Heat treatment equipment
By controlling the atmosphere dew point in the metal strip bright annealing device and using SiO2 fiber insulation materials, the problem of ceramic fibers easily disintegrating in a reducing atmosphere is solved, and high-quality bright annealing of metal strips and long life of the insulation materials are achieved.
Patent Information
- Application Number
- CN202080083926.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-20
- Filing Date
- 2020-11-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-11-27
AI Technical Summary
When existing metal strip bright annealing devices use ceramic fiber insulation materials in a reducing atmosphere, SiO2 is easily reduced, causing material disintegration and dust generation, affecting the quality of the metal strip.
By controlling the dew point of the atmosphere in the heating belt to keep it between the upper limit dew point that can maintain the brightness of the metal belt and the lower limit dew point that prevents the reduction of SiO2, use ceramic fibers containing SiO2 as thermal insulation materials, and adjust the atmosphere through dehumidification or humidification devices The amount of moisture in it prevents the reduction of SiO2.
It effectively inhibits the oxidation of the surface of the metal strip, maintains the brightness of the metal strip, and prevents the reduction of SiO2 in the thermal insulation material, extending the service life of the ceramic fiber and avoiding the generation of dust.
Smart Images

Figure CN114761585B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a heat treatment apparatus for bright annealing a metal strip. Background Art
[0002] In order to remove the internal stress of the metal strip caused by cold rolling, a heat treatment apparatus is known which performs bright annealing of the metal strip in a reducing atmosphere.
[0003] Patent Document 1 discloses a continuous annealing furnace for hot dip plating having a muffle furnace structure in which a low temperature holding zone is composed of steel plates, which is a so-called horizontal furnace that conveys a metal strip in a horizontal direction. Patent Document 2 discloses a horizontal bright continuous annealing furnace for a metal strip in which a furnace is lined with refractory bricks. Patent Document 3 discloses a manufacturing facility for a nickel-plated thin steel plate in which the heat insulating material in the furnace is composed of ceramic fibers.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Utility Model Publication No. 03-1472
[0007] Patent Document 2: Japanese Patent No. 4268281
[0008] Patent Document 3: Japanese Patent Application Publication No. 2003-201595 Summary of the invention
[0009] Technical problem to be solved by the invention
[0010] In Patent Document 1, since the muffle furnace structure of the furnace body is composed of steel plates, it is deformed by heating at high temperatures. In particular, in the case of a horizontal furnace, since the furnace roof is made of steel plates in a long section, the furnace roof sags due to its own weight, the deformation in shape is large, the air flow in the furnace is turbulent, and the temperature distribution in the furnace is poor. In Patent Document 2, although refractory bricks are not easily deformed, due to the heavy weight of refractory bricks, the workability during assembly, maintenance and replacement is poor, and the weight of the annealing furnace is also heavy, so the annealing furnace needs to be set in a place with load resistance.
[0011] In Patent Document 3, ceramic fibers are used because the annealing of the steel plate and the diffusion treatment of the nickel plating are performed at about 800°C in a non-reducing atmosphere. Ceramic fibers are light in weight and have excellent workability, but since they contain SiO2, SiO2 is reduced in a high-temperature reducing atmosphere and SiO2 is converted to Si. Therefore, the ceramic fibers disintegrate, and frequent maintenance and replacement of the ceramic fibers are required. Dust is generated when the ceramic fibers disintegrate, and the dust falls on the metal strip. In particular, in the case of a horizontal furnace, since the area of the furnace top is large, the amount of dust falling is large, and the quality of the metal strip is reduced.
[0012] Therefore, the technical problem of the present invention is to provide a heat treatment apparatus for bright annealing a metal strip, which can suppress the degradation of a heat insulating material made of ceramic fibers containing SiO2 even in a reducing atmosphere.
[0013] Technical solutions adopted to solve technical problems
[0014] In order to solve the above-mentioned technical problems, a heat treatment device according to one embodiment of the present invention is characterized in that it is provided with a heating belt for heating a metal strip, an insulating material used as the furnace inner wall of the heating belt and made of ceramic fibers containing SiO2, and a gas supply part for supplying a reducing gas to the heating belt, so that the dew point is maintained between an upper limit dew point that can make the metal strip bright and a lower limit dew point that will not reduce the SiO2 contained in the insulating material, and bright annealing is performed on the metal strip in a reducing atmosphere.
[0015] In order to solve the above-mentioned technical problems, a heat treatment device in one embodiment of the present invention is a heat treatment device for bright annealing a metal strip in a reducing atmosphere, characterized in that the heat treatment device comprises: a furnace body, the furnace body having a heating belt for heating the metal strip, and a cooling belt arranged on the downstream side of the conveying direction of the metal strip relative to the heating belt; an insulating material, the insulating material is used as the furnace inner wall of the heating belt and is made of ceramic fiber containing SiO2; a gas supply unit for supplying reducing gas into the furnace body; a dew point measuring unit for measuring the dew point of the atmosphere in the heating belt; and a dew point adjusting unit for adjusting the dew point, the dew point adjusting unit being controlled according to the dew point measured by the dew point measuring unit so that the dew point is maintained between an upper limit dew point that can make the metal strip bright and a lower limit dew point that will not reduce the SiO2 contained in the insulating material.
