A bismuth oxybromide-lignin composite photocatalyst and its preparation method and application
By combining with lignin and synthesizing BiOBr/Lignin composite photocatalyst by hydrothermal method, the lack of performance problems of BiOBr in the photocatalytic process was solved, and the effect of improving the photocatalytic reaction performance and enhancing the stability of the catalyst was achieved.
Patent Information
- Application Number
- CN202210492405.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-07
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-05-07
AI Technical Summary
Bismuth bromine oxide (BiOBr) has disadvantages such as poor adsorption performance, low quantum efficiency, rapid recombination of electron-hole pairs and small specific surface area during photocatalysis, which weakens its catalytic degradation performance.
By combining with lignin, a bismuth bromine oxide-lignin composite photocatalyst (BiOBr/Lignin) was synthesized by hydrothermal method, and the catalytic performance was enhanced by the high specific surface area and functional groups of lignin.
The photocatalytic reaction performance of BiOBr is improved, the absorption of visible light and the concentration of pollutants around the catalyst are enhanced, the original shortcomings of BiOBr are overcome, and the stability and recycling efficiency of the catalyst are high.
Smart Images

Figure CN114733534B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of environmental materials, in particular to industrial wastewater such as printing and dyeing and pulping and papermaking, and specifically to a bismuth oxybromide-lignin composite photocatalyst and a preparation method and application thereof. Background Art
[0002] With the development of industrialization, environmental pollution has become a serious problem, especially water pollution, among which the wastewater discharge of pulp and paper industry and printing and dyeing industry has ranked at the forefront of my country's industrial wastewater discharge. The wastewater is characterized by high content of various organic matter and is therefore not easy to treat. Advanced oxidation processes (AOPs), such as ozone, Fenton and photo-Fenton processes, photolysis, photocatalysis, etc., have attracted considerable research interest, thanks to the highly active intermediates (·O2 - and ·OH). Photocatalysis is considered an effective method for removing water pollutants because of its excellent advantages such as mild reaction conditions, simple operation process, high efficiency and low cost. In the photocatalytic process, sunlight is converted into sustainable chemical energy or electrical energy, and active substances with strong oxidizing power are generated, including holes, superoxide radicals and hydroxyl radicals. This oxidizing substance can effectively convert harmful organic pollutants into small molecules with low toxicity without causing secondary pollution. Therefore, semiconductor photocatalysis technology is a very promising environmental remediation technology.
[0003] Bismuth oxybromide (BiOBr) has a bandgap of 2.7-2.9 eV and is a narrow-bandgap semiconductor with good visible light response and high photogenerated electron-hole separation efficiency. The excellent performance of BiOBr mainly comes from its layered structure, which consists of [Bi2O2] sheets and double halogen atom sheets interlaced. Bi and O are linked by strong covalent bonds within the Bi2O2 layers. The special internal electric field between the bismuth oxide layers and the halogen atoms can effectively separate electrons and holes, making BiOBr materials widely used in the degradation of dyes, various phenols, water pollutants and many antibiotics. However, BiOBr has some disadvantages such as poor adsorption performance, low quantum efficiency, rapid recombination of electron-hole pairs and small specific surface area, which weaken the catalytic degradation performance. Constructing composite materials is an effective way to improve the separation efficiency of photogenerated electron-hole pairs in photocatalysts. Lignin is one of the most abundant renewable aromatic polymers in nature, and a large amount of lignin is produced as a by-product every year in the pulp and paper industry. Lignin is cheap, easily degradable and low in toxicity. It is considered an effective substitute for petroleum fuels and has been widely used in the development of new materials. There is no report on the preparation of BiOBr / Lignin composite photocatalysts by combining BiOBr and lignin. Lignin is formed into biochar by hydrothermal method, which can effectively enhance the photocatalytic effect of BiOBr. Summary of the invention
[0004] In order to solve the current shortcomings of bismuth oxybromide (BiOBr), the purpose of the present invention is to provide a bismuth oxybromide-lignin composite photocatalyst and its preparation method and application, so as to enhance the visible light catalytic effect of BiOBr, so as to apply it to actual wastewater treatment.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] The first object of the present invention is to provide a bismuth oxybromide-lignin composite photocatalyst, which comprises bismuth oxybromide and lignin, wherein the mass of the lignin is 1wt% to 12wt% of the mass of the bismuth oxybromide. Lignin, as a byproduct of the pulp and paper industry, is abundant in source, has a large specific surface area and rich functional groups, and the biochar formed by the hydrothermal method has many pores, can effectively adsorb pollutants, and enhance photocatalytic performance.
