A method for overcoming the red iron scale on the surface of hot-rolled steel strip
By optimizing the hot rolling process and descaling process, the problem of poor adaptability and poor effect of the red iron sheet defects on the steel strip surface is solved, and effective improvement of silicon-containing steel products is achieved, reducing costs and improving hot rolling efficiency.
Patent Information
- Application Number
- CN202210167419.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-02-23
AI Technical Summary
The methods for overcoming the defects of red iron sheets on the steel strip surface in the prior art are not adaptable, have little guidance on actual operation, and have no significant effect.
By optimizing the hot rolling process, the product design contains mass fractions of C, Si and P. The slab is heated to 1190-1260℃, and is quickly cooled after rough rolling and finishing rolling. High-pressure water is used to descalate the residual oxygen and SO2 content of the heating furnace is controlled. , optimize the descaling process to completely remove the Fe2SiO4 layer and avoid the production of red iron sheets.
It significantly improves the defects of red iron sheets on the steel strip surface, and is suitable for all kinds of silicon-containing steel products. It makes full use of cheap Si elements, reduces costs, shortens the furnace time, improves the efficiency of hot rolling, and reduces the correction rate of red iron sheets by 90%.
Smart Images

Figure CN114749484B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hot-rolled steel strip preparation, and in particular to a method for overcoming red iron scale on the surface of a hot-rolled steel strip directly heated. Background Art
[0002] Hot-rolled products are prone to produce flakes, strips, or even a layer of red rust on the surface of the finished steel coil due to mismatched composition design and process control, or unreasonable hot rolling process control. The surface of the finished steel coil is covered with a layer of red rust, which is attached to the surface of the steel plate and appears dark red. It is one of the "common diseases" on the hot-rolled strip steel production line. After pickling, this type of product has obvious color difference on the surface, commonly known as "tiger skin pattern". Such products are scrapped due to poor surface quality during subsequent electroplating and electrophoresis. This defect seriously reduces the pickling efficiency of steel products and is prone to "under-pickling" or "over-pickling" defects in the pickling line. This defect is common in silicon-containing products, and Si is a cheap strengthening element. Some products have to adopt a silicon-free design due to the red iron sheet defect, which results in an increase in alloy elements such as metal Mn, increasing the product design cost. In addition, with the promotion and application of hot charging and hot delivery technology, the slabs are charged into the furnace and heated using a direct hot charging process. The charging temperature of the slabs is not lower than 400°C. The surface state of the slabs has changed greatly compared with conventional cold charging. The iron oxide layer is dense, and the oxidation inside the surface of the slab is more serious than when the cold slab is heated, which makes it more likely to produce more serious red iron scale defects.
[0003] In the prior art, there are generally two methods to overcome the red iron scale defect. One is to reduce the Si in the steel to at least below 0.12%, preferably below 0.10%; the other is to increase the heating temperature of the slab and descale above the melting point of Fe2SiQ4 to improve the efficiency of removing the oxide scale. However, the above methods are not highly adaptable to the product, are not very instructive for actual operation, and are not very effective in solving the surface red iron scale defect. Summary of the invention
[0004] The problem solved by the present invention is that the method for overcoming the red iron scale defect on the surface of steel strip in the prior art has poor adaptability to products, poor guidance for actual operation, and at least one aspect in that the effect of solving the red iron scale defect on the surface is not significant.
[0005] In order to solve the above problems, the present invention provides a method for overcoming the red iron scale on the surface of hot-rolled steel strip by direct hot charging, comprising the following steps:
[0006] Step S1, product design, the product at least includes the following components by mass fraction: 0.06%-0.50% C, 0.1%-1.35% Si and 0.01%-0.025% P
[0007] Step S2, heating the slab, heating the hot-charged and hot-delivered slab in a heating furnace to a steel-out temperature of 1190-1260° C. and then taking it out of the furnace, and the hot-charged and hot-delivered slab has a furnace time range of 100-155 minutes;
[0008] Step S3, rough rolling and finish rolling, rough rolling the hot-charged and hot-delivered slab into an intermediate strip, and then entering the finishing mill for finish rolling to obtain a strip steel pre-product, wherein the temperature range of the intermediate strip includes 950-1080° C., and the final rolling temperature range after the finish rolling includes 860-950° C.;
[0009] Step S4, cooling after rolling, the strip pre-product directly enters the cooling mode of water cooling, air cooling, water cooling, and air cooling after leaving the finishing mill, and is coiled to obtain a direct hot-rolled hot-rolled steel strip.