[0016] Effects of the Invention
[0017] The less moisture in the atmosphere in the furnace, the more favorable it is to the brightness of the metal strip, which can suppress the oxidation of the metal strip surface. However, when lightweight ceramic fibers are used as thermal insulation materials for the inner wall of the furnace, they act in the direction of reducing SiO2 contained in the thermal insulation materials, which is disadvantageous to the thermal insulation materials. Therefore, the inventors of the present application have realized the existence of a dew point (i.e., moisture content) within an appropriate range that can simultaneously achieve the maintenance of brightness and the prevention of SiO2 reduction, and have achieved the present invention.
[0018] According to the present invention, by keeping the dew point (i.e., moisture content) of the atmosphere in the heating zone between the upper limit dew point and the lower limit dew point, the moisture content in the reducing atmosphere is suitable for maintaining the brightness of the metal strip and preventing the reduction of SiO2 contained in the thermal insulation material. As a result, the metal strip can be made bright and the degradation of the thermal insulation material due to the reduction of SiO2 contained in the thermal insulation material can be prevented. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic cross-sectional view of the heat treatment apparatus according to the first embodiment.
[0020] Figure 2 This is a diagram schematically illustrating the relationship between temperature and dew point of the atmosphere.
[0021] Figure 3 This is a diagram schematically illustrating the relationship between temperature and dew point of the atmosphere.
[0022] Figure 4 It is a schematic cross-sectional view of another form of the heat treatment apparatus according to the first embodiment.
[0023] Figure 5 It is a schematic cross-sectional view of a heat treatment apparatus according to a second embodiment.
[0024] Figure 6 It is a schematic cross-sectional view of another form of the heat treatment apparatus according to the second embodiment. DETAILED DESCRIPTION
[0025] Hereinafter, an embodiment of a heat treatment apparatus 1 according to the present invention will be described with reference to the drawings.
[0026] [First embodiment]
[0027] Reference Figure 1 , a heat treatment apparatus 1 according to a first embodiment will be described. Figure 1 It is a schematic cross-sectional view of the heat treatment apparatus 1 according to the first embodiment.
[0028] like Figure 1 As shown, a bright annealing furnace (heat treatment device) 1 for continuously bright annealing a metal strip 3 includes a furnace body 10 , gas supply units 9 , 28 , a dew point measuring unit 22 , dew point adjusting units 24 , 27 , and a control unit 20 . Figure 1 The bright annealing furnace (heat treatment device) 1 shown is a horizontal furnace whose furnace body extends in the lateral direction (horizontal direction). In a horizontal furnace, the conveying mechanism for conveying the metal strip 3 can be simplified, and the height of the heat treatment device 1 can be suppressed from increasing.
[0029] exist Figure 1In the embodiment, the metal strip 3 is conveyed horizontally from left to right. The metal strip 3 is formed of, for example, a stainless steel material containing Cr. The stainless steel material containing Cr is, for example, austenitic stainless steel SUS304 or ferritic stainless steel SUS430.
[0030] The furnace body 10 is composed of a steel box body, and has a heating belt 12 and a cooling belt 14. The heating belt 12 extends in the lateral direction (horizontal direction) and is arranged on the upstream side of the conveying direction of the metal strip 3 (the inlet side of the metal strip 3). The heating belt 12 is heated by a heating unit 16. The heating unit 16 is, for example, an electric heater. The control unit 20 controls the heating belt 12 according to the temperature measured by a temperature measuring unit not shown in the figure so that the heating belt 12 reaches a specified annealing temperature (here, it refers to the temperature in the heating process in the heating process and the heating process in the cooling process in the annealing). The annealing temperature in the present application refers to the furnace atmosphere temperature in the heating belt 12. For example, in the case of a common stainless steel material, the annealing temperature suitable for bright annealing is a temperature range of 800°C to 1250°C, and the control unit 20 controls the heating unit 16 in such a way that the annealing temperature falls within the above temperature range.
[0031] The cooling belt 14 is provided on the downstream side (the exit side of the metal belt 3) in the conveying direction of the metal belt 3. In the cooling belt 14, since annealing is performed, cooling is mainly performed by standing, and therefore no heating device or heat insulating material 17 is provided. However, the cooling belt 14 may be provided with some cooling device according to the situation.
[0032] The insulating material 17 is installed on the inner surface (furnace inner wall) of the furnace wall such as the side wall, furnace top and bottom of the furnace body 10. The insulating material 17 is made of ceramic fiber containing SiO2. The insulating material 17 can be constructed by, for example, piercing a plate or felt made of ceramic fiber on a large number of rod-shaped studs installed on the furnace wall and pressing with a washer-shaped metal fitting to maintain it. The insulating material 17 is a fiber with Al2O3 (aluminum oxide) and SiO2 (silicon dioxide) as main components, for example, a ceramic fiber made of alumina-silicon dioxide with an Al2O3 content of 30 to 60% by mass and an SiO2 content of 40 to 70% by mass.