[0007] The second object of the present invention is to provide a method for preparing the above-mentioned bismuth oxybromide-lignin composite photocatalyst. Commonly used methods for synthesizing bismuth oxybromide include hydrothermal method, hydrolysis method, precipitation method, sol-gel method and microwave method. Among them, the hydrothermal method is the simplest and most convenient to operate, and the morphology of the synthesized bismuth oxybromide is easy to control and has good crystallinity. The steps for synthesizing the bismuth oxybromide-lignin composite photocatalyst by the hydrothermal method are as follows: disperse the bromide salt and lignin in a dispersant to obtain a dispersion, dissolve the bismuth salt in an alcohol reagent to obtain a bismuth salt solution; add the bismuth salt solution to the dispersion and mix evenly to obtain a reaction solution; pour the reaction solution into a hydrothermal kettle, and heat the hydrothermal kettle to cause the reaction solution to undergo a hydrothermal reaction. After the reaction is completed, cool to room temperature, and the resulting product is successively separated, washed, and vacuum dried at a temperature of 50-60°C to obtain a bismuth oxybromide-lignin composite photocatalyst (BiOBr / Lignin composite photocatalyst)
[0008] The main chemical reactions involved in the above hydrothermal reaction process are as follows: Bi and O in the reaction solution are linked by covalent bonds to form a [Bi2O2] layered structure, which then forms a BiOBr layered structure with a double Br layer. Lignin is converted into biochar through hydrothermal reaction, and BiOBr grows on the biochar to finally obtain a BiOBr / Lignin composite photocatalyst.
[0009] Preferably, the molar ratio of the bismuth salt to the bromide salt is 1:1 to 1:2.
[0010] Preferably, the temperature of the hydrothermal reaction is 140-200° C. and the time is 24-48 hours.
[0011] Preferably, the dispersant is water, nitric acid or sulfuric acid; and the alcohol reagent is anhydrous ethanol, ethylene glycol or isopropanol.
[0012] Preferably, the lignin is at least one of alkali lignin and lignin sulfonate; the bismuth salt is any one of bismuth nitrate, bismuth sulfate, bismuth chloride or bismuth acetate; and the bromide salt is any one of potassium bromide and sodium bromide.
[0013] The third object of the present invention is to provide the use of the bismuth oxybromide-lignin composite photocatalyst in treating wastewater under visible light as in the first object. Further preferably, the wastewater is printing and dyeing wastewater or pulping and papermaking wastewater.
[0014] Compared with the prior art, the present invention has the following advantages:
[0015] (1) The BiOBr / Lignin composite photocatalyst prepared by the present invention effectively utilizes lignin, a by-product of the pulp and paper industry, thereby achieving sustainable utilization of resources and can also treat wastewater from the pulp and paper industry.
[0016] (2) The BiOBr / Lignin composite photocatalyst prepared by the method of the present invention overcomes the shortcomings of BiOBr such as poor adsorption performance, low quantum efficiency, rapid recombination of electron-hole pairs and small specific surface area, and increases the concentration of pollutants around the catalyst, thereby enhancing the photocatalytic reaction performance of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 XRD patterns of the products prepared in Comparative Example and Examples 1 to 5;
[0018] Figure 2 Scanning electron micrographs of BiOBr (a), Biochar (b) and BiOBr / 2wt% Lignin (cd);
[0019] Figure 3 It is the X-ray energy spectrum (EDS) of BiOBr / 2wt%Lignin;
[0020] Figure 4 XPS spectra of BiOBr4 and BiOBr / 2wt% Lignin (a), and high-resolution XPS spectra of Br, Bi, O and C elements (be). DETAILED DESCRIPTION
[0021] The present invention is further described below in conjunction with the examples so that those skilled in the art can better understand the present invention and implement it, but the examples are not intended to limit the present invention. The raw materials or reagents used in the following examples are all commercially available products.
