Molded article with decorative effect and method for preparing the same

By using a combination of high-content neutralizing acid copolymers with polyamide and liquid-based pigments in molded products, the problem of difficult to achieve marble-type decorative effects in the prior art is solved, and the ideal visual effect and mold of molded products are achieved automation of the manufacturing process.

CN114787267BActive Publication Date: 2024-12-06DOW GLOBAL TECHNOLOGIES LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080048916.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-02
Filing Date
2020-06-30
Publication Date
2024-12-06
Estimated Expiration
2040-06-30

AI Technical Summary

Technical Problem

The prior art is difficult to achieve ideal decorative effects in molded products, especially marble-type or natural weathered metal patterns, and the addition of additional components complicates the material properties while maintaining automation and reproducibility of the molding process. Visual effects.

Method used

Injection molding is performed using at least 75% neutralizing acid copolymer combined with 0.1% to 5% polyamide-based pigment masterbatch and 0.1% to 5% liquid-based pigment masterbatch to form a molded product by poly The interaction of amide and liquid-based pigment masterbatch produces decorative effects such as marble textures and metallic background colors.

Benefits of technology

A uniform and opaque decorative effect in molded products is achieved, similar to color stripes of natural stone or metal, enhancing visual value while maintaining the effectiveness and automation of the molding process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003441992270000191
    Figure BDA0003441992270000191
Patent Text Reader

Abstract

The molded article with decorative effect comprises at least 75% by weight of a neutralized acid copolymer. The molded article comprises 0.1% to 5% by weight of a polyamide-based pigment masterbatch. The polyamide-based pigment masterbatch comprises 30% to 95% by weight of a polyamide and 5% to 70% by weight of a first pigment associated with the polyamide. The molded article also comprises 0.1% to 5% by weight of a second pigment derived from a liquid-based pigment masterbatch; and 0.1% to 0.7% by weight of an oil-based carrier derived from the liquid-based pigment masterbatch. The method for preparing the molded article comprises dry mixing the neutralized acid copolymer, the polyamide-based pigment masterbatch and the liquid-based pigment masterbatch to form an initial mixture; feeding the initial mixture to an injection molding device; and molding the initial mixture with the injection molding device to form the molded article.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to U.S. Provisional Patent Application No. 62 / 869,771, filed on July 2, 2019, the entire disclosure of which is hereby incorporated by reference herein. Technical Field

[0003] The present disclosure relates generally to molded articles, and more particularly, to molded articles having decorative effects. Background Art

[0004] Neutralized acid copolymers (e.g., ionomer resins) are materials with highly desirable properties for use in molded articles, including, but not limited to, cosmetic containers and perfume bottles. In particular, neutralized acid copolymers are well suited for the type of injection molding processes used to form such articles. The ability to decorate such molded articles or to create unusual or dramatic visual effects with molded articles is of high value to consumer product manufacturers and the consumers themselves.

[0005] For example, the ability to form a molded article from a molding process (e.g., injection molding) often relies on a variety of properties of the material being molded. While the particular material being molded may be well suited to the molding process in its original form, the addition of ingredients, such as pigments, to produce a desired visual effect may alter the properties of the molded material in a manner that significantly complicates the molding process. Conversely, artistic desires for a certain visual effect may be hampered by the inability of the molding process to incorporate the additional ingredients required to achieve such an effect.

[0006] One particular, highly desirable visual effect for molded articles includes decorative patterns, including color stripes that simulate patterns in stone (e.g., marble) or naturally weathered or tarnished metals. Although a limited degree of marble-type effects have been achieved in neutralized acid copolymer molded articles by incorporating colored polyamides into blends of the copolymers, the effects have been limited to striped patterns in an otherwise transparent or translucent copolymer matrix. There remains a continuing need for additional types of decorative effects in molded articles prepared from neutralized acid copolymer materials, as well as a continuing need for methods of preparing molded articles in a manner that incorporates additional ingredients while maintaining efficient reproducibility and automation of large-scale molding processes. Summary of the invention

[0007] Against the above background, embodiments of the present disclosure relate to molded articles with decorative effects. The molded article comprises at least 75% by weight of a neutralized acid copolymer based on the total weight of the molded article. The molded article also comprises 0.1% to 5% by weight of a polyamide-based pigment masterbatch based on the total weight of the molded article. The polyamide-based pigment masterbatch comprises 30% to 95% by weight of polyamide based on the total weight of the polyamide-based pigment masterbatch, and 5% to 70% by weight of a first pigment associated with polyamide based on the total weight of the polyamide-based pigment masterbatch. The molded article also comprises 0.1% to 5% by weight of a second pigment derived from a liquid-based pigment masterbatch based on the total weight of the molded article; and 0.1% to 0.7% by weight of an oil-based carrier derived from the liquid-based pigment masterbatch based on the total weight of the molded article.

