Production method for accurately controlling nitrogen content of vanadium-containing steel grade
Through an automated nitrogen source addition system and an intelligent production control system, precise control of the nitrogen content of vanadium-containing steel is achieved, the problem of nitrogen content fluctuations is solved, product quality and production efficiency are improved, and cost is reduced.
Patent Information
- Application Number
- CN202410969145.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art cannot accurately control the addition of nitrogen sources in vanadium-containing steel, resulting in large fluctuations in nitrogen content, affecting product quality, and increasing subsequent processing and inspection costs.
An automated nitrogen source addition system and an intelligent production control system are adopted, combined with real-time nitrogen content monitoring and feedback control, the nitrogen source addition amount and smelting parameters are accurately adjusted to ensure uniform dissolution and diffusion of nitrogen elements and achieve accurate control of nitrogen content.
It improves product quality stability, reduces defective rate and production costs, optimizes production processes, reduces energy and raw materials waste, and enhances corporate competitiveness.
Smart Images

Figure CN119040725A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steelmaking, and in particular to a production method for accurately controlling the nitrogen content of vanadium-containing steel. Background Art
[0002] Vanadium has a high melting point, the same as niobium and tantalum in the same subgroup in metal elements. It is a refractory metal with a high melting point. The content of this element in the earth's crust is 0.02%. It is solid at room temperature. The appearance of dense vanadium metal blocks is silver-gray. Vanadium belongs to the fifth subgroup of the periodic table with an atomic number of 23 and a body-centered cubic lattice structure. The nitrogen content in vanadium-containing steel is usually low, usually below 30ppm. Vanadium-containing steel is a special alloy steel in which vanadium is added to improve its strength, wear resistance and corrosion resistance. The nitrogen content is usually low because nitrogen can easily cause brittleness of steel and affect the processing performance of steel. Therefore, when producing vanadium-containing steel, the nitrogen content is usually controlled at a low level.
[0003] After searching, the existing Chinese patent publication number is CN114686750A, which provides a production method for accurately controlling the nitrogen content of vanadium-containing steel, including converter, refining, and continuous casting processes; in the converter process, different deoxidizer addition standards are formulated according to the different carbon content of the converter steel; in the refining process, the type and amount of refining slag added are fixed, and different top slag addition methods are adopted according to whether the produced steel is equipped with silicon manganese balls, and the top slag addition amount is appropriately fine-tuned according to the actual situation on site; the bottom blowing control of the refining process adopts a nitrogen-argon switching method, and the nitrogen-argon switching time is set to 4-12 minutes according to different nitrogen content control targets in the steel.
[0004] In the above patent, the addition of nitrogen source cannot be precisely controlled, resulting in large fluctuations in the nitrogen content in the product during the nitrogen source addition process, making the product quality unstable and difficult to meet customer needs and standard requirements. The unstable nitrogen content will cause product quality problems, increase subsequent processing and inspection costs, and require rework or waste disposal, increasing production costs.
[0005] Therefore, those skilled in the art provide a production method for accurately controlling the nitrogen content of vanadium-containing steel to solve the problems raised in the above background technology. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides a production method for accurately controlling the nitrogen content of vanadium-containing steels, so as to solve the problem that the addition of nitrogen source cannot be accurately controlled, resulting in large fluctuations in the nitrogen content in the product during the nitrogen source addition process, making the product quality unstable and difficult to meet customer needs and standard requirements. In addition, the instability of nitrogen content can cause product quality problems and increase the cost of subsequent processing and inspection.
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions: A production method for accurately controlling the nitrogen content of vanadium-containing steel, comprising the following steps:
[0008] Step 1: Preparation of raw materials: prepare raw materials containing vanadium steel and nitrogen source;
[0009] Step 2: Smelting: placing the vanadium-containing steel into a smelting furnace for smelting;
[0010] Step 3: Automated nitrogen source addition system: accurately control the amount and rate of nitrogen source addition based on real-time nitrogen content monitoring data;
[0011] Step 4: Intelligent production control system: Equipped with an intelligent production control system to monitor and adjust the temperature, pressure and atmosphere parameters during the smelting process in real time;
[0012] Step 5: stirring and mixing: During the smelting process, the smelting furnace is stirred by means of a stirrer to make the nitrogen source evenly dissolved in the molten steel;
[0013] Step 6: Real-time monitoring and feedback control: Online nitrogen content monitoring equipment monitors the nitrogen content in the molten steel in real time and automatically adjusts the smelting parameters in combination with the feedback control system;
[0014] Step 7. Reaction time: Control the reaction time according to the nitrogen content and steel characteristics to ensure that the nitrogen element is fully dissolved and diffused into the steel;
[0015] Step 8: Sampling and analysis: Take samples regularly to analyze and test the nitrogen content in the molten steel;
[0016] Step 9: Cooling and solidification: After the nitrogen content reaches the target, control the cooling rate to make the steel solidify evenly;
[0017] Step 10. Environmental protection measures: Take energy-saving and emission-reduction measures to reduce environmental pollution during the production process.