[0022] Embodiment 1:
[0023] 1g of alkaline lignin was placed in a beaker and dried in an oven at 40°C for 30 minutes before use. 4mmol Bi(NO3)3·5H2O was dissolved in 30mL of anhydrous ethanol and stirred evenly by ultrasonication to obtain a Bi(NO3)3·5H2O solution; 4mmol KBr and 0.0244g of lignin were added to 20ml of distilled water respectively and stirred evenly to obtain a dispersion; then the Bi(NO3)3·5H2O solution was added to the dispersion containing KBr and lignin, ultrasonicated for 30min, and then stirred vigorously for 30min to obtain a reaction solution; the reaction solution was poured into a 100mL stainless steel hydrothermal autoclave lined with polytetrafluoroethylene, and placed in an oven and heated at 160°C for 24h to perform a hydrothermal reaction; after the reaction was completed, the obtained product was separated, washed, and dried in sequence to obtain a bismuth oxybromide-lignin composite photocatalyst, namely, a BiOBr / 2wt% Lignin photocatalyst (2wt% represents the mass percentage of lignin in the BiOBr catalyst), marked as BL2.
[0024] Comparative Example 1
[0025] Compared with Example 1, in the comparative example, when preparing the dispersion liquid, the amount of lignin added was 0 g, that is, no lignin was added to obtain the BiOBr photocatalyst.
[0026] Example 2 to Example 5
[0027] Compared with Example 1, the difference between Examples 2 to 5 is that the amount of lignin added is different, and the other processes are the same as Example 1. The amounts of lignin added in Examples 2 to 5 are: 0.0122g, 0.0488g, 0.0976g, and 0.122g, respectively; the products obtained in Examples 2 to 5 are respectively recorded as BiOBr / 1wt%Lignin (BL1), BiOBr / 4wt%Lignin (BL4), BiOBr / 8wt%Lignin (BL8), and BiOBr / 10wt%Lignin (BL10).
[0028] Photocatalytic performance test
[0029] The photocatalytic performance of the photocatalysts prepared in Examples 1-5 and the comparative example was tested respectively, and the method was as follows: 50 mg of the photocatalyst was added to 250 mL of a 30 mg / L rhodamine B solution, irradiated with a 300w Xe lamp (a 420 nm cutoff filter was installed at the outlet of the light source), and the degradation rate of rhodamine B was tested after 1 hour. The results are shown in Table 1 below.
[0030] Table 1 Degradation rate of rhodamine B by photocatalysts prepared in Examples 1-5 and Comparative Examples
[0031]
[0032] It can be seen from Table 1 that the photocatalytic efficiency of the composite catalyst doped with lignin is higher than that of pure BiOBr, and with the increase of the lignin doping amount, the catalytic efficiency of the composite catalyst first increases and then decreases, among which BL2 has the best effect.
[0033] The BiOBr / 2wt% Lignin that had been tested for catalytic performance was centrifuged and taken out from the Rhodamine B solution. After washing and drying, the process was repeated three times for treating 250 mL of a 30 mg / L Rhodamine B solution. The solution was irradiated with a 300w Xe lamp (a 420 nm cutoff filter was installed at the outlet of the light source). The degradation rate of Rhodamine B after 1 hour is shown in Table 2 below:
[0034] Table 2 Degradation rate of Rhodamine B after BiOBr / 2wt% Lignin was reused three times
[0035]
[0036] From Table 2, it can be seen that after the three series of repeated experiments, the catalytic effect of the catalyst was only slightly reduced, which shows that the catalyst has good repeatability and stability.