[0010] Optionally, in step S2, the residual oxygen content in the soaking section of the heating furnace ranges from 0.5 to 3%.
[0011] Optionally, in step S2, the content of SO2 in the mixed gas in the heating furnace is not more than 200 mg / m 3 .
[0012] Optionally, in step S2, the steel tapping temperature is the temperature of the upper surface of the hot-charged and hot-delivered slab, and the temperature of the lower surface of the hot-charged and hot-delivered slab is 20-25°C lower than the temperature of the upper surface of the hot-charged and hot-delivered slab.
[0013] Optionally, in step S3, the rough rolling of the hot-charged and hot-delivered slab into an intermediate strip comprises: rough rolling the hot-charged and hot-delivered slab for 6 passes, during which the frame of the rough rolling mill is descaled at least 3 times, and the frame is descaled once before the last rough rolling pass.
[0014] Optionally, during the rack dephosphorization process, the pressure range of the descaling water includes 18-23 MPa.
[0015] Optionally, in step S3, during the finish rolling process, the pressure range of the descaling water in the descaling box includes 20-23 MPa, and the speed of the intermediate strip passing through the descaling point is not greater than 1.0 m / s.
[0016] Optionally, in step S3, during the finishing rolling process, inter-stand cooling water is used in the finishing rolling mill group, and the water volume range includes 0-1000L / min.
[0017] Optionally, in step S4, the average cooling rate before coiling is not less than 10°C / s.
[0018] Optionally, in step S4, the coiling temperature range includes 475-700°C.
[0019] The method for overcoming the red scale on the surface of the hot-rolled steel strip in direct hot-charging according to the present invention has the advantage over the prior art that, in the present invention, the method for overcoming the red scale on the surface of the hot-rolled steel strip in direct hot-charging improves the red scale defect on the surface of the steel strip by optimizing the hot rolling process, is applicable to various silicon-containing steel products, and can effectively overcome the red scale defect caused by the hot charging and hot delivery process, and the effect is significant. At the same time, the process method can fully use the cheap Si element for strengthening, reduce costs, shorten the furnace time, and improve the hot rolling efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a flow chart of a method for overcoming the red iron scale on the surface of a hot-rolled steel strip in direct heating according to an embodiment of the present invention;
[0021] Figure 2 This is a diagram showing the effect of applying the method for overcoming the red iron scale on the surface of hot-rolled steel strip in direct heating according to the embodiment of the present invention to improve the red iron scale defect of medium silicon structural steel products;
[0022] Figure 3 Comparison of the effect of using the method of overcoming the red iron scale on the surface of hot-rolled steel strip in the embodiment of the present invention and the conventional technology on improving the red iron scale defect of medium silicon structural steel products Figure 1 ;
[0023] Figure 4 Comparison of the effect of using the method of overcoming the red iron scale on the surface of hot-rolled steel strip in the embodiment of the present invention and the conventional technology on improving the red iron scale defect of medium silicon structural steel products Figure 2 ;
[0024] Figure 5 Comparison of the effect of using the method of overcoming the red iron scale on the surface of hot-rolled steel strip in the embodiment of the present invention and the conventional technology on improving the red iron scale defect of medium silicon structural steel products Figure 3 ;
[0025] Figure 6 Comparison of the effect of using the method of overcoming the red iron scale on the surface of hot-rolled steel strip in the embodiment of the present invention and the conventional technology on improving the red iron scale defect of medium silicon structural steel products Figure 4 ;
[0026] Figure 7 Comparison of the effect of using the method of overcoming the red iron scale on the surface of hot-rolled steel strip in the embodiment of the present invention and the conventional technology on improving the red iron scale defect of medium silicon structural steel products Figure 5 . DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present application will be described clearly and in detail below with reference to the accompanying drawings.