[0008] Additional embodiments of the present disclosure relate to methods for preparing molded articles and molded articles prepared by the methods. The method includes dry mixing a neutralized acid copolymer, a polyamide-based pigment masterbatch, and a liquid-based pigment masterbatch to form an initial mixture; feeding the initial mixture to an injection molding device; and injection molding the initial mixture with the injection molding device to form a molded article. The initial mixture contains at least 75 weight percent of the neutralized acid copolymer based on the total weight of the initial mixture; 0.1 weight percent to 5 weight percent of the polyamide-based pigment masterbatch; and 0.2 weight percent to 5.7 weight percent of the liquid-based pigment masterbatch. The polyamide-based pigment masterbatch may contain 30 weight percent to 95 weight percent of polyamide based on the total weight of the polyamide-based pigment masterbatch, and 5 weight percent to 70 weight percent of a first pigment associated with the polyamide based on the total weight of the polyamide-based pigment masterbatch. The liquid-based pigment masterbatch may include 5 to 60 wt % of the second pigment based on the total weight of the liquid-based pigment masterbatch, and 40 to 95 wt % of the oil-based carrier based on the total weight of the liquid-based pigment masterbatch.

[0009] These and other features, aspects and advantages of the present invention will become better understood with reference to the following description and appended claims.

[0010] Additional features and advantages of the embodiments described herein will be set forth in the detailed description that follows, and in part will be readily apparent to those skilled in the art from that description or recognized by practicing the embodiments described herein, including the detailed description that follows, the claims, and the accompanying drawings.

[0011] It should be understood that both the foregoing overall description and the following detailed description describe various embodiments and are intended to provide an overview or framework for understanding the nature and character of the claimed subject matter. The accompanying drawings are included to provide a further understanding of the various embodiments, and are incorporated into and constitute a part of this specification. DETAILED DESCRIPTION

[0012] Reference will now be made in detail to an embodiment of a molded article having a decorative effect. A method for preparing the molded article will then be described.

[0013] According to the molded article of the embodiment, at least 75% by weight of the neutralized acid copolymer can be included according to the total weight of the molded article. The molded article also includes 0.1% by weight to 5% by weight of a polyamide-based pigment masterbatch according to the total weight of the molded article. The polyamide-based pigment masterbatch can include 30% by weight to 95% by weight of polyamide according to the total weight of the polyamide-based pigment masterbatch, and 5% by weight to 70% by weight of the first pigment associated with the polyamide according to the total weight of the polyamide-based pigment masterbatch. In some embodiments, the polyamide is nylon, such as nylon 6. The molded article can also include 0.1% by weight to 5% by weight of a second pigment derived from a liquid-based pigment masterbatch according to the total weight of the molded article; and 0.1% by weight to 0.7% by weight of an oil-based carrier derived from a liquid-based pigment masterbatch according to the total weight of the molded article.

[0014] The molded article according to the embodiment shows a decorative effect, which is produced by the interaction of the components of the molded article during the molding process (e.g., extrusion or injection molding). For example, the neutralized acid copolymer without any additional components can be a substantially optically transparent or transparent material. The first pigment associated with the pigment masterbatch formula based on polyamide can impart uneven color stripes through the volume of the molded article. The second pigment based on the liquid-based pigment masterbatch can impart substantially uniform coloring to the entire molded article volume. Therefore, the decorative effect in the article can include a marble pattern of stripes from the first pigment on a blank tray of uniform color from the second pigment. The uniform blank tray produced by the second pigment can make the neutralized acid polymer, which is originally substantially transparent or transparent, translucent or substantially opaque. If the neutralized acid polymer is substantially opaque to the second pigment, the color stripes from the first pigment may be similar to the color stripe pattern naturally present in decorative stone or metal objects.