[0018] The selection and proportion of raw materials have an important impact on the nitrogen content of the final product. Through the smelting process, the vanadium-containing components in the steel are dissolved, providing a uniform reaction medium for the subsequent addition of nitrogen sources. Through the automated nitrogen source addition system, the addition of nitrogen sources can be accurately controlled according to real-time monitoring data to achieve the goal of accurately controlling the nitrogen content of vanadium-containing steels. The intelligent production control system can monitor and adjust various parameters in the smelting process in real time to ensure the stability and controllability of the smelting process. Stirring and mixing can promote the full contact and reaction between the nitrogen source and the molten steel, ensuring that the nitrogen element can be evenly dissolved and diffused into the steel. Real-time monitoring and feedback control can timely detect and correct the deviation of nitrogen content from the target value, ensuring the accuracy and stability of the production process. Reasonable control of reaction time can ensure the full reaction of nitrogen source and molten steel, so that the nitrogen content in the steel reaches the expected target. Sampling analysis can monitor and verify the nitrogen content in the production process, and timely discover and solve potential problems. By controlling the cooling rate, the uniformity and stability of the internal structure of the steel can be ensured, ensuring the quality of the final product. In the production process, environmental protection measures can reduce energy consumption and waste gas emissions, reduce the impact on the environment, and achieve sustainable development.
[0019] Preferably, in the step 2, the internal temperature range of the smelting furnace during the smelting process is 1600° C.-1750° C., and the smelting treatment time range is 0.5 h-4 h.
[0020] Preferably, in step 3, the operation steps of the automated nitrogen source addition system are as follows:
[0021] a. Install nitrogen source adding equipment, including nitrogen supply system, valves, flow meter, used to add nitrogen source into the smelting furnace;
[0022] b. Design control system, including sensors, actuators, and controller components, to monitor nitrogen content and control nitrogen source addition;
[0023] c. Develop a feedback algorithm to adjust the amount of nitrogen source added based on real-time monitoring data and the set target range;
[0024] d. Install an online nitrogen content monitoring system to monitor the nitrogen content in the molten steel in real time and feed the monitoring data back to the control system;
[0025] e. Connect the control system to the nitrogen source adding equipment. The system automatically adjusts the amount of nitrogen source added based on monitoring data and feedback algorithms.
[0026] Correct installation and debugging of the equipment can ensure the accuracy and stability of nitrogen source addition; the design of the control system should take into account the sensitivity and accuracy of the sensor, as well as the response speed and precision of the actuator, to achieve precise control of the nitrogen source addition process; the feedback algorithm can automatically adjust the amount of nitrogen source added according to the deviation between the actual monitored nitrogen content and the target range, so that it gradually approaches the set target value to achieve precise control; through real-time monitoring, the changes in nitrogen content can be obtained in time to provide accurate data support for the control system so that the amount of nitrogen source added can be adjusted in time; through automatic adjustment, precise control of the nitrogen source addition process can be achieved to ensure that the nitrogen content in the molten steel can stably reach the set target range, and achieve precise control of the nitrogen content of vanadium-containing steel production requirements.
[0027] Preferably, in step 3, the formula of the feedback algorithm is:
[0028]
[0029] Among them, K p is the proportional gain, K i is the integration time constant, K d is the differential time constant, e(t) is the error signal, that is, the difference between the set value and the actual value, represents the integral term of the error, Represents the differential term of the error.
[0030] Preferably, in step 4, the operation steps of the intelligent production control system are as follows:
[0031] a. Sensor deployment: deploy temperature sensors, pressure sensors, and humidity sensors;
[0032] b. Data acquisition: Design a data acquisition system to collect data transmitted by sensors;
[0033] c. Data processing: process and analyze the collected data;
[0034] d. Application of artificial intelligence algorithms: Use artificial intelligence algorithms to analyze and model data;
[0035] e. Control system design: Design intelligent control systems and apply artificial intelligence algorithms to control systems;
[0036] f. System integration: Integrate sensors, data acquisition systems, artificial intelligence algorithms and control systems to establish a complete intelligent production control system;
[0037] g. Real-time monitoring and adjustment: Adjust and optimize production parameters based on monitoring data.
[0038] The deployment location and number of sensors should be reasonably selected to ensure accurate monitoring of key parameters; the data acquisition system can collect and store the data obtained by the sensors in real time, providing a data basis for subsequent data processing and analysis; through data processing technology, the collected data can be cleaned, sorted, and denoised for subsequent data analysis and modeling; through artificial intelligence algorithms, hidden rules and trends can be discovered in the data, and the smelting process can be modeled and predicted to provide accurate reference and decision-making basis for the control system; the intelligent control system can automatically adjust the temperature, pressure, and atmosphere parameters in the smelting process according to the analysis results of the artificial intelligence algorithm to achieve precise control of the production process; system integration can realize data interaction and collaborative work between components to ensure the stable operation and efficient operation of the intelligent production control system; through real-time monitoring, the changes in various parameters in the smelting process can be obtained in time, and the production parameters can be adjusted and optimized according to the monitoring data to achieve precise control and optimization of the smelting process.
[0039] Preferably, in step four, the processing and analysis of the collected data in the intelligent production control system includes data cleaning, feature extraction, and data modeling; data cleaning refers to processing the original data and removing erroneous data; feature extraction refers to extracting features from the original data that are valuable for problem modeling, usually involving data conversion, dimensionality reduction, or selection of specific features; data modeling is the use of machine learning and deep learning algorithms to model and train the cleaned and feature-extracted data.