[0028] The term "some embodiments" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same implementation or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0029] like Figure 1 As shown, the embodiment of the present invention provides a method for overcoming the red iron scale on the surface of a hot-rolled steel strip, comprising the following steps:
[0030] Step S1, product design, the product at least includes the following components by mass fraction: 0.06%-0.50% C, 0.1%-1.35% Si and 0.01%-0.025% P;
[0031] Step S2, heating the slab, heating the hot-charged and hot-delivered slab in a heating furnace to a steel-out temperature of 1190-1260° C. and then taking it out of the furnace, and the hot-charged and hot-delivered slab has a furnace time range of 100-155 minutes;
[0032] Step S3, rough rolling and finish rolling, rough rolling the hot-charged and hot-delivered slab into an intermediate strip, and then entering the finishing mill for finish rolling to obtain a strip steel pre-product, wherein the temperature range of the intermediate strip includes 950-1080° C., and the final rolling temperature range after the finish rolling includes 860-950° C.;
[0033] Step S4, cooling after rolling, the strip pre-product directly enters the cooling mode of water cooling, air cooling, water cooling, and air cooling after leaving the finishing mill, and is coiled to obtain a direct hot-rolled hot-rolled steel strip.
[0034] In this embodiment, when designing the product composition, the Si design range is relatively wide, which can reach 1.35%, so as to give full play to the strengthening effect of Si in steel, avoid deliberately reducing the Si content below 0.12% to overcome the red iron scale defect on the strip surface, and increase the use of other more precious metals, thereby reducing the design cost of the product.
[0035] In some embodiments, the product further includes 0.45%-1% Cr and / or 0.34%-1% Mo to meet the special requirements of the steel strip product.
[0036] It should be noted that, in the heating process of the hot-charged and hot-delivered slab in this embodiment, the Si element therein will be enriched on the surface to form a dense Fe2SiO4 layer, and the oxidation reaction rate of the matrix inside the Fe2SiO4 layer will be greatly reduced, thereby preventing the matrix from further oxidation. However, the Fe2SiO4 layer has a strong pinning effect, which can easily cause FeO residue and generate red iron scale. In order to overcome the red iron scale defect, the Fe2SiO4 layer needs to be completely removed. If the Fe2SiO4 layer is not completely removed, a thicker red iron scale defect will be formed on the surface of the strip; and when Fe2SiO4 is in liquid state, the pinning effect is weak, and the use of high-pressure water for descaling can more thoroughly remove the Fe2SiO4 layer, so that the inner oxide layer is completely exposed, and it is removed in the subsequent process, thereby avoiding the generation of secondary surface red iron scale defects. The temperature of hot-charged and hot-delivered slabs is higher than 400℃. There is no process in which the iron oxide scale on the surface of the cold-charged slab is broken and oxidized relatively fully during the cooling process. The iron oxide scale on the surface of the slab is relatively dense, and the degree of oxidation inside the slab is more serious than that of the cold-charged slab. The iron oxide scale on the slab is not easy to remove after heating.
[0037] For this reason, the surface temperature of the hot-charged and hot-delivered slab during descaling in this embodiment is not less than 1175°C. Combined with the rough rolling buckle control, the temperature of the lower surface of the hot-charged and hot-delivered slab is 20-25°C lower than the temperature of the upper surface of the hot-charged and hot-delivered slab. Considering the heat transfer and heat loss inside the slab, the preferred steel-out temperature range of the upper surface of the hot-charged and hot-delivered slab is 1190-1260°C, and the steel-out temperature of the specific steel grade is determined according to the distance from the heating furnace to the descaling box, the temperature drop model and the special characteristics of the steel grade.
[0038] In addition, under the condition of ensuring the uniformity of the slab heating temperature, the shorter the time the hot-charged and hot-delivered slabs are in the furnace, the better. Therefore, in this embodiment, the time the hot-charged and hot-delivered slabs are in the furnace ranges from 100 to 155 minutes, and the specific time in the furnace can be adjusted accordingly according to the content of each component in the hot-charged and hot-delivered slabs.
[0039] In some embodiments, in step S2, the residual oxygen content in the soaking section of the heating furnace is in the range of 0.5-3%, thereby making the atmosphere in the heating furnace weakly reducing and reducing the high temperature oxidation of the hot-charged and hot-delivered slabs.
[0040] In some embodiments, in step S2, the content of SO2 in the mixed gas in the heating furnace is not more than 200 mg / m 3 It can effectively prevent FeS from gathering on the surface of hot-charged and hot-delivered slabs to form a dense iron oxide layer, which increases the difficulty of descaling.
[0041] In some embodiments, in step S3, the rough rolling of the hot-charged and hot-delivered slab into an intermediate strip comprises: rough rolling the hot-charged and hot-delivered slab for 6 passes, during which the frame of the rough rolling mill is descaled at least 3 times, and the frame is descaled once before the last rough rolling pass to remove the pinning effect of fayalite and the influence of the relatively dense oxide layer formed by the direct hot-charged slab.