[0015] The decorative effect in the molded article may be caused by the phase morphology of the components of the molded article. For example, in the molded article, the neutralized acid copolymer can be a continuous phase in the molded article. In the same molded article, a polyamide-based pigment masterbatch comprising a first pigment and a related polyamide (e.g., nylon 6) can exist as the first secondary phase in the molded article. The first secondary phase is not evenly distributed in the continuous phase. In the same molded article, a second pigment derived from a liquid-based pigment masterbatch can exist as a second secondary phase in the molded article. The second secondary phase may or may not be evenly distributed in the continuous phase. In the same molded article, an oil-based carrier can exist as a third secondary phase in the molded article. The third secondary phase may or may not be evenly distributed in the continuous phase. In some embodiments, the first secondary phase is not evenly distributed in the continuous phase, and one or both of the second secondary phase and the third secondary phase are evenly distributed in the continuous phase.

[0016] Examples of decorative effects of molded articles according to embodiments may include, but are not limited to, graystone effects, white marble with brown stripes, black marble with white stripes, oxidized metal finishes, old brass, earthy copper, onyx finishes, and obsidian finishes. Depending on the desired decorative effect, such as graystone, white light brown marble, or oxidized metal, a background color or blank canvas and a stripe color can be selected, and then a suitable pigment can be selected to prepare a formula or initial mixture to be molded. For example, for graystone or white marble, a white liquid pigment can be used as a background, and a black or light brown solid color concentrate based on polyamide (e.g., nylon 6) can be used for stripes. For onyx or obsidian finishes, the background color can be obtained by a black liquid pigment and a white solid color concentrate based on polyamide (e.g., nylon 6) for stripes. For metal finishes, copper or silver liquid pigments can be added to obtain a metallic background color, and a combination of black and light brown solid color concentrates based on polyamide (e.g., nylon 6) can be used for stripes.

[0017] According to an embodiment, the neutralized acid copolymer of the molded article can be an ionomer resin. In some embodiments, the neutralized acid copolymer can be a neutralized ethylene acid copolymer. The molded article can contain at least 75 weight %, or at least 80 weight %, or at least 85 weight %, or at least 90 weight %, or at least 95 weight % of the neutralized acid copolymer based on the total weight of the molded article.

[0018] Ionomer resins can be produced by any means known to those skilled in the art, such as by neutralizing ethylene acid copolymers with one or more metal ions. Ethylene acid copolymers are polymers comprising repeating units derived from ethylene and about 1 wt % to about 50 wt %, or about 5 wt % to about 40 wt %, or 10 wt % to 25 wt % of a comonomer, such as acrylic acid, methacrylic acid, ethacrylic acid, or a combination of two or more thereof, based on the total weight of the ethylene copolymer. Ionomer resins are generally well known to those skilled in the art.

[0019] Examples of ethylene acid copolymers can include up to 35 weight percent of optional comonomers such as carbon monoxide, sulfur dioxide, acrylonitrile, maleic anhydride, maleic acid diesters, maleic acid, maleic acid monoesters, itaconic acid, fumaric acid, fumaric acid monoesters, salts of these acids, glycidyl acrylate, glycidyl methacrylate and glycidyl vinyl ether, methyl acrylate, ethyl acrylate, isopropyl acrylate, butyl acrylate, amyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate and butyl methacrylate, amyl methacrylate or a combination of two or more thereof, wherein the alkyl group can be linear or branched.

[0020] The acid groups of the ionomer resin are at least partially neutralized. According to the total carboxylic acid content, the neutralization of the acid groups in the ionomer resin can be, for example, in the range of about 0.1% to about 100%, or about 10% to about 90%, or about 20% to about 80%, or about 30% to about 60%, or about 20% to about 40% of the carboxylic acid groups in the ionomer resin neutralized with the metal ion. The metal ion can be monovalent, divalent, trivalent, polyvalent or a combination of two or more thereof. Examples include Li, Na, K, Ag, Hg, Cu, Be, Mg, Ca, Sr, Ba, Cd, Sn, Pb, Fe, Co, Zn, Ni, Al, Sc, Hf, Ti, Zr, Ce and a combination of two or more thereof. If the metal ion is polyvalent, a complexing agent can be included, such as stearate, oleate, salicylate and phenolate groups, as disclosed in U.S. Patent No. 3,404,134. Specific examples of neutralizing metal ions include Na, Zn, or combinations thereof. Additional examples include sodium or zinc ions derived from salts such as NaOH, NaHCO 3 、Na 2 CO 3 、NaHSO 4 、NaH 2 PO 4 、Na 2 HPO 3 , sodium stearate, sodium oleate, sodium salicylate, sodium phenol, Zn(OH) 2 、ZnCO 3 、ZnCO 3、ZnSO 4 、ZnHPO 4 、ZnHPO 3 , zinc oxide, zinc stearate, zinc oleate, zinc salicylate, zinc phenolate, Mg(OH) 2 MgCO 3 MgCO 3 MgSO 4 MgHPO 4 MgHPO 3 , magnesium stearate, magnesium oleate, magnesium salicylate, magnesium phenolate or a combination of two or more thereof.