[0040] In intelligent production control systems, data cleaning can improve the quality and accuracy of data, reduce the impact of noise and interference on data analysis and modeling, and ensure the reliability of subsequent data processing and analysis. By converting, reducing the dimension of raw data, or selecting specific features, the dimension of the data can be reduced, and more representative and distinctive features can be extracted to provide better input data for subsequent data modeling and training, thereby improving the prediction accuracy and stability of the model. Data modeling can help intelligent production control systems achieve automated decision-making and precise control, and improve production efficiency and product quality.
[0041] Preferably, in step 4, the artificial intelligence algorithm includes a linear regression model formula, a logistic regression model formula, and a SVM classifier formula;
[0042] Linear regression model formula: [y=w0+w1x1+w2x2+...+w n x n ],
[0043] Where y is the input variable, (x1, x2, ..., x n ) are input variables, (w0, w1, w2, ..., w n) are model parameters;
[0044] Logistic regression model formula:
[0045] Where P(y=1|x) is the probability of the output being class 1, (x1, x2, ..., x n ) are input variables, (w0, w1, w2, ..., w n ) are model parameters;
[0046] SVM classifier formula: [f(x) = sign(w T ·x+b)],
[0047] Where f(x) is the output of the classifier, x is the input feature vector, w is the weight vector, and b is the bias term.
[0048] The linear regression model is used to establish the linear relationship between input variables and continuous output variables. The linear regression model can be used to predict and optimize continuous variables in intelligent production control systems, and optimize production parameters to improve product quality and production efficiency. The logistic regression model is used to establish the relationship between input variables and binary output variables. The logistic regression model can be used for classification problems in intelligent production control systems. Support vector machine (SVM) is a commonly used classifier. In the formula, the sample category is judged by the inner product of the input feature vector and the weight vector plus the bias term.
[0049] Preferably, in step 5, the stirring speed interval of the stirrer is 100r / min-500r / min, and the stirring time interval of the stirrer is 30min-80min. In step 5, the nitrogen dissolution reaction in the stirring and dissolving process obeys Xihuat's law, and the solubility of the gas is proportional to the square root of the partial pressure of the gas in the gas phase. The dissolution reaction formula is: Wherein, w[N] is the solubility of nitrogen in molten iron; is the equilibrium constant of the reaction; The partial pressure of nitrogen in the gas phase that is in equilibrium with the nitrogen in the molten steel.
[0050] Preferably, in step nine, after the nitrogen content reaches the target, the steel is cooled to 20°C-30°C, and the cooling time interval is 15min-40min.
[0051] Preferably, in step 10, the specific implementation method of taking energy-saving and emission-reduction measures is as follows:
[0052] a. Use energy-saving lamps and lighting control systems to reduce lighting energy consumption;
[0053] b. Install energy-saving air-conditioning systems, heating systems and insulation materials to reduce building energy consumption;
[0054] c. Use high-efficiency energy-saving motors and variable frequency speed regulators to reduce motor energy consumption;
[0055] d. Use waste heat recovery technology to recover energy using waste heat.
[0056] The use of LED energy-saving lamps can reduce lighting energy consumption. In addition, a lighting control system can automatically adjust the lighting brightness according to actual needs to avoid energy waste. Energy-saving air-conditioning equipment and heat pump systems are used to optimize the working mode of the heating system, and insulation materials are used in buildings to reduce energy transfer and loss, and reduce air-conditioning and heating energy consumption. By installing a variable frequency speed regulator, the operating speed of the motor can be adjusted according to actual load requirements to avoid excessive energy consumption. By adopting waste heat recovery technology, waste heat can be converted into reusable energy, which can maximize energy utilization efficiency, reduce dependence on other energy sources, and achieve energy recycling.
[0057] Depend on Figure 4 It can be seen that as the desulfurization rate in steel increases from 0.019% to 0.060%, the nitrogen content in molten steel increases from 0.0010% to 0.0030%. The main reason is that the conditions for refining and desulfurization are high temperature, high basicity, large slag volume, and low oxidizability. While oxygen as a surface active element decreases, the effect of molten steel in inhibiting nitrogen absorption decreases. Under the stirring action of argon flow, the exposed surface of molten steel increases, which increases the mass transfer coefficient of nitrogen in the air to molten steel, and the nitrogen content of molten steel increases. Therefore, the molten iron must be deeply desulfurized during pretreatment to ensure that the sulfur content of the molten iron entering the furnace is below 0.012%. At the same time, in order to reduce the nitrogen absorption in the slag making and desulfurization process of the refining process, an effective method is to slag in advance. Therefore, the converter is doped with 150kg-200kg of white ash during the steel tapping process, and slag desulfurization is performed during the steel tapping deoxidation and alloying process to reduce the sulfur content in the LF refining incoming steel, and increase the desulfurization time within a fixed refining time.