[0042] In some embodiments, during the descaling process of the frame and the rough rolling descaling box, the pressure range of the descaling water includes 18-23 MPa to ensure the impact force of the descaling water, so that the descaling effect is better.
[0043] Optionally, in step S3, the finishing rolling is performed for 7 passes, and during the finishing rolling process, the upper surface of the descaling box is affected by the change in descaling distance as the thickness of the strip varies, which affects the impact force of the descaling water. Therefore, the pressure range of the descaling water in the descaling box includes 20-23MPa, and the speed of the intermediate strip passing through the descaling point is not more than 1.0m / s.
[0044] In addition, in step S3, during the finishing rolling process, inter-stand cooling water is used in the finishing rolling mill group, and the water volume range includes 0-1000L / min to control the temperature of the intermediate strip, while ensuring a high rolling speed and shortening the high temperature section time of the strip.
[0045] It should also be noted that 860°C is the upper limit temperature for the high-temperature generation of Fe2O3. Rolling above this temperature can inhibit the generation of Fe2O3 in the finishing rolling stage, while below this temperature, it is easy to generate surface rust-like 3rd red iron scale defects. Therefore, in this embodiment, the final rolling temperature range after finishing rolling includes 860-950°C. The high final rolling temperature can properly ensure the plasticity of the oxide scale and prevent the surface oxide scale layer from breaking and cracking during the rolling process.
[0046] Optionally, in step S4, the average cooling rate before coiling is not less than 10°C / s, which can quickly reduce the surface temperature of the steel strip, shorten the steel strip and help reduce the thickness of the iron oxide layer.
[0047] Optionally, in step S4, the coiling temperature range includes 475-700° C., so that the rolling effect is better.
[0048] Therefore, in this embodiment, high final rolling temperature, rapid rolling and rapid cooling can effectively avoid the occurrence of secondary and tertiary red iron scale defects.
[0049] Therefore, in this embodiment, the method for overcoming the red scale on the surface of the hot-rolled steel strip can fully use the cheap Si element for strengthening, reduce costs, shorten the furnace time, and improve the hot rolling efficiency. At the same time, by optimizing the hot rolling process to improve the red scale defect on the surface of the steel strip, it is applicable to various silicon-containing steel products and can effectively overcome the red scale defect caused by the hot charging and hot delivery process, and the effect is significant. Figure 2 As shown, taking the medium silicon structural steel product as an example, before the method in this embodiment was used to overcome the red iron scale on the surface of the hot-rolled steel strip with direct heating, the production line had a total of more than 2,000 tons of red iron scale downgraded and re-judged throughout the year. After the method in this embodiment was used to overcome the red iron scale on the surface of the hot-rolled steel strip with direct heating, the total re-judgment was only 50 tons. The user feedback was good, there were no new problems with the product, the overall performance consistency was good, and no user quality objections occurred. In addition, the method in this embodiment to overcome the red iron scale on the surface of the hot-rolled steel strip with direct heating has been widely used in a variety of products such as carbon structural steel, low alloy structural steel, automotive steel, medium and high carbon alloy steel, and has shown good control effects in products of various composition systems. The red iron scale defect re-judgment rate of the production line has been declining year by year, with a cumulative decline of up to 90%.
[0050] Example 1
[0051] This embodiment provides a method for overcoming the red iron scale on the surface of a hot-rolled steel strip, comprising the following steps:
[0052] Step 1, product Q235B, the product includes the following components by mass fraction: 0.16% C, 0.2% Si and 0.018% P;
[0053] Step 2, heating the slab, heating the hot-charged and hot-delivered slab with an initial temperature of 590° C. in a heating furnace to a tapping temperature of 1210° C. and then taking it out of the furnace, and the hot-charged and hot-delivered slab is kept in the furnace for 116 minutes;
[0054] Step 3, rough rolling and finish rolling, rough rolling the hot-charged and hot-delivered slab into an intermediate strip, and then entering the finishing mill for finish rolling to obtain a strip pre-product, wherein the temperature range of the intermediate strip includes 950-1080° C., the final rolling temperature after the finish rolling is 870-895° C., the descaling pressure of the rough rolling and finishing rolling stands is 18-23 MPa, and the descaling speed of the finish rolling is 0.85 m / s;
[0055] Step 4, cooling after rolling. After the strip pre-product leaves the finishing mill, it directly enters a cooling mode of water cooling, air cooling, water cooling, and air cooling. The average cooling rate is 20.6°C / s, and after coiling, a direct hot-rolled hot-rolled steel strip is obtained.