[0037] Example 6
[0038] Put 1g of lignin sulfonate into a beaker and dry it in an oven at 40℃ for 30 minutes to obtain lignin. Dissolve 4mmol BiCl3 in 30mL of anhydrous ethanol and stir evenly to obtain BiCl3 solution; add 4mmol KBr and 0.122g of lignin to 20ml of distilled water and stir evenly to obtain a dispersion; then add the BiCl3 solution to the dispersion containing NaBr and lignin, first ultrasonicate for 30min, then stir vigorously for 30min to obtain a reaction solution; pour the reaction solution into a 100mL stainless steel hydrothermal autoclave lined with polytetrafluoroethylene, place it in an oven and heat it at 200℃ for 48h to perform a hydrothermal reaction; after the reaction is completed, the obtained product is separated, washed and dried in sequence to obtain the BiOBr / 10wt% Lignin photocatalyst.
[0039] 50 mg of BiOBr / 10 wt% Lignin catalyst was added to 250 mL of 30 mg / L Rhodamine B solution and irradiated with a 300 w Xe lamp (a 420 nm cutoff filter was installed at the outlet of the light source). After 1 hour, the degradation rate of Rhodamine B was 79.81%.
[0040] Example 7
[0041] The preparation method of lignin is the same as that of Example 6. 2mmol Bi2(SO4)3 is dissolved in 30mL anhydrous ethanol and stirred evenly by ultrasonication to obtain Bi2(SO4)3 solution; 4mmol NaBr and 0.0976g lignin are added to 20ml distilled water and stirred evenly to obtain a dispersion; then the Bi2(SO4)3 solution is added to the dispersion containing NaBr and lignin, first ultrasonicated for 30min, then vigorously stirred for 30min to obtain a reaction solution; the reaction solution is poured into a 100mL stainless steel hydrothermal autoclave lined with polytetrafluoroethylene, placed in an oven and heated at 140°C for 48h to perform a hydrothermal reaction; after the reaction is completed, the obtained product is separated, washed and dried in sequence to obtain BiOBr / 8wt%Lignin.
[0042] 50 mg of BiOBr / 8 wt% Lignin catalyst was added to 250 mL of 30 mg / L Rhodamine B solution and irradiated with a 300w Xe lamp (a 420 nm cutoff filter was installed at the outlet of the light source). After 1 hour, the degradation rate of Rhodamine B was 76.43%.
[0043] Example 8
[0044] The preparation method of lignin is the same as that of Example 1. 4mmol Bi(NO3)3·5H2O is dissolved in 30mL of anhydrous ethanol and stirred evenly by ultrasonication to obtain Bi(NO3)3·5H2O solution; 4mmol KBr and 0.122g of lignin are added to 20ml of nitric acid and stirred evenly to obtain a dispersion; then the Bi(NO3)3·5H2O solution is added to the dispersion containing KBr and lignin, ultrasonicated for 30min, and then vigorously stirred for 30min to obtain a reaction solution; the reaction solution is poured into a 100mL stainless steel hydrothermal autoclave lined with polytetrafluoroethylene, and placed in an oven and heated at 160°C for 12h to perform a hydrothermal reaction; after the reaction is completed, the obtained product is separated, washed, and dried in sequence to obtain BiOBr / 10wt%Lignin.
[0045] 50 mg of BiOBr / 10 wt% Lignin catalyst was added to 250 mL of 30 mg / L Rhodamine B solution and irradiated with a 300 w Xe lamp (a 420 nm cutoff filter was installed at the outlet of the light source). After 1 hour, the degradation rate of Rhodamine B was 72.36%.