[0033] The interior of the furnace body 10 of the bright annealing furnace 1 is filled with reducing atmosphere gas. The inlet sealing roller 13 and the outlet sealing roller 15 are respectively arranged at the inlet opening and the outlet opening of the furnace body 10. The inlet sealing roller 13 and the outlet sealing roller 15 prevent the external gas from invading the furnace body 10 by maintaining the pressure inside the furnace body 10 slightly higher than the atmospheric pressure. However, even if the metal strip 3 is clamped by the inlet sealing roller 13 and the outlet sealing roller 15, a trace amount of moisture will be brought into the furnace body 10 from the external air in the state of being attached to the surface of the metal strip 3 at the inlet sealing roller 13. In addition, at the outlet sealing roller 15, a trace amount of atmosphere gas flows out of the furnace in the same form. Therefore, it is necessary to measure and adjust the dew point (moisture content) of the atmosphere at the heating zone 12 from time to time.
[0034] The gas supply unit includes a gas supply device 9 and a second regulating valve 28, which supplies reducing gas to the furnace body 10 through a gas supply pipe 5. In other words, the reducing gas is supplied to the heating belt 12. The gas supply device 9 is, for example, a gas cylinder. The reducing gas is a gas containing hydrogen, such as a gas in which hydrogen and nitrogen are mixed in a ratio of 3:1. By adjusting the opening of the second regulating valve 28 provided in the gas supply pipe 5, the supply amount of the reducing gas can be controlled. The opening of the second regulating valve 28 is controlled by the control unit 20. By supplying reducing gas, the amount leaked from the inlet sealing roller 13 and the outlet sealing roller 15 can be supplemented. In addition, at Figure 1 In the bright annealing furnace 1 shown, the gas supply pipe 5 is arranged on the upstream side of the cooling zone 14, but the supply position of the reducing gas is not particularly limited. The reducing gas supplied from the gas supply pipe 5 is diffused as an atmosphere gas throughout the interior of the furnace body 10 including the heating zone 12, and then discharged to the outside of the furnace body 10.
[0035] Conventionally, the reducing gas supplied from the gas supply device 9 is a gas with a low dew point (i.e., low water content), for example, a gas with a JIS hydrogen grade 1 and a dew point of -70°C. Therefore, in the present application, the dew point of the atmosphere in the furnace can be adjusted by the dew point adjustment unit 24 provided with the dehumidifier 25 or the humidifier 26, so the reducing gas supplied from the gas supply device 9 does not need to be a gas with a low dew point (i.e., low water content). That is, as the reducing gas supplied from the gas supply device 9, a gas containing a larger amount of water than the conventional JIS hydrogen grade 1 can be used, for example, a gas equivalent to JIS hydrogen grade 2 and a dew point of -60°C can be used.
[0036] The dew point measuring unit 22 measures the dew point of the atmosphere (hereinafter sometimes referred to as "atmospheric gas") in the heating zone 12 of the furnace body 10 through the dew point measuring pipe 6. The dew point measuring unit 22 is, for example, a capacitive dew point meter or a mirror cooling dew point meter. The measured dew point data is sent to the control unit 20 and stored in the storage unit of the control unit 20. Figure 1In the bright annealing furnace 1 shown, the dew point measurement pipe 6 is arranged on the downstream side of the heating zone 12, but the measurement position of the dew point is not particularly limited.
[0037] The dew point adjustment unit includes a dew point adjustment device 24 and a first regulating valve 27, and adjusts the dew point of the atmosphere in the heating zone 12. The dew point adjustment device 24 includes at least one of a dehumidifier 25 and a humidifier 26. Thus, the dew point of the atmosphere in the heating zone 12 can be appropriately adjusted according to the dew point of the reducing gas supplied by the gas supply units 9 and 28 and the dew point of the target atmosphere.
[0038] The dew point adjusting device 24 extracts a part of the atmosphere through the inlet side duct 7 provided on the upstream side of the conveying direction of the heating belt 12, adjusts the dew point, i.e., the moisture content of the extracted atmosphere, and then returns it to the furnace body 10 through the outlet side duct 8 provided on the downstream side of the conveying direction of the heating belt 12. The atmospheric gas circulates between the dew point adjusting device 24 and the furnace body 10, so that the dew point of the atmosphere in the heating belt 12 is maintained at a specified dew point.
[0039] The dew point adjustment device 24 (i.e., the dehumidification device 25 and the humidification device 26) is controlled by the control unit 20. The circulation amount of the atmosphere gas can be controlled by adjusting the opening of the first regulating valve 27 provided in the inlet side duct 7. The opening of the first regulating valve 27 is controlled by the control unit 20.
[0040] The dehumidifier 25 has the function of removing moisture contained in the atmosphere (dehumidifying the atmosphere) and lowering the dew point of the atmosphere. The dehumidifier 25 has, for example, an adsorption tower and a separation tower filled with an adsorbent. The adsorbent is a synthetic zeolite such as a molecular sieve, a natural zeolite, activated carbon, silica gel, alumina, activated alumina, etc. Dehumidification using an adsorbent can easily control the dew point of the atmosphere after dehumidification to a specified dew point, and the obtained atmosphere is very clean.