[0056] like Figure 3As shown, the left side is a picture taken by a surface detector of a hot-rolled steel strip prepared by direct heating loading using the method for overcoming the red iron scale on the surface of the hot-rolled steel strip prepared by direct heating loading using the present embodiment, and the right side is a picture taken by a surface detector of a hot-rolled steel strip prepared by direct heating loading using the conventional technology. It can be seen from the figure that the method for overcoming the red iron scale on the surface of the hot-rolled steel strip prepared by direct heating loading using the present embodiment is more effective in improving the red iron scale defects of medium-silicon structural steel products than the conventional technology.
[0057] Example 2
[0058] This embodiment provides a method for overcoming the red iron scale on the surface of a hot-rolled steel strip in direct heating. The difference from the embodiment 1 is as follows:
[0059] Product Q355B, composition: 0.16% C, 0.25% Si and 0.018% P;
[0060] Relevant process parameters: slab initial temperature 620℃, furnace time 138min, tapping temperature 1220℃, descaling pressure of roughing and finishing mills 18-23MPa, descaling speed 0.8m / s, final rolling temperature 865-889℃, coiling temperature 590℃, average cooling rate 19.5℃ / s.
[0061] like Figure 4 As shown, the left side is a picture taken by a surface detector of a hot-rolled steel strip prepared by direct heating using the method for overcoming the red iron scale on the surface of the hot-rolled steel strip in direct heating using the present embodiment, and the right side is a picture taken by a surface detector of a hot-rolled steel strip prepared by direct heating using the conventional technology. It can be seen from the figure that the method for overcoming the red iron scale on the surface of the hot-rolled steel strip in direct heating using the present embodiment is more effective in improving the red iron scale defects of medium-silicon structural steel products than the conventional technology.
[0062] Example 3
[0063] This embodiment provides a method for overcoming the red iron scale on the surface of a hot-rolled steel strip in direct heating. The difference from the embodiment 1 is as follows:
[0064] Product 510L, composition: 0.08% C, 0.2% Si and 0.01% P;
[0065] Relevant process parameters: slab initial temperature 520℃, furnace time 130min, tapping temperature 1220℃, descaling pressure 18-23MPa, descaling speed 0.85m / s, final rolling temperature 860-885℃, coiling temperature 610℃, average cooling rate 18.6℃ / s.
[0066] like Figure 5As shown, the left side is a picture taken by a surface detector of a hot-rolled steel strip prepared by direct heating using the method for overcoming the red iron scale on the surface of the hot-rolled steel strip in direct heating using the present embodiment, and the right side is a picture taken by a surface detector of a hot-rolled steel strip prepared by direct heating using the conventional technology. It can be seen from the figure that the method for overcoming the red iron scale on the surface of the hot-rolled steel strip in direct heating using the present embodiment is more effective in improving the red iron scale defects of medium-silicon structural steel products than the conventional technology.
[0067] Example 4
[0068] This embodiment provides a method for overcoming the red iron scale on the surface of a hot-rolled steel strip in direct heating. The difference from the embodiment 1 is as follows:
[0069] Product 40Cr, composition: 0.4% C, 0.25% Si, 0.015% P and 1% Cr;
[0070] Relevant process parameters: slab initial temperature 680℃, furnace time 130min, tapping temperature 1220℃, descaling pressure 18-23MPa, descaling speed 0.85m / s, final rolling temperature 900℃, coiling temperature 630℃, cooling rate 21.5℃ / s.
[0071] like Figure 6 As shown, the left side is a picture taken by a surface detector of a hot-rolled steel strip prepared by direct heating using the method for overcoming the red iron scale on the surface of the hot-rolled steel strip in direct heating using the present embodiment, and the right side is a picture taken by a surface detector of a hot-rolled steel strip prepared by direct heating using the conventional technology. It can be seen from the figure that the method for overcoming the red iron scale on the surface of the hot-rolled steel strip in direct heating using the present embodiment is more effective in improving the red iron scale defects of medium-silicon structural steel products than the conventional technology.