[0046] Example 9
[0047] The preparation method of lignin is the same as that of Example 1. 4mmol Bi(CH3COO)3 is dissolved in 30mL anhydrous ethanol and stirred evenly by ultrasonication to obtain Bi(CH3COO)3 solution; 4mmol KBr and 0.1464g lignin are added to 20ml distilled water and stirred evenly to obtain a dispersion; then the Bi(CH3COO)3 solution is added to the dispersion containing KBr and lignin, ultrasonicated for 30min, and then stirred vigorously for 30min to obtain a reaction solution; the reaction solution is poured into a 100mL stainless steel hydrothermal autoclave lined with polytetrafluoroethylene, and placed in an oven and heated at 160°C for 48h to perform a hydrothermal reaction; after the reaction is completed, the obtained product is separated, washed, and dried in sequence to obtain BiOBr / 12wt%Lignin.
[0048] 50 mg of BiOBr / 12 wt% Lignin catalyst was added to 250 mL of eucalyptus chemical-mechanical pulp biochemical effluent with a COD of 273 mg / L, and irradiated with a 300 w Xe lamp (a 420 nm cutoff filter was installed at the outlet of the light source). After 1 hour, the COD removal rate was 52.65%.
[0049] Material characterization
[0050] In order to study the crystal phase and structure of the BiOBr prepared in the comparative example and the composite photocatalysts prepared in Examples 1 to 5, we performed XRD characterization on them. The results are as follows: Figure 1 shown. Figure 1 It shows that all samples show similar diffraction peaks in the X-ray diffraction patterns, indicating that all samples are high-purity crystals without impurity peaks. All diffraction peaks of the BiOBr samples synthesized by hydrothermal reaction match those of the tetragonal crystal JCPDF No.09-0393, and there are no impurity peaks. No obvious carbon structure diffraction peaks were observed between 20° and 30° of the composite photocatalyst, most likely because the main peak of biochar at 20° to 30° overlaps with the (101) peak of the tetragonal BiOBr at 25.16°. Figure 1 The diffraction peak intensities of all composite photocatalysts were significantly reduced compared with those of pure BiOBr, indicating that the addition of lignin may have led to lattice defects in BiOBr. The change in lattice constants also indicated that there was some interaction between BiOBr crystals and lignin structures after hydrothermal synthesis.
[0051] Figure 2Scanning electron microscope images of BiOBr (a), Biochar (b) and BiOBr / 2wt% Lignin (cd); it can be seen from the figure that BiOBr is a layered flaky structure with a size distribution between 500nm and 1μm. The product formed by the hydrothermal reaction of lignin is biochar (Biochar). It can be seen from the figure that Biochar is a block structure with a large enough surface area and many scaly structures on the surface, with a size of about 150μm. Figure 2 c and 2d are SEM images of BiOBr / 2wt%Lignin composite photocatalyst at different magnifications. It can be seen that in the BiOBr / 2wt%Lignin composite photocatalyst, BiOBr is evenly dispersed on Biochar. This allows BiOBr to expose more active sites, providing transmission channels for photogenerated electrons and increasing the contact opportunities between BiOBr and reactant molecules. At the same time, EDS energy spectrum analysis was performed on BiOBr / 2wt%Lignin, as shown in Figure 3 As shown, from Figure 3 It can be seen that the BiOBr / 2wt% Lignin catalyst contains Br, Bi, O and C elements, which further proves that BiOBr is successfully and evenly dispersed and grown on the surface of Biochar.