[0041] The humidifier 26 has a function of adding moisture to the atmosphere (humidifying the atmosphere) and raising the dew point of the atmosphere by generating a gas containing moisture obtained by mixing water vapor or liquid phase water with the atmosphere and sending the gas containing moisture into the furnace body 10. The humidifier 26 is, for example, a bubbling type that passes the atmosphere through water stored in a container, a spray nozzle type that sprays water vapor in a mist form to the atmosphere, or a membrane exchange type that uses a hollow fiber membrane with high water vapor permeability.
[0042] The control unit 20 is electrically connected to the dew point measuring unit 22, the dew point adjusting device 24, the first regulating valve 27, the second regulating valve 28, and the heating unit 16. The control unit 20 can be configured using a computer including a computing unit such as a CPU (Central Processing Unit), and a storage unit such as a RAM (Random Access Memory) and a ROM (Read Only Memory).
[0043] The control unit 20 controls the gas supply units 9, 28 and the dew point adjustment units 24, 27 according to the dew point measured by the dew point measurement unit 22. That is, the control unit 20 controls the supply amount of the reducing gas supplied from the gas supply device 9 by controlling the opening of the second regulating valve 28. In addition, the control unit 20 controls the circulation amount of the atmosphere gas by the dew point adjustment device 24 by controlling the opening of the first regulating valve 27. Thereby, automation of bright annealing (heat treatment) can be realized.
[0044] The control unit 20 controls the dehumidifier 25 or the humidifier 26 in the dew point adjustment device 24 to operate. When the control unit 20 controls the dehumidifier 25 to operate, the dew point of the atmosphere, i.e., the amount of moisture, is reduced by removing the moisture contained in the atmosphere. When the control unit 20 controls the humidifier 26 to operate, the dew point of the atmosphere, i.e., the amount of moisture, is increased by increasing the moisture contained in the atmosphere. In this way, automation of bright annealing (heat treatment) can be achieved.
[0045] [Other aspects of the first embodiment]
[0046] As described above, even if a sealing structure is adopted in which the metal strip 3 is sandwiched by the inlet sealing roller 13, a small amount of moisture is brought into the interior of the furnace body 10 from the external air in a state of being attached to the surface of the metal strip 3, so the dew point (moisture content) of the atmosphere increases. Therefore, by using hydrogen gas with an extremely low dew point as a reducing gas, the moisture contained in the atmosphere can be diluted and the dew point of the atmosphere can be lowered. In addition, even if hydrogen gas with an extremely low dew point is used as a reducing gas, the dew point of the atmosphere can be increased by reducing the flow rate of the reducing gas using the second regulating valve 28. In addition, when a small amount of moisture can be prevented from being brought into the interior of the furnace body 10 from the external air by some means, by using hydrogen gas with a slightly higher dew point as a reducing gas, the moisture contained in the atmosphere can be increased and the dew point of the atmosphere can be increased.
[0047] Therefore, when not using Figure 1 In the case of the dehumidifying device 25 or the humidifying device 26 shown in the figure, the dew point of the atmosphere in the heating zone 12 can be adjusted. Figure 4 As shown, the control unit 20 controls the second regulating valve 28 according to the dew point of the atmosphere measured by the dew point measuring unit 22 to adjust the flow rate of the reducing gas supplied by the gas supply device 9, thereby adjusting the dew point of the atmosphere in the furnace body 10 including the heating zone 12. In this way, automation of bright annealing (heat treatment) can be achieved. Here, depending on the amount of moisture brought into the furnace body 10 from the external gas, hydrogen with an extremely low dew point or hydrogen with a slightly higher dew point can be used as the reducing gas supplied from the gas supply device 9. Thus, the gas supply device 9 and the second regulating valve 28 play the role of the dew point adjusting device 24a. In this way, the dew point adjusting device 24a can be configured with a simple structure.
[0048] [Control of the dew point of the atmosphere]
[0049] As described above, the less water in the atmosphere in the heating zone 12 of the furnace body 10, the oxidation of the surface of the metal strip 3 is suppressed, which is more favorable to the brightness of the metal strip 3, but it acts in the direction of reducing SiO2 contained in the insulation material 17, which is disadvantageous to the insulation material 17. Therefore, the inventors of the present application have focused on the existence of a dew point (i.e., water content) within an appropriate range that can achieve both maintaining brightness and preventing SiO2 reduction, and have achieved the present invention.
[0050] Reference Figure 2 Control of the dew point of the atmosphere in the heating zone 12 will be described. Figure 2 This is a diagram schematically illustrating the relationship between temperature and dew point of the atmosphere. Figure 2 In the graph, the horizontal axis represents the annealing temperature in the heating zone 12 and the equilibrium temperature of oxidation-reduction of SiO 2 , and the vertical axis represents the dew point of the atmosphere in the heating zone 12 . Figure 2 In FIG. 1 , A is a straight line indicating a dew point of -30°C, and S is an oxidation-reduction equilibrium curve of SiO2. When the dew point is higher than the equilibrium curve S, SiO2 is oxidized, and when the dew point is lower than the equilibrium curve S, SiO2 is reduced. In addition, the intersection points where the straight line A intersects with the annealing temperatures of 800°C and 1250°C are a and b, respectively, and the intersection points where the equilibrium curve S intersects with the equilibrium temperatures of 800°C and 1250°C are c and d, respectively. These temperatures and intersection points correspond to, for example, annealing of a stainless steel material.