[0058] The present invention provides a production method for accurately controlling the nitrogen content of vanadium-containing steel. It has the following beneficial effects:
[0059] 1. The present invention uses an automated nitrogen source addition system and accurately controls the addition amount and rate of the nitrogen source according to real-time nitrogen content monitoring data, thereby accurately controlling the nitrogen content in vanadium steel, ensuring product quality stability, avoiding the problem of low product performance due to component differences, and thus improving product reliability. Accurately controlling the nitrogen content can reduce the defective rate of the product, avoid product defects caused by component deviations, and reduce waste and costs in the production process.
[0060] 2. The present invention can monitor the parameters in the production process in real time through the intelligent production control system, and automatically adjust the production parameters according to the set target values, so as to achieve precise control of the nitrogen content of vanadium-containing steels and improve the stability of the production process. The intelligent system can optimize the production process, improve production efficiency, reduce the waste of energy and raw materials, reduce production costs, and enhance the competitiveness of enterprises. At the same time, the intelligent system reduces the possibility of human intervention, reduces the error rate of operators, and improves the stability and reliability of the production process. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 It is a schematic diagram of the process of the present invention;
[0062] Figure 2 A schematic diagram of the operating steps of the automated nitrogen source addition system of the present invention;
[0063] Figure 3 It is a schematic diagram of the operation steps of the intelligent production control system of the present invention;
[0064] Figure 4 It is a schematic diagram of the change of nitrogen increase amount under the desulfurization rate of the present invention. DETAILED DESCRIPTION
[0065] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0066] It should be noted that the terms "first" and "second" in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0067] The present invention is described in detail below in conjunction with the accompanying drawings:
[0068] Embodiment 1:
[0069] Please see attached Figure 1 - Attachment Figure 4 The embodiment of the present invention provides a production method for accurately controlling the nitrogen content of vanadium-containing steel, comprising the following steps:
[0070] Step 1: Preparation of raw materials, preparation of vanadium-containing steel and nitrogen source;
[0071] Step 2: Melting: placing the vanadium-containing steel into a melting furnace and melting it at an internal temperature range of 1600°C-1750°C for 2 hours;
[0072] Step 3: Automated nitrogen source addition system: Install nitrogen supply system, valves, flow meter, design control system, develop feedback algorithm, install nitrogen content online monitoring system, and connect the control system with nitrogen source addition equipment;
[0073] Step 4: Intelligent production control system: deploy temperature sensors, pressure sensors, humidity sensors, design data acquisition systems, perform data processing and analysis, apply artificial intelligence algorithms, design intelligent control systems, integrate sensors and control systems, and monitor and adjust production parameters in real time;
[0074] Step 5: Stirring and mixing: the stirring speed range of the stirrer is 200r / min-400r / min, and the stirring time is 60min;
[0075] Step 6: Real-time monitoring and feedback control: real-time monitoring of nitrogen content by online nitrogen content monitoring equipment, and automatic adjustment of smelting parameters according to the feedback control system;
[0076] Step 7: Reaction time: Control the reaction time to ensure that the nitrogen element is fully dissolved and diffused into the steel;
[0077] Step 8: Sampling and analysis: Take samples regularly to analyze and test the nitrogen content in the molten steel;
[0078] Step 9: Cooling and solidification: When the nitrogen content reaches the target, cool the steel to 25°C for 30 minutes;
[0079] Step 10. Environmental protection measures: Adopt waste heat recovery technology, use high-efficiency energy-saving motors and variable frequency speed regulators to reduce energy consumption.
[0080] Embodiment 2:
[0081] Please see attached Figure 1 - Attachment Figure 4 The embodiment of the present invention provides a production method for accurately controlling the nitrogen content of vanadium-containing steel, comprising the following steps:
[0082] Step 1: Preparation of raw materials: preparation of vanadium-containing steel and nitrogen source;
[0083] Step 2: Melting: Put the vanadium-containing steel into a melting furnace and melt it at an internal temperature range of 1650°C-1800°C for 3 hours;
[0084] Step 3: Automated nitrogen source addition system: Install nitrogen supply system, valves, flow meter, design control system, develop feedback algorithm, install nitrogen content online monitoring system, and connect the control system with nitrogen source addition equipment;
[0085] Step 4: Intelligent production control system: deploy temperature sensors, pressure sensors, humidity sensors, design data acquisition systems, perform data processing and analysis, apply artificial intelligence algorithms, design intelligent control systems, integrate sensors and control systems, and monitor and adjust production parameters in real time;
[0086] Step 5: Stirring and mixing: the stirring speed range of the stirrer is 150r / min-450r / min, and the stirring time is 45min;
[0087] Step 6: Real-time monitoring and feedback control: real-time monitoring of nitrogen content by online nitrogen content monitoring equipment, and automatic adjustment of smelting parameters according to the feedback control system;
[0088] Step 7: Reaction time: Control the reaction time to ensure that the nitrogen element is fully dissolved and diffused into the steel;
[0089] Step 8: Sampling and analysis: Take samples regularly to analyze and test the nitrogen content in the molten steel;
[0090] Step 9: Cooling and solidification: When the nitrogen content reaches the target, cool the steel to 30°C for 20 minutes;
[0091] Step 10. Environmental protection measures: Use energy-saving lamps and lighting control systems, install energy-saving air-conditioning systems and insulation materials to reduce energy consumption.