[0072] Example 5
[0073] This embodiment provides a method for overcoming the red iron scale on the surface of a hot-rolled steel strip in direct heating. The difference from the embodiment 1 is as follows:
[0074] Product DP600, composition: 0.06% C, 1.25% Si, 0.01% P, 0.45% Cr and 0.34% Mo;
[0075] Relevant process parameters: slab initial temperature 620℃, furnace time 155min, tapping temperature 1230℃, descaling pressure 18-23MPa, descaling speed ≤0.80m / s, final rolling temperature 860-895℃, coiling temperature 580℃, cooling rate 19.6℃ / s.
[0076] like Figure 7As shown, the left side is a picture taken by a surface detector of a hot-rolled steel strip prepared by direct heating using the method for overcoming the red iron scale on the surface of the hot-rolled steel strip in direct heating using the present embodiment, and the right side is a picture taken by a surface detector of a hot-rolled steel strip prepared by direct heating using the conventional technology. It can be seen from the figure that the method for overcoming the red iron scale on the surface of the hot-rolled steel strip in direct heating using the present embodiment is more effective in improving the red iron scale defects of medium-silicon structural steel products than the conventional technology.
[0077] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A method for overcoming the red iron scale on the surface of hot-rolled steel strip, characterized in that: The steps include: Step S1, product design, the product at least includes the following components by mass fraction: 0.06%-0.50% C, 0.2%-1.35% Si and 0.01%-0.025% P; Step S2, heating the slab, heating the hot-charged and hot-delivered slab in a heating furnace to a steel-out temperature of 1190-1260° C. and then taking it out of the furnace, wherein the steel-out temperature is the temperature of the upper surface of the hot-charged and hot-delivered slab, the temperature of the lower surface of the hot-charged and hot-delivered slab is 20-25° C. lower than the temperature of the upper surface of the hot-charged and hot-delivered slab, and the time the hot-charged and hot-delivered slab is in the furnace ranges from 100 to 155 minutes; Step S3, rough rolling and finish rolling, rough rolling the hot-charged and hot-delivered slab into an intermediate strip, and then entering the finishing mill for finish rolling to obtain a strip steel pre-product, wherein the temperature range of the intermediate strip includes 950-1080° C., the final rolling temperature range after the finish rolling includes 860-950° C., and the surface temperature of the hot-charged and hot-delivered slab during descaling is not less than 1175° C.; Step S4, cooling after rolling, the strip pre-product directly enters the cooling mode of water cooling, air cooling, water cooling, and air cooling after leaving the finishing mill, and is coiled to obtain a direct hot-rolled hot-rolled steel strip.
2. The method for overcoming the red iron scale on the surface of hot-rolled steel strip according to claim 1, characterized in that: In step S2, the residual oxygen content in the soaking section of the heating furnace ranges from 0.5 to 3%.
3. The method for overcoming the red iron scale on the surface of hot-rolled steel strip according to claim 1, characterized in that: In step S2, the content of SO2 in the mixed gas in the heating furnace is not more than 200 mg / m 3 .
4. The method for overcoming the red iron scale on the surface of hot-rolled steel strip according to claim 1, characterized in that: In step S3, the rough rolling of the hot-charged and hot-delivered slab into an intermediate strip comprises: rough rolling the hot-charged and hot-delivered slab for 6 passes, during which the frame of the rough rolling mill is descaled for no less than 3 times, and the frame is descaled once before the last rough rolling pass.
5. The method for overcoming the red iron scale on the surface of the hot-rolled steel strip according to claim 4 is characterized in that: During the rack descaling process, the pressure range of the descaling water includes 18-23 MPa.
6. The method for overcoming the red iron scale on the surface of hot-rolled steel strip according to claim 1, characterized in that: In step S3, during the finish rolling process, the pressure of the descaling water in the descaling box is in the range of 20-23 MPa, and the speed of the intermediate strip passing through the descaling point is not greater than 1.0 m / s.
7. The method for overcoming the red iron scale on the surface of hot-rolled steel strip according to claim 1, characterized in that: In step S3, during the finishing rolling process, inter-stand cooling water is used in the finishing rolling mill group, and the water volume range includes 0-1000L / min.
8. The method for overcoming the red iron scale on the surface of hot-rolled steel strip according to claim 1, characterized in that: In step S4, the average cooling rate before coiling is not less than 10°C / s.
9. The method for overcoming the red iron scale on the surface of hot-rolled steel strip according to claim 1, characterized in that: In step S4, the coiling temperature range includes 475-700°C.