[0051] The dew point of the atmosphere corresponds to the amount of water contained in the atmosphere. For example, if the dew point is -30°C, the water content is approximately 338 (g / m 3 ), the dew point is -35℃, the moisture content is about 203 (g / m 3 ), the dew point is -40℃, the moisture content is about 119 (g / m 3 ), the dew point is -45℃, the moisture content is about 68 (g / m 3 ), the dew point is -50℃, the moisture content is about 38 (g / m 3 ), the dew point is -55℃, the moisture content is about 21 (g / m 3 ), the dew point is -60℃, the moisture content is about 11 (g / m 3 ), the dew point is -65℃, the moisture content is about 5.6 (g / m 3 ), the dew point is -70℃, the moisture content is about 2.7 (g / m 3 ). Therefore, as the dew point of the atmosphere decreases, the amount of moisture contained in the atmosphere decreases.
[0052] When the surface of the metal strip 3 is oxidized, an oxide film is formed on the surface of the metal strip 3. When the metal strip 3 is a stainless steel material containing Cr, an oxide film formed by a combination of Cr and Fe with oxygen is formed. It is said that in order to suppress the surface oxidation of the metal strip 3, it is desirable that the dew point of the atmosphere is as low as possible, that is, the amount of water contained in the atmosphere is as small as possible.
[0053] However, in the actual heat treatment process, it was found that when the thickness of the oxide film formed on the surface of the metal strip 3 becomes thinner than a certain thickness, the effect on the brightness of the metal strip 3 decreases. Therefore, by making the upper limit dew point of the atmosphere below -30°C, the formation of the oxide film in the metal strip 3 can be suppressed, and the metal strip 3 has a certain degree of brightness and almost no product problems. Figure 2 The straight line A in φ represents the maximum upper limit dew point for suppressing the formation of oxide film in the metal strip 3. The intersection a is the maximum upper limit dew point at 800°C, and the intersection b is the maximum upper limit dew point at 1250°C.
[0054] When commercializing a metal strip 3 of a stainless steel material having brightness, it is appropriate to adjust the upper limit dew point of the atmosphere to be below -30°C. In the stainless steel material, in order to obtain a metal strip 3 with a higher degree of brightness, it is sufficient to adjust the upper limit dew point of the atmosphere to be below -45°C. In order to obtain a metal strip 3 with a higher degree of brightness, it is sufficient to adjust the upper limit dew point of the atmosphere to be below -65°C (straight line X in the figure). Therefore, in the stainless steel material, according to the degree of brightness of the metal strip 3 to be bright annealed, the upper limit dew point that can make the metal strip 3 have brightness is set in the range of -30°C to -65°C. According to this configuration, a metal strip 3 with desired brightness can be obtained.
[0055] A ceramic fiber insulation material 17 is provided on the inner surface of the furnace wall (furnace inner wall). Conventionally, in a horizontal bright annealing furnace 1, when refractory bricks made of high-purity alumina containing high-purity Al2O3 (alumina) are used in an arched laminated structure, the expansion and contraction of the refractory bricks when the temperature in the furnace rises and falls causes dust to be generated and the quality of the metal strip 3 to be reduced.
[0056] In the horizontal bright annealing furnace 1 of the present application, by using ceramic fibers containing SiO2 as the insulating material 17, it is possible to suppress the generation of dust and obtain a high-quality metal strip 3. However, the reduction resistance of SiO2 contained in the ceramic fiber is lower than that of Al2O3 (alumina), and when the ceramic fiber is used in a highly reducing atmosphere, it is believed that the ceramic fiber deteriorates and becomes brittle due to the reduction of SiO2, and dust is generated.
[0057] In the present invention, the inventors of the present application focus on the oxidation-reduction characteristics (thermodynamic characteristics) of SiO2, so that the thermal insulation material 17 made of ceramic fibers containing SiO2 can also be used in a highly reducing atmosphere. Figure 2 As shown, with the oxidation-reduction equilibrium curve S of SiO2 as the boundary, the upper side of the equilibrium curve S is the area where SiO2 remains in an oxidized state, and the lower side of the equilibrium curve S is the area where SiO2 is reduced.
[0058] The dew point at the intersection c where the oxidation-reduction equilibrium curve S of SiO2 intersects the equilibrium temperature of 800°C is about -95°C, and the dew point at the intersection d where the oxidation-reduction equilibrium curve S of SiO2 intersects the equilibrium temperature of 1250°C is about -60°C. This dew point is the lower limit dew point at which SiO2 contained in the heat insulating material 17 will not be reduced at the equilibrium temperature of 800°C to 1250°C, which is suitable for bright annealing of stainless steel materials, for example. Therefore, when the annealing temperature of the heating belt 12 is in the range of 800°C to 1250°C, the control unit 20 controls the dew point of the atmosphere so that it does not fall below the equilibrium curve S, thereby preventing SiO2 from being reduced. In this way, dust is prevented from being generated due to the deterioration of the heat insulating material 17 made of ceramic fibers, and a high-quality metal belt 3 can be obtained.
