cord core wire 45 is buried in the adhesive rubber layer 53. Fig.12The timing belt 60 has a rubber layer 61 composed of a belt body 61a and a plurality of tooth portions 61b, and a tooth cloth 62 covering the surface of the rubber layer 61 on the tooth portion 61b side, and has a structure in which the cord core wire 45 is buried in the belt body 61a.

[0119] Fig.13 The results of evaluating the interfacial bonding strength between glass fiber and matrix resin according to the presence or absence of CNT attachment are shown. In this evaluation, a plurality of test pieces A obtained by embedding CNT composite fibers using glass fiber as fiber 11 in soft epoxy resin and a plurality of test pieces B obtained by embedding glass fiber (raw fiber) in soft epoxy resin are prepared and evaluated by a fragmentation method.

[0120] For test piece A, in the same order as above, the glass fiber (raw yarn) is passed through the dispersion 28 irradiated with ultrasound, so that the CNT 14 is fully and evenly attached to the glass fiber, thereby forming a fiber 11 having a structure 12 formed on its surface. In addition, no sizing agent or bonding portion is given. A glass fiber with a structure 12 formed on the surface is taken out, and the glass fiber is buried in a soft epoxy resin, thereby preparing test piece A. The diameter of the glass fiber (raw yarn) is about 16μm. The SEM photograph obtained by observing the structure 12 formed on the surface of the glass fiber used in test piece A is as shown Fig.14 shown.

[0121] A single glass fiber (raw yarn) to which no CNTs were attached was buried in a soft epoxy resin to prepare test piece B. The preparation conditions of test piece B were the same as those of test piece A except that no CNTs were attached to the glass fiber.

[0122] A tensile load was applied to each test piece A and each test piece B until the glass fiber was not cut, and then the length of each cut piece of glass fiber of a certain length in each test piece was measured, and the average length of the cut pieces (cut fiber length) was calculated for each test piece.

[0123] The cut fiber lengths of the test pieces A and B measured by the fragmentation method as described above are as follows: Fig.13 As shown. Comparing the case where the test piece A, i.e., CNT14 is attached to the glass fiber, with the case where the CNT is not attached to the glass fiber, it can be seen that the cut fiber length is shortened and the interface bonding strength between the glass fiber and the matrix resin is higher. In the test pieces A and B, since the diameter of the glass fiber is more than 10 μm, the stress concentration at the interface becomes significant, but in the test piece A, since CNT14 exists on the surface of the glass fiber, the elastic modulus of the resin at the interface is increased, and the interface bonding strength is improved by easing the stress concentration.

[0124] Explanation of symbols

[0125] 10, 10A: composite materials;

[0126] 11: Fiber;

[0127] 12: structure;

[0128] 14: Carbon nanotubes;

[0129] 20: fiber bundle;

[0130] 38: Fixing resin part.

Claims

1. A composite material, characterized in that: include: fiber; as well as The structure is composed of a plurality of carbon nanotubes, forming a network structure in which the carbon nanotubes are directly in contact with each other, and the carbon nanotubes attached to the surface of the fiber are directly attached to the surface of the fiber, wherein the carbon nanotube is in a curved shape with a curved portion, The structure is a structure in which the carbon nanotubes are woven into a non-woven fabric in a fibrous form, the structure has a void portion surrounded by the plurality of carbon nanotubes, and the thickness of the structure is within a range of 50 nm to 300 nm. A sizing agent is fixed on the surface of the plurality of carbon nanotubes, the volume of the sizing agent is 30% or less relative to the volume of the plurality of carbon nanotubes, and the sizing agent is fixed in a manner not to fill the gaps. During the attachment, the fiber is immersed in a dispersion to which ultrasonic vibration is applied and in which the carbon nanotubes are dispersed, and moves in the dispersion. The depth of the distance from the liquid surface of the dispersion to which the fiber moves is set to D, and the wavelength of the standing wave of the ultrasonic vibration generated in the dispersion by the ultrasonic wave is set to λ. When n is set to an integer greater than 1, n·λ / 2-λ / 8≤D≤n·λ / 2+λ / 8 is satisfied.

2. The composite material according to claim 1, characterized in that The fiber has a diameter in the range of 5 μm or more and 100 μm or less.

3. A method for manufacturing a composite material, characterized in that: include: an ultrasonic step of applying ultrasonic vibration to a dispersion in which a plurality of carbon nanotubes having a curved shape and a curved portion and contained in the carbon nanotube attachment groove are dispersed; as well as an attachment step of immersing fibers in the dispersion liquid to which the ultrasonic vibration is applied, so that the plurality of carbon nanotubes are attached to the fibers to form a structure on the surface of the fibers, In the attachment process, the long fiber is moved linearly in the dispersion at a specified depth between guide rollers arranged in the carbon nanotube attachment groove, the depth of the distance the fiber moves from the liquid surface of the dispersion is set to D, the wavelength of the standing wave of the ultrasonic vibration generated in the dispersion by the ultrasonic process is set to λ, and when n is set to an integer greater than 1, n·λ / 2-λ / 8≤D≤n·λ / 2+λ / 8 is satisfied.

4. The method for producing a composite material according to claim 3, characterized in that: In the ultrasonic step, the frequency of the ultrasonic vibration is within a range of 40 kHz to 950 kHz.

Citation Information

Patent Citations

  • CNT / carbon fiber composite material, fiber-reinforced molded article using the composite material and method for producing composite material

    JP2013076198A

  • Composite material production method and composite material

    CN107429477A

  • Carbon nanotube assembly and its manufacturing method

    JP2008201626A

  • Apparatus for textile processing and method of manufacturing

    US20180230634A1