[0092] Embodiment three:
[0093] Please see attached Figure 1 - Attachment Figure 4 The embodiment of the present invention provides a production method for accurately controlling the nitrogen content of vanadium-containing steel, comprising the following steps:
[0094] Step 1: Preparation of raw materials: prepare vanadium-containing steel and nitrogen source;
[0095] Step 2: Melting: Put the vanadium-containing steel into a melting furnace and melt it at an internal temperature range of 1550°C-1700°C for 1.5 hours;
[0096] Step 3: Automated nitrogen source addition system: Install nitrogen supply system, valves, flow meters, design control system, develop feedback algorithm, install nitrogen content online monitoring system, and connect the control system with nitrogen source addition equipment;
[0097] Step 4: Intelligent production control system: deploy temperature sensors, pressure sensors, humidity sensors, design data acquisition systems, perform data processing and analysis, apply artificial intelligence algorithms, design intelligent control systems, integrate sensors and control systems, and monitor and adjust production parameters in real time;
[0098] Step 5: Stirring and mixing: The stirring speed range of the stirrer is 120r / min-400r / min, and the stirring time is 50min;
[0099] Step 6: Real-time monitoring and feedback control: The nitrogen content is monitored in real time by online nitrogen content monitoring equipment, and the smelting parameters are automatically adjusted according to the feedback control system;
[0100] Step 7: Reaction time: Control the reaction time to ensure that the nitrogen element is fully dissolved and diffused into the steel;
[0101] Step 8: Sampling and analysis: Take samples regularly to analyze and test the nitrogen content in the molten steel;
[0102] Step 9: Cooling and solidification: When the nitrogen content reaches the target, cool the steel to 22°C for 25 minutes;
[0103] Step 10: Environmental protection measures: Use high-efficiency energy-saving motors and variable frequency speed regulators, use energy-saving lamps and lighting control systems to reduce energy consumption.
[0104] Embodiment 4:
[0105] Please see attached Figure 1 - Attachment Figure 4 The embodiment of the present invention provides a production method for accurately controlling the nitrogen content of vanadium-containing steel, comprising the following steps:
[0106] Step 1: Preparation of raw materials: prepare vanadium-containing steel and nitrogen source;
[0107] Step 2: Melting: Put the vanadium-containing steel into a melting furnace and melt it at an internal temperature range of 1700°C-1850°C for 3.5 hours;
[0108] Step 3: Automated nitrogen source addition system: Install nitrogen supply system, valves, flow meters, design control system, develop feedback algorithm, install nitrogen content online monitoring system, and connect the control system with nitrogen source addition equipment;
[0109] Step 4: Intelligent production control system: deploy temperature sensors, pressure sensors, humidity sensors, design data acquisition systems, perform data processing and analysis, apply artificial intelligence algorithms, design intelligent control systems, integrate sensors and control systems, and monitor and adjust production parameters in real time;
[0110] Step 5: Stirring and mixing: The stirring speed range of the stirrer is 150r / min-500r / min, and the stirring time is 60min;
[0111] Step 6: Real-time monitoring and feedback control: The nitrogen content is monitored in real time by online nitrogen content monitoring equipment, and the smelting parameters are automatically adjusted according to the feedback control system;
[0112] Step 7: Reaction time: Control the reaction time to ensure that the nitrogen element is fully dissolved and diffused into the steel;
[0113] Step 8: Sampling and analysis: Take samples regularly to analyze and test the nitrogen content in the molten steel;
[0114] Step 9: Cooling and solidification: When the nitrogen content reaches the target, cool the steel to 28°C for 35 minutes;
[0115] Step 10: Environmental protection measures: Use waste heat recovery technology, install energy-saving air-conditioning systems and insulation materials to reduce energy consumption.
[0116] Embodiment five:
[0117] Please see attached Figure 1 - Attachment Figure 4 The embodiment of the present invention provides a production method for accurately controlling the nitrogen content of vanadium-containing steel, comprising the following steps:
[0118] Step 1: Preparation of raw materials: prepare vanadium-containing steel and nitrogen source;
[0119] Step 2: Melting: Put the vanadium-containing steel into a melting furnace and melt it at an internal temperature range of 1620℃-1770℃ for 2.5h;
[0120] Step 3: Automated nitrogen source addition system: Install nitrogen supply system, valves, flow meters, design control system, develop feedback algorithm, install nitrogen content online monitoring system, and connect the control system with nitrogen source addition equipment;
[0121] Step 4: Intelligent production control system: deploy temperature sensors, pressure sensors, humidity sensors, design data acquisition systems, perform data processing and analysis, apply artificial intelligence algorithms, design intelligent control systems, integrate sensors and control systems, and monitor and adjust production parameters in real time;
[0122] Step 5: Stirring and mixing: The stirring speed range of the stirrer is 130r / min-450r / min, and the stirring time is 55min;
[0123] Step 6: Real-time monitoring and feedback control: The nitrogen content is monitored in real time by online nitrogen content monitoring equipment, and the smelting parameters are automatically adjusted according to the feedback control system;
[0124] Step 7: Reaction time: Control the reaction time to ensure that the nitrogen element is fully dissolved and diffused into the steel;
[0125] Step 8: Sampling and analysis: Take samples regularly to analyze and test the nitrogen content in the molten steel;
[0126] Step 9: Cooling and solidification: When the nitrogen content reaches the target, cool the steel to 26°C for 30 minutes;
[0127] Step 10: Environmental protection measures: Use high-efficiency energy-saving motors and variable frequency speed regulators, use energy-saving lamps and lighting control systems to reduce energy consumption.