[0059] When the annealing temperature of the heating belt 12 is 800°C to 1250°C (for example, when the metal belt 3 is made of stainless steel), the control unit 20 controls the dew point adjustment units 24 and 27 so that the dew point of the atmosphere is within Figure 2 The heat insulating material 17 is kept within the region surrounded by the intersections a, b, d and c. Thus, the metal strip 3 can be made bright and at the same time, the heat insulating material 17 can be prevented from being deteriorated due to the reduction of SiO2 contained in the heat insulating material 17.
[0060] [Second Embodiment]
[0061] Reference Figure 5 , a heat treatment apparatus 1 according to a second embodiment will be described. Figure 5 It is a schematic cross-sectional view of a heat treatment apparatus 1 according to a second embodiment.
[0062] like Figure 5 As shown in FIG. 1 , the bright annealing furnace (heat treatment device) 1 of the second embodiment includes a furnace body 10, a gas supply unit 9, a dew point measuring unit 22, and dew point adjusting units 24, 27a, and 28a. Figure 1 Compared with the bright annealing furnace (heat treatment device) 1 of the first embodiment shown, the bright annealing furnace (heat treatment device) 1 of the second embodiment omits the control unit 20 such as a computer. Therefore, the operator who operates the bright annealing furnace (heat treatment device) 1 becomes a substitute for the control unit 20.
[0063] The operator can manually control at least one of the second regulating valve (dew point adjusting unit) 28a and the first regulating valve (dew point adjusting unit) 27a according to the dew point measured by the dew point measuring unit 22. That is, the operator can visually obtain the dew point measured by the dew point measuring unit 22 through a monitor or the like. In addition, the operator can control the supply amount of the reducing gas supplied from the gas supply device 9 by manually controlling the second regulating valve (dew point adjusting unit) 28a according to the measured dew point. In addition, the operator can control the circulation amount of the atmosphere gas based on the dew point adjusting device 24 by controlling the first regulating valve (dew point adjusting unit) 27a according to the measured dew point.
[0064] In addition, the operator controls the dehumidifier 25 in the dew point adjusting device 24 to operate, thereby removing moisture contained in the atmosphere, and the dew point, that is, the moisture content of the atmosphere is reduced. In addition, the operator controls the humidifier 26 in the dew point adjusting device 24 to operate, thereby increasing the moisture contained in the atmosphere, and thereby the dew point, that is, the moisture content of the atmosphere is increased.
[0065] Thus, by keeping the dew point (i.e., moisture content) of the atmosphere in the heating belt 12 between the upper dew point and the lower dew point, the moisture content in the reducing atmosphere is suitable for maintaining the brightness of the metal strip 3 and preventing the reduction of SiO2 contained in the heat insulating material 17. As a result, the metal strip 3 can be made bright and the deterioration of the heat insulating material 17 due to the reduction of SiO2 contained in the heat insulating material 17 can be prevented.
[0066] [Other aspects of the second embodiment]
[0067] like Figure 6 As shown, in addition to the control unit 20, the dew point adjustment device 24 (dehumidification device 25 and humidification device 26) is omitted, and the gas supply device 9 and the second regulating valve (dew point adjustment unit) 28a can also be used as the dew point adjustment device 24a. In this way, the dew point adjustment device 24a can be simply configured. The operator can control the dew point adjustment device 24a according to the dew point of the atmosphere measured by the dew point measuring unit 22. That is, the operator can visually obtain the dew point measured by the dew point measuring unit 22 through a monitor or the like. In addition, the operator can control the flow rate of the reducing gas supplied by the gas supply device 9 by manually controlling the second regulating valve (dew point adjustment unit) 28a according to the measured dew point.
[0068] Thus, by keeping the dew point (i.e., moisture content) of the atmosphere in the heating belt 12 between the upper dew point and the lower dew point, the moisture content in the reducing atmosphere is suitable for maintaining the brightness of the metal strip 3 and preventing the reduction of SiO2 contained in the heat insulating material 17. As a result, the metal strip 3 can be made bright and the deterioration of the heat insulating material 17 due to the reduction of SiO2 contained in the heat insulating material 17 can be prevented.
[0069] The manual control in the second embodiment does not need to be performed continuously by the operator all the time, and also includes a case where the operator occasionally or regularly monitors the dew point and does not perform special control if there is no abnormality.
[0070] Although specific embodiments and numerical values of the present invention have been described, the present invention is not limited to the above-described embodiments and numerical values, and can be implemented with various modifications within the scope of the present invention.
[0071] The operator may perform at least one of the following operations instead of the control unit 20: obtaining the dew point measured by the dew point measuring unit 22, and controlling the dew point adjusting units 27a, 28a according to the dew point measured by the dew point measuring unit 22 so that the dew point is maintained between the upper limit dew point and the lower limit dew point.
[0072] The bright annealing furnace (heat treatment device) 1 may also be made into a vertical furnace in which the furnace body 10 extends in the longitudinal direction (vertical direction).
[0073] In the bright annealing furnace (heat treatment device) 1, an inlet sealing belt may be provided on the upstream side of the conveying direction of the heating belt 12, and the inlet sealing roller 13 may be arranged in the inlet sealing belt. An outlet sealing belt may also be provided on the downstream side of the conveying direction of the cooling belt 14, and the outlet sealing roller 15 may be arranged in the outlet sealing belt. The heating belt 12 may be composed of an inlet sealing belt, a preheating belt, and a soaking belt (all not shown). The cooling belt 14 may be composed of an outlet sealing belt, a rapid cooling belt, and a slow cooling belt (all not shown).