[0021] In an embodiment, the neutralized acid copolymer of the molded article can be an ionomer resin having a melt flow index of 4 g / 10 min to 6 g / 10 min measured according to ASTM D1238. In an embodiment, the neutralized acid copolymer of the molded article can be an ethylene methacrylic acid copolymer, wherein the methacrylic acid groups of the copolymer are at least partially neutralized by sodium ions. In an embodiment, the neutralized acid copolymer of the molded article can include 15 wt % to 30 wt % or 15 wt % to 20 wt % of acrylic acid or methacrylic acid copolymerized units, and 70 wt % to 85 wt % of ethylene copolymerized units, based on the total weight of the neutralized acid copolymer. In an embodiment, the neutralized acid copolymer of the molded article can have about 30% to about 70%, or 30% to 60%, or 40% to 70% of the carboxylic acid groups of the neutralized acid copolymer neutralized to a carboxylate salt containing sodium cations.

[0022] In an embodiment, the neutralized acid copolymer can be an ionomer formed from a partially neutralized precursor acid copolymer. The precursor acid copolymer can include copolymerized units of ethylene and copolymerized units of α,β-ethylenically unsaturated carboxylic acids having 3 to 8 carbon atoms from 5 wt % to 30 wt % based on the total weight of the precursor acid copolymer. All individual values ​​and subranges from 5 wt % to 30 wt % are included and disclosed herein. For example, in some embodiments, the precursor acid copolymer includes copolymerized units of ethylene and copolymerized units of α,β-ethylenically unsaturated carboxylic acids having 3 to 8 carbon atoms from 5 wt % to 25 wt %, 7 wt % to 25 wt %, or 7 wt % to 22 wt % based on the total weight % of the precursor acid copolymer. The comonomer content can be measured using any suitable technique, such as techniques based on nuclear magnetic resonance ("NMR") spectroscopy, and for example by methods as described in U.S. Pat. No. 7,498,282 13 C NMR analysis, which is incorporated herein by reference.

[0023] Examples of suitable α,β-unsaturated carboxylic acids having 3 to 8 carbon atoms may include, but are not limited to, acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, monomethyl maleic acid, and combinations of two or more of these acid comonomers. In some embodiments, the α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms comprises acrylic acid and methacrylic acid. In other embodiments, the α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms comprises acrylic acid.

[0024] The melt index I2 of the partially neutralized precursor acid copolymer is 10 g / 10 min to 4,000 g / 10 min. The melt index I2 is determined according to ASTM D1238 at 190 ° C, 2.16 kg. All individual values ​​and subranges of 10 g / 10 min to 4,000 g / 10 min are included and disclosed herein. For example, in some embodiments, the melt index I2 of the precursor acid copolymer may be 10 g / 10 min to 2,500 g / 10 min, 10 g / 10 min to 1,250 g / 10 min, 25 g / 10 min to 1,000 g / 10 min, 25 g / 10 min to 750 g / 10 min, 50 g / 10 min to 500 g / 10 min, or 100 g / 10 min to 450 g / 10 min.

[0025] The partially neutralized precursor acid copolymer can be synthesized in a continuous process, wherein each reactive comonomer and one or more solvents (if present) are continuously fed into a stirred reactor together with an initiator. The selection of the initiator is based on the expected reactor temperature range and the decomposition temperature of the initiator, and this selection criteria is well known in the industry. Generally speaking, during the synthesis of the precursor acid copolymer by copolymerization of ethylene and acid comonomers, the reaction temperature can be maintained at about 120°C to about 300°C or about 140°C to about 260°C. The pressure in the reactor can be maintained at about 130MPa to about 310MPa or about 165MPa to 250MPa.