[0128] Summary:
[0129] There are significant differences between Example 1 and Example 2 in terms of smelting temperature, time, stirring parameters and cooling conditions, but both adopt advanced automation and intelligent technologies, as well as environmental protection measures, to ensure the production process of accurately controlling the nitrogen content of vanadium-containing steel, which can improve production efficiency, reduce energy consumption, and ensure stable product quality; there are significant differences between Example 3 and Example 4 in terms of smelting parameters, stirring methods, and cooling conditions, but both adopt advanced automation and intelligent technologies, as well as environmental protection measures, to ensure the production process of accurately controlling the nitrogen content of vanadium-containing steel, which can improve production efficiency, reduce energy consumption, and ensure stable product quality; Example 5 adopts a precise control method, including an automated nitrogen source addition system, an intelligent production control system, and stirring, mixing, and real-time monitoring steps, and ensures precise control of the nitrogen content of vanadium-containing steel by optimizing smelting parameters and production processes. At the same time, energy-saving and emission reduction measures are adopted to improve production efficiency and reduce environmental pollution.
[0130] Experimental design:
[0131] Comparative experiment 1: Effect of melting temperature on nitrogen content
[0132] Experimental group operation steps:
[0133] The first step is to prepare vanadium-containing steel and nitrogen source, with an amount of 100 grams, and accurately weigh them using a precision balance in a dry environment;
[0134] The second step is to use an arc melting furnace to put 100 grams of vanadium-containing steel and nitrogen source into the furnace, and melt them at an internal temperature range of 1600°C-1750°C. The melting process should last for 60 minutes.
[0135] Step 3: Use a high-temperature thermal imager to monitor the temperature changes in the furnace;
[0136] Step 4: The temperature control range of the furnace is 1600℃-1750℃, which can be monitored and adjusted by the thermometer inside the furnace;
[0137] Step 5: Control the laboratory environment temperature to 20-25°C and the relative humidity to 40%-60%;
[0138] Step 6: Start the automated nitrogen source addition system and intelligent production control system to maintain stable production conditions;
[0139] Step 7: Use a time recording instrument to accurately record the details and duration of system operations;
[0140] Step 8: Take samples regularly to analyze and test the nitrogen content in the molten steel;
[0141] Control group operation steps:
[0142] The first step is to prepare vanadium-containing steel and nitrogen source, with an amount of 100 grams, and accurately weigh them using a precision balance in a dry environment;
[0143] The second step is to use an arc melting furnace to put 100 grams of vanadium-containing steel and nitrogen source into the furnace and melt them at an internal temperature range of 1650°C-1800°C. The melting process needs to last for 60 minutes.
[0144] Step 3: Use a high-temperature thermal imager to monitor the temperature changes in the furnace;
[0145] Step 4: The temperature control range of the furnace is 1650℃-1800℃, which can be monitored and adjusted by the thermometer inside the furnace;
[0146] Step 5: Control the laboratory environment temperature to 20-25°C and the relative humidity to 40%-60%;
[0147] Step 6: Start the automated nitrogen source addition system and intelligent production control system to maintain stable production conditions;
[0148] Step 7: Use a time recording instrument to accurately record the details and duration of system operations;
[0149] Step 8: Take samples regularly and analyze and test the nitrogen content in the molten steel.
[0150] Experimental data table:
[0151]
[0152]
[0153] Comparative experiment 2: Effect of stirring and mixing conditions on nitrogen content
[0154] Experimental group operation steps:
[0155] The first step is to prepare vanadium-containing steel and nitrogen source, with an amount of 120 grams, and accurately weigh them using a precision balance in a dry environment;
[0156] The second step is to use a high-speed stirrer for smelting operation, and set the stirring speed to 300r / min and the stirring time to 50min;
[0157] Step 3: Use a mixing mechanics calculation instrument to monitor the mechanical parameters during the mixing process and record the precise settings and operation time of the mixing equipment;
[0158] Step 4: The laboratory environment temperature control range is 20-25℃, and the relative humidity control range is 40%-60%.
[0159] Step 5: Start the automated nitrogen source addition system and intelligent production control system to maintain stable production conditions;
[0160] Step 6: Use a time recording instrument to accurately record the details and duration of system operations;
[0161] Control group operation steps:
[0162] The first step is to prepare vanadium-containing steel and nitrogen source, with an amount of 120 grams, and accurately weigh them using a precision balance in a dry environment;
[0163] The second step is to use a high-speed stirrer for smelting operation, and set the stirring speed to 400r / min and the stirring time to 60min;
[0164] Step 3: Use a mixing mechanics calculation instrument to monitor the mechanical parameters during the mixing process and record the precise settings and operation time of the mixing equipment;
[0165] Step 4: The laboratory environment temperature is controlled within the range of 20-25°C and the relative humidity is controlled within the range of 40%-60%;
[0166] Step 5: Start the automated nitrogen source addition system and intelligent production control system to maintain stable production conditions;
[0167] Step 6. Use a time recording instrument to accurately record the details and duration of system operations.