[0052] In order to analyze the elemental composition and valence state of each element in BiOBr and BiOBr / 2wt% Lignin, X-ray photoelectron spectroscopy was used to characterize them. Figure 4 XPS spectra of BiOBr, BiOBr / 2wt% Lignin and each element. Figure 4 b is the spectrum of Br 3d. It can be found that there are two strong spin-orbit splitting energy peaks at 68.46eV and 69.49eV, which are respectively related to the Br 3d 5 / 2 and Br 3d 3 / 2 The Bi 4f spectrum of 4c shows two independent symmetrical peaks at 159.46 and 164.78 eV, which belong to Bi 4f 7 / 2 and Bi 4f 5 / 2 The peak binding energies of Br 3d, Bi 4f and O1s of BL2 are 0.26-0.44 eV lower than those of BiOBr. This is because of the interaction of electrons, mainly due to the strong interaction between some unpaired π electrons of conjugated carbon atoms and free electrons on the BiOBr surface, resulting in charge transfer conversion. The O1s peak of BiOBr ( Figure 4d) There are two peaks at 530.21 and 531.61 eV, which are related to the lattice O atoms (Bi-O bonds) and the surface -OH, respectively. According to the shift of the peak positions of the O1s and Bi4f spectra, we can guess that a Bi-C bond is formed between the conjugated carbon and BiOBr. The binding energies of C1s of BL2 at 284.65, 286.11, and 288.13 eV match the CC, CO, and C=O bonds, respectively. Due to the low amount of lignin doping, the peak of C1s is very uneven.
[0053] In summary, the BiOBr / Lignin photocatalyst prepared by the method of the present invention can accelerate the separation of photogenerated electrons and holes, improve the absorption of visible light and the concentration of pollutants around the catalyst, enhance the photocatalytic reaction performance, and has stable properties and high recycling efficiency, and has a good effect on the treatment of industrial wastewater such as printing and dyeing and pulp and paper making.
[0054] Obviously, the described embodiments are only some embodiments of the present invention, but not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A bismuth oxybromide-lignin composite photocatalyst, characterized in that: The bismuth oxybromide-lignin composite photocatalyst comprises bismuth oxybromide and lignin, wherein the mass of the lignin is 1 wt% to 8 wt% of the mass of the bismuth oxybromide; The preparation method of the bismuth oxybromide-lignin composite photocatalyst comprises the following steps: dispersing a bromine salt and lignin in a dispersant to obtain a dispersion, dissolving a bismuth salt in an alcohol reagent to obtain a bismuth salt solution; adding the bismuth salt solution to the dispersion and mixing evenly to obtain a reaction liquid; pouring the reaction liquid into a hydrothermal kettle, and heating the hydrothermal kettle to allow the reaction liquid to undergo a hydrothermal reaction, and after the reaction is completed, cooling to room temperature, and separating, washing, and drying the obtained product in sequence to obtain a bismuth oxybromide-lignin composite photocatalyst; The lignin is alkali lignin; The dispersant is water, nitric acid or sulfuric acid; The alcohol reagent is anhydrous ethanol, ethylene glycol or isopropanol; The temperature of the hydrothermal reaction is 140-200° C. and the time is 24-48 hours.
2. The method for preparing the bismuth oxybromide-lignin composite photocatalyst according to claim 1, characterized in that: The method comprises the following steps: dispersing a bromine salt and lignin in a dispersant to obtain a dispersion, dissolving a bismuth salt in an alcohol reagent to obtain a bismuth salt solution; adding the bismuth salt solution to the dispersion and mixing them uniformly to obtain a reaction liquid; pouring the reaction liquid into a hydrothermal kettle, heating the hydrothermal kettle to allow the reaction liquid to undergo a hydrothermal reaction, cooling to room temperature after the reaction is completed, and sequentially separating, washing and drying the obtained product to obtain a bismuth oxybromide-lignin composite photocatalyst.
3. The method for preparing the bismuth oxybromide-lignin composite photocatalyst according to claim 2, characterized in that: The molar ratio of the bismuth salt to the bromine salt is 1:1 to 1:
2.
4. The method for preparing the bismuth oxybromide-lignin composite photocatalyst according to claim 2 or 3, characterized in that: The bismuth salt is any one of bismuth nitrate, bismuth sulfate, bismuth chloride or bismuth acetate; the bromide salt is any one of potassium bromide and sodium bromide.
5. Use of the bismuth oxybromide-lignin composite photocatalyst as claimed in claim 1 in treating wastewater under visible light.
6. The use according to claim 5, characterized in that: The wastewater is printing and dyeing wastewater or pulping and papermaking wastewater.
Citation Information