[0074] Figure 1 Although the bright annealing furnace 1 shown in the figure includes both the dehumidifying device 25 and the humidifying device 26 , it may be configured to include either the dehumidifying device 25 or the humidifying device 26 .
[0075] Figure 3 The oxidation-reduction equilibrium curve C of Cr2O3 (chromium oxide) obtained by oxidation of the Cr component in the stainless steel material is shown in FIG. In the above embodiment, the upper limit of the dew point is described as -30°C, but it is considered that the oxidation of the stainless steel material can be prevented by controlling the dew point of the atmosphere so that it does not exceed the oxidation-reduction equilibrium curve C of Cr2O3. Therefore, in the case of stainless steel materials, the control unit 20 can also control the dew point adjustment unit 24, 24a so that the dew point of the atmosphere is maintained at Figure 3 The area enclosed by the intersection points e, f, d and c in .
[0076] The metal strip 3 bright annealed in a reducing atmosphere can be applied to various metal materials other than the above-mentioned stainless steel materials, such as pure metals such as nickel, titanium or copper, low expansion alloys, magnetic alloys, heat-resistant alloys, or corrosion-resistant alloys.
[0077] The present invention and embodiments can be summarized as follows.
[0078] A heat treatment device 1 according to an embodiment of the present invention is characterized in that it comprises a heating belt 12 for heating a metal strip 3, an insulating material 17 which is used as the furnace inner wall of the heating belt 12 and is made of ceramic fibers containing SiO2, and a gas supply section 9, 28, 28a for supplying a reducing gas to the heating belt 12, so that the dew point is maintained between an upper limit dew point at which the metal strip 3 has brightness and a lower limit dew point at which the SiO2 contained in the insulating material 17 is not reduced, and the metal strip 3 is bright annealed in a reducing atmosphere.
[0079] According to the above configuration, by maintaining the dew point (i.e., moisture content) of the atmosphere in the heating belt 12 between the upper limit dew point and the lower limit dew point, the moisture content in the reducing atmosphere is suitable for maintaining the brightness of the metal belt 3 and preventing the reduction of SiO2 contained in the heat insulating material 17. As a result, the metal belt 3 can have brightness and at the same time, the degradation of the heat insulating material 17 due to the reduction of SiO2 contained in the heat insulating material 17 can be prevented.
[0080] A heat treatment device 1 according to an embodiment of the present invention is a heat treatment device 1 for bright annealing a metal strip 3 in a reducing atmosphere, wherein the heat treatment device 1 comprises: a furnace body 10 having a heating belt 12 for heating the metal strip 3, and a cooling belt 14 arranged on the downstream side of the conveying direction of the metal strip 3 relative to the heating belt 12; a heat insulating material 17, which is used as the furnace inner wall of the heating belt 12 and is made of ceramic fiber containing SiO2; and a reducing agent is supplied into the furnace body 10. A gas supply unit 9, 28, 28a for gas; a dew point measuring unit 22 for measuring the dew point of the atmosphere in the heating belt 12; and a dew point adjusting unit 24, 24a, 27, 27a, 28, 28a for adjusting the dew point, wherein the dew point adjusting unit 24, 24a, 27, 27a, 28, 28a is controlled according to the dew point measured by the dew point measuring unit 22 so that the dew point is maintained between an upper limit dew point that can make the metal belt 3 bright and a lower limit dew point that will not reduce the SiO2 contained in the insulating material 17.
[0081] According to the above configuration, by maintaining the dew point (i.e., moisture content) of the atmosphere in the heating belt 12 between the upper limit dew point and the lower limit dew point, the moisture content in the reducing atmosphere is suitable for maintaining the brightness of the metal belt 3 and preventing the reduction of SiO2 contained in the heat insulating material 17. As a result, the metal belt 3 can have brightness and at the same time, the degradation of the heat insulating material 17 due to the reduction of SiO2 contained in the heat insulating material 17 can be prevented.
[0082] In the heat treatment apparatus 1 according to one embodiment, the dew point adjusting units 24 , 27 , and 28 are controlled by the control unit 20 .
[0083] According to the above-described embodiment, automation of bright annealing (heat treatment) can be achieved.
[0084] In the heat treatment apparatus 1 according to one embodiment, the upper limit dew point is -30°C.
[0085] According to the above-described embodiment, a metal strip 3 having brilliance can be obtained.
[0086] Furthermore, in the heat treatment apparatus 1 of one embodiment, the upper limit dew point is set within a range of -30°C to -65°C according to the degree of brightness of the metal strip 3 to be bright annealed.
[0087] According to the above-described embodiment, the metal strip 3 having desired brightness can be obtained.
[0088] Furthermore, in the heat treatment apparatus 1 according to one embodiment, the dew point adjustment unit 24 includes at least one of a dehumidifier 25 and a humidifier 26 .