[0168] Experimental data table:
[0169] Stirring time (min) Nitrogen content in experimental group (%) Nitrogen content of control group (%) 50 0.27 0.24 60 0.32 0.29
[0170] Comparative experiment 3: Effect of cooling and solidification conditions on nitrogen content
[0171] Experimental group operation steps:
[0172] The first step is to prepare vanadium-containing steel and nitrogen source, with an amount of 150 grams, and accurately weigh them using a precision balance in a dry environment;
[0173] Step 2: Pour equal amounts of vanadium-containing steel and nitrogen source into a smelting furnace for smelting, and set the cooling temperature to 26°C and the cooling time to 30 minutes;
[0174] Step 3: After the smelting is completed, use a thermometer and timer to accurately measure the temperature;
[0175] Step 4: Control the laboratory environment temperature to 20-25°C and the relative humidity to 40%-60%;
[0176] Step 5: Start the automated nitrogen source addition system and intelligent production control system to maintain stable production conditions;
[0177] Step 6: Use a time recording instrument to accurately record the details and duration of system operations;
[0178] Control group operation steps:
[0179] The first step is to prepare vanadium-containing steel and nitrogen source, with an amount of 150 grams, and accurately weigh them using a precision balance in a dry environment;
[0180] Step 2: Pour equal amounts of vanadium-containing steel and nitrogen source into a smelting furnace for smelting, and set the cooling temperature to 28°C and the cooling time to 35 minutes;
[0181] Step 3: After the smelting is completed, use a thermometer and timer to accurately measure the temperature;
[0182] Step 4: Control the laboratory environment temperature to 20-25°C and the relative humidity to 40%-60%.
[0183] Step 5: Start the automated nitrogen source addition system and intelligent production control system to maintain stable production conditions;
[0184] Step 6. Use a time recording instrument to accurately record the details and duration of system operations.
[0185] Experimental data table:
[0186] Cooling time (min) Nitrogen content in experimental group (%) Nitrogen content of control group (%) 30 0.28 0.25 35 0.33 0.30
[0187] Comparative experiment summary:
[0188] Comparative experiment 1: Effect of melting temperature on nitrogen content
[0189] The experiment found that as the melting temperature increased, the nitrogen content in the steel showed an upward trend;
[0190] In the experimental group, the nitrogen content reached the highest value of 0.39% when the melting temperature was 1750°C;
[0191] The nitrogen content of the control group was 0.36% at a melting temperature of 1750°C;
[0192] The nitrogen content of the experimental group was significantly higher than that of the control group, indicating that the nitrogen content was more easily increased at higher melting temperatures.
[0193] Comparative experiment 2: Effect of stirring and mixing conditions on nitrogen content
[0194] The experimental results show that the effect of stirring time on the nitrogen content in steel
[0195] The nitrogen content of the experimental group reached 0.32% when the stirring time was 60 min, while that of the control group was 0.29% under the same conditions;
[0196] The nitrogen content in the experimental group was slightly higher than that in the control group, indicating that a longer stirring time was helpful to increase the nitrogen content.
[0197] Comparative experiment 3: Effect of cooling and solidification conditions on nitrogen content
[0198] When the cooling time was 35 min, the nitrogen content of the experimental group reached 0.33%, while that of the control group was 0.30%;
[0199] The nitrogen content in the experimental group was higher than that in the control group, indicating that a longer cooling period was helpful in increasing the nitrogen content.
[0200] Based on the results of the three groups of experiments, it can be seen that under the conditions of high melting temperature, long stirring time and long cooling time, the nitrogen content in the steel will be relatively high. The experimental results provide an important reference for studying steel properties and provide guidance for optimizing the production process.
[0201] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A production method for accurately controlling the nitrogen content of vanadium-containing steel, characterized in that: The following steps are involved: Step 1: Preparation of raw materials: prepare raw materials containing vanadium steel and nitrogen source; Step 2: Smelting: placing the vanadium-containing steel into a smelting furnace for smelting; Step 3: Automated nitrogen source addition system: accurately control the amount and rate of nitrogen source addition based on real-time nitrogen content monitoring data; Step 4: Intelligent production control system: Equipped with an intelligent production control system to monitor and adjust the temperature, pressure and atmosphere parameters during the smelting process in real time; Step 5: stirring and mixing: During the smelting process, the smelting furnace is stirred by means of a stirrer to make the nitrogen source evenly dissolved in the molten steel; Step 6: Real-time monitoring and feedback control: Online nitrogen content monitoring equipment monitors the nitrogen content in the molten steel in real time and automatically adjusts the smelting parameters in combination with the feedback control system; Step 7. Reaction time: Control the reaction time according to the nitrogen content and steel characteristics to ensure that the nitrogen element is fully dissolved and diffused into the steel; Step 8: Sampling and analysis: Take samples regularly to analyze and test the nitrogen content in the molten steel; Step 9: Cooling and solidification: After the nitrogen content reaches the target, control the cooling rate to make the steel solidify evenly; Step 10. Environmental protection measures: Take energy-saving and emission-reduction measures to reduce environmental pollution during the production process.