[0026] The reactor may be, for example, an autoclave reactor, such as those described in U.S. Patent No. 2,897,183, which describes an autoclave reactor equipped with a device for intense stirring. U.S. Patent No. 2,897,183 also describes a continuous process for carrying out ethylene polymerization under a "substantially constant environment". This environment is maintained by maintaining certain parameters (e.g., pressure, temperature, initiator concentration, and the ratio of polymer product to unreacted ethylene) substantially constant during the polymerization reaction. Such conditions can be achieved in any of a variety of continuously stirred tank reactors, such as a continuously stirred isothermal reactor and a continuously stirred adiabatic reactor.

[0027] The reaction mixture containing the precursor acid copolymer is vigorously stirred and continuously removed from the autoclave. After the reaction mixture leaves the reaction vessel, the resulting precursor acid copolymer product is separated from volatile unreacted monomers and solvent (if present) by conventional procedures, such as by evaporating the unpolymerized material and solvent under reduced pressure or at elevated temperature. Non-limiting examples of precursor acid copolymers include those available from Dow Chemical Company under the trade name NUCREL TM of copolymers.

[0028] Generally, in order to obtain the neutralized acid copolymer as the ionomer formed by the partially neutralized precursor acid copolymer, during the polymerization reaction, the reactor contents can be maintained under the condition that a single phase is substantially present in the whole reactor. This can be achieved by adjusting the reactor temperature, by adjusting the reactor pressure, by adding a cosolvent or by any combination of these technologies, as described in U.S. Patent No. 5,028,674. Conventional means can be used to determine whether a single phase is substantially maintained in the whole reactor. For example, Hasch et al., "High-Pressure Phase Behavior of Mixtures of Poly(Ethylene-co-Methyl Acrylate) with Low-Molecular Weight Hydrocarbons", Journal of Polymer Science: Part B: Polymer Physics, Vol. 30, 1365-1373 (1992) describe the cloud point measurement that can be used to determine the boundary between single-phase and multiphase conditions.

[0029] In order to obtain an ionomer for use as a neutralized acid copolymer in a molded article according to an embodiment of the present disclosure, the precursor acid copolymer is neutralized with a base containing a metal cation so that the acid groups (e.g., carboxylic acid) in the precursor acid copolymer react to form acid salt groups (e.g., carboxylates). In embodiments herein, about 25% to about 65%, or about 30% to about 60%, or about 35% to about 60%, or about 30% to about 55%, or about 35% to about 55% of the acid groups of the α,β-ethylenically unsaturated carboxylic acid derived from the precursor acid copolymer are neutralized. The neutralization level of the acid groups of the α,β-ethylenically unsaturated carboxylic acid derived from the precursor acid copolymer can be calculated based on the amount of basic metal compound added or measured using infrared spectroscopy. The actual neutralization level can be measured using infrared spectroscopy by comparing the concentration of the acid groups at 1530 cm -1 Up to 1630cm -1The absorption peaks at 1690 cm-1 can be attributed to the stretching vibration of the carboxylate anion and -1 To 1710cm -1 The amount of basic metal compound capable of neutralizing the acidic groups can be provided by adding a stoichiometric amount of basic compound calculated to neutralize the target amount of acid moieties in the acid copolymer. Non-limiting examples of ionomers include those available from The Dow Chemical Company under the trade name SURLYN TM of ionomers.

[0030] It is believed that any stable cation and any combination of two or more stable cations are suitable as counter ions of acid groups in ionomers. Counter ions of acid groups in ionomers can include, for example, divalent and monovalent cations, such as cations of alkali metals, alkaline earth metals, and some transition metals. For example, in some embodiments, the cation is a divalent cation (such as zinc, calcium or magnesium). For example, in other embodiments, the cation is a monovalent cation (such as potassium or sodium). In other embodiments, the acid groups of α,β-ethylenically unsaturated carboxylic acids derived from precursor acid copolymers are neutralized by a base containing sodium ions. The base containing sodium ions can provide a sodium ionomer, in which the hydrogen atoms of the acid groups of the precursor acid are replaced by sodium cations. In order to obtain an ionomer used as a neutralized acid copolymer in an embodiment, the precursor acid copolymer can be neutralized by any conventional procedure, such as those described in U.S. Patents Nos. 3,404,134 and 6,518,365.