[0089] According to the above-described embodiment, the dew point of the atmosphere in the heating zone 12 can be appropriately adjusted based on the dew point of the reducing gas supplied by the gas supply units 9 , 28 , 28 a and the dew point of the target atmosphere.
[0090] In addition, in one embodiment of the heat treatment device 1, the gas supply part 9, 28, 28a includes a gas supply device 9 and a regulating valve 28, 28a for regulating the flow rate of the reducing gas supplied by the gas supply device 9, and the gas supply device 9 and the regulating valve 28, 28a play the role of the dew point adjustment part 24, 24a.
[0091] According to the above-described embodiment, the dew point adjusting devices 24 and 24 a can be configured with a simple configuration.
[0092] In the heat treatment apparatus 1 according to one embodiment, the heat treatment apparatus 1 is a horizontal furnace in which the furnace body 10 extends in the lateral direction.
[0093] According to the above embodiment, the conveying mechanism for conveying the metal strip 3 can be simplified, and the height of the heat treatment device 1 can be suppressed from increasing. In addition, the disintegration of the ceramic fiber and the generation of dust can be prevented, so that the insulating material 17 made of lightweight ceramic fiber can be used even in a horizontal furnace with a large furnace top area.
[0094] Furthermore, in the heat treatment apparatus 1 according to one embodiment, the metal belt 3 is formed of a stainless steel material containing Cr.
[0095] According to the above-described embodiment, the formation of an oxide film in the metal strip 3 can be suppressed, and the metal strip 3 can be endowed with brightness.
[0096] In the heat treatment apparatus 1 according to one embodiment, the temperature range of the heating zone 12 is 800°C to 1250°C.
[0097] According to the above-described embodiment, the metal strip 3 can be heated at a temperature suitable for bright annealing.
[0098] Furthermore, in the heat treatment apparatus 1 according to one embodiment, the reducing gas includes hydrogen gas.
[0099] According to the above-described embodiment, the metal strip 3 may be reduced and bright annealed.
[0100] Explanation of symbols
[0101] 1...Bright annealing furnace (heat treatment device)
[0102] 3. Metal belt
[0103] 5...Gas supply pipeline
[0104] 6...Dew point measurement pipeline
[0105] 7...Inlet side pipe
[0106] 8...Outlet side pipe
[0107] 9... Gas supply device (gas supply unit, dew point adjustment unit)
[0108] 10……Furnace body
[0109] 12...Heating belt
[0110] 13...Inlet sealing roller
[0111] 14...Cooling belt
[0112] 15...Export sealing roller
[0113] 16...Heating unit
[0114] 17...Insulation materials
[0115] 20……Control Department
[0116] 22……Dew point measurement unit
[0117] 24...Dew point adjustment device (dew point adjustment unit)
[0118] 24a...Dew point adjustment device (dew point adjustment unit)
[0119] 25...Dehumidification device
[0120] 26...Humidifier
[0121] 27……First regulating valve (dew point adjustment unit)
[0122] 27a: First regulating valve (dew point adjusting unit)
[0123] 28... Second regulating valve (gas supply unit, dew point adjustment unit)
[0124] 28a... Second regulating valve (gas supply unit, dew point adjustment unit)
[0125] A……Straight line indicating the dew point of -30℃
[0126] C……Oxidation-reduction equilibrium curve of Cr2O3
[0127] S... Oxidation-reduction equilibrium curve of SiO2.
Claims
1. A heat treatment device, characterized in that: A heating zone for bright annealing a metal strip formed of a stainless steel material containing Cr in a reducing atmosphere, a heat insulating material made of ceramic fibers containing SiO2 and used as a furnace inner wall of the heating zone, a temperature control unit for controlling the heating temperature in the heating zone, a dew point measuring unit for measuring the dew point of the atmosphere in the heating zone, and a dew point adjusting unit for controlling the dew point of the atmosphere in the heating zone by dehumidification and humidification, In the diagram illustrating the relationship between the heating temperature and the atmosphere dew point, a range suitable for the bright annealing is defined. The range is surrounded by an upper temperature limit line indicating an upper limit bright annealing temperature, a lower temperature limit line indicating a lower limit bright annealing temperature, an upper dew point line corresponding to the oxidation-reduction equilibrium curve of Cr2O3 and capable of providing brightness, and a lower dew point line corresponding to the oxidation-reduction equilibrium curve of SiO2 and not causing reduction of SiO2. The temperature control unit and the dew point adjustment unit are respectively controlled so that the heating temperature and the atmosphere dew point are within the range.
2. The heat treatment device according to claim 1, characterized in that The dew point adjustment unit includes both a dehumidifier and a humidifier.
3. The heat treatment device according to claim 1 or 2, characterized in that: The dew point adjustment unit includes a gas supply device that supplies a reducing gas to the heating zone, and a regulating valve that is provided between the heating zone and the gas supply device and regulates a flow rate of the reducing gas.
4. The heat treatment device according to claim 1, characterized in that The upper limit dew point is set within a range of -30°C to -65°C depending on the degree of brightness of the metal strip to be bright annealed.
5. The heat treatment device according to claim 1, characterized in that The temperature range of the heating zone is 800°C to 1250°C.
6. The heat treatment device according to claim 1, characterized in that The ceramic fiber contains 40 to 70 mass % of the SiO2.