2. A production method for accurately controlling the nitrogen content of vanadium-containing steel according to claim 1, characterized in that: In the step 2, the internal temperature range of the smelting furnace during the smelting process is 1600° C.-1750° C., and the smelting treatment time range is 0.5 h-4 h.
3. A production method for accurately controlling the nitrogen content of vanadium-containing steel according to claim 1, characterized in that: In step 3, the operation steps of the automated nitrogen source addition system are as follows: a. Install nitrogen source adding equipment, including nitrogen supply system, valves, flow meter, used to add nitrogen source into the smelting furnace; b. Design control system, including sensors, actuators, and controller components, to monitor nitrogen content and control nitrogen source addition; c. Develop a feedback algorithm to adjust the amount of nitrogen source added based on real-time monitoring data and the set target range; d. Install an online nitrogen content monitoring system to monitor the nitrogen content in the molten steel in real time and feed the monitoring data back to the control system; e. Connect the control system to the nitrogen source adding equipment. The system automatically adjusts the amount of nitrogen source added based on monitoring data and feedback algorithms.
4. A production method for accurately controlling the nitrogen content of vanadium-containing steel according to claim 3, characterized in that: In step 3, the formula of the feedback algorithm is: Among them, K p is the proportional gain, K i is the integration time constant, K d is the differential time constant, e(t) is the error signal, that is, the difference between the set value and the actual value, represents the integral term of the error, Represents the differential term of the error.
5. The production method for accurately controlling the nitrogen content of vanadium-containing steel according to claim 1, characterized in that: In step 4, the operation steps of the intelligent production control system are as follows: a. Sensor deployment: deploy temperature sensors, pressure sensors, and humidity sensors; b. Data acquisition: Design a data acquisition system to collect data transmitted by sensors; c. Data processing: process and analyze the collected data; d. Application of artificial intelligence algorithms: Use artificial intelligence algorithms to analyze and model data; e. Control system design: Design intelligent control systems and apply artificial intelligence algorithms to control systems; f. System integration: Integrate sensors, data acquisition systems, artificial intelligence algorithms and control systems to establish a complete intelligent production control system; g. Real-time monitoring and adjustment: Adjust and optimize production parameters based on monitoring data.
6. A production method for accurately controlling the nitrogen content of vanadium-containing steel according to claim 5, characterized in that: In the step 4, the intelligent production control system processes and analyzes the collected data, including data cleaning, feature extraction, and data modeling; data cleaning refers to processing the original data to remove erroneous data; feature extraction refers to extracting features valuable for problem modeling from the original data, usually involving data conversion, dimensionality reduction, or selection of specific features; Data modeling is the use of machine learning and deep learning algorithms to model and train data after cleaning and feature extraction.
7. A production method for accurately controlling the nitrogen content of vanadium-containing steel according to claim 5, characterized in that: In the step 4, the artificial intelligence algorithm includes a linear regression model formula, a logistic regression model formula, and a SVM classifier formula; Linear regression model formula: [y=w0+w1x1+w2x2+…+w n x n ], Among them, y is the input variable, (x1, x2, …, x n ) are input variables, (w0,w1,w2,…,w n ) are model parameters; Logistic regression model formula: Among them, P(y=1|x) is the probability of the output being category 1, (x1,x2,…,x n ) are input variables, (w0,w1,w2,…,w n ) are model parameters; SVM classifier formula: [f(x) = sign(w T ·x+b)], Where f(x) is the output of the classifier, x is the input feature vector, w is the weight vector, and b is the bias term.
8. The production method for accurately controlling the nitrogen content of vanadium-containing steel according to claim 1, characterized in that: In the step 5, the stirring speed range of the stirrer is 100r / min-500r / min, and the stirring time range of the stirrer is 30min-80min. In the step 5, the nitrogen dissolution reaction in the stirring and dissolving process obeys Xihuat's law, and the solubility of the gas is proportional to the square root of the partial pressure of the gas in the gas phase. The dissolution reaction formula is: Where w[N] is the solubility of nitrogen in molten iron; K N2 is the equilibrium constant of the reaction; P N2 The partial pressure of nitrogen in the gas phase that is in equilibrium with the nitrogen in the molten steel.
9. The production method for accurately controlling the nitrogen content of vanadium-containing steel according to claim 1, characterized in that: In the step nine, after the nitrogen content reaches the target, the steel is cooled to 20°C-30°C, and the cooling time interval is 15min-40min.
10. A production method for accurately controlling the nitrogen content of vanadium-containing steel according to claim 1, characterized in that: In step 10, the specific implementation method of taking energy-saving and emission-reduction measures is as follows: a. Use energy-saving lamps and lighting control systems to reduce lighting energy consumption; b. Install energy-saving air-conditioning systems, heating systems and insulation materials to reduce building energy consumption; c. Use high-efficiency energy-saving motors and variable frequency speed regulators to reduce motor energy consumption; d. Use waste heat recovery technology to recover energy using waste heat.
Citation Information
Cited By
Steelmaking process method and system based on smelting temperature data optimization
CN122411633A
Steelmaking process optimization based on smelting temperature data: methods and systems
CN122411633B