[0031] According to an embodiment, the molded article comprises 0.1 wt % to 5 wt %, or 0.1 wt % to 2 wt %, or 0.1 wt % to 1 wt %, or 0.1 wt % to 0.7 wt % of a pigment masterbatch based on polyamide, based on the total weight of the molded article. The pigment masterbatch based on polyamide comprises polyamide and a first pigment associated with polyamide. In an example embodiment, the pigment masterbatch based on polyamide may comprise 30 wt % to 95 wt % of polyamide based on the total weight of the pigment masterbatch based on polyamide, and 5 wt % to 70 wt % of the first pigment associated with polyamide based on the total weight of the pigment masterbatch based on polyamide. In some embodiments, the molded article may comprise a plurality of pigment masterbatches based on polyamide. In such embodiments, the molded article comprises 0.1 wt % to 5 wt %, or 0.1 wt % to 2 wt %, or 0.1 wt % to 1 wt %, or 0.1 wt % to 0.7 wt % of all pigment masterbatches based on polyamide, based on the total weight of the molded article.

[0032] In molded articles, a pigment masterbatch based on polyamide can form a first secondary phase in a continuous phase of a neutralized acid copolymer. For example, the first secondary phase can be distributed in the volume of the neutralized acid copolymer in a pattern similar to spots or stripes. In this regard, the association of the first pigment with the polyamide itself can be manifested in the molded article because the first pigment is retained in the first secondary phase and will not leach or leak to impart color to the continuous phase of the neutralized acid copolymer while being separated or separated from the polyamide matrix that constitutes the first secondary phase. The association of the first pigment with the polyamide can include chemical bonding between the molecules of the first pigment and the polyamide, which can be detected and verified by known analytical techniques.

[0033] Pigment masterbatches based on polyamide are well known to those skilled in the art of molded plastics. Pigment masterbatches based on polyamide can generally be pigment molecules uniformly dispersed in a polyamide matrix. For example, pigment masterbatches based on polyamide are obtained in bulk form (e.g., pellets). For example, pellets can be added to the neutralized acid copolymer in bulk form to prepare for a molding process, such as extrusion or injection molding.

[0034] Examples of the polyamide component of the polyamide-based pigment masterbatch include homopolyamides, copolyamides, polyamides or mixtures or blends of polyamides with another polymer. Exemplary homopolyamides and copolyamides include ω-aminocaproic acid, ω-aminoheptanoic acid, ω-aminooctanoic acid, ω-aminononanoic acid, ω-aminodecanoic acid, ω-aminoundecanoic acid, a)-aminolauric acid, caprolactam, lactam-7, lactam-8, lactam-9, lactam-10, lactam-11 and / or laurolactam. The polyamide can be selected from the group of polyamides made, for example, from dimethylenediamine, trimethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, polyetherdiamines and mixtures thereof on the one hand; and oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, non-dicarboxylic acids, sebacic acid, undecanedioic acid, dodecanedioic acid, dimerized fatty acids and mixtures thereof on the other hand. Specific examples of polyamides include nylons, such as nylon 6.

[0035] In some embodiments, the polyamide of the polyamide-based pigment masterbatch may have a Vicat softening point that is lower than the temperature at which the neutralized acid copolymer is fully plasticized after a molding process (e.g., extrusion or injection molding). Without being bound by theory, it is believed that this relationship of temperature may affect the manner in which the polyamide-based pigment masterbatch forms streaks within the volume of the neutralized acid copolymer.

[0036] The polyamide-based pigment masterbatch of the molded article can be any polyamide-based pigment masterbatch prepared by known methods, the method comprising melt blending a polyamide with one or more suitable dyes or pigments used together as the first pigment of the molded article. Any type of dye or pigment is suitable, provided that it is stable at the high temperatures encountered during the molding process.

[0037] Example dyes include monoazo complexes, especially chromium complexes that are sufficiently stable at the high operating temperatures encountered during molding. Additional examples of dyes include halogen-containing triazine-based or vinyl-containing metallated azo dyes, especially those metallated with chromium, nickel or copper.

[0038] Further examples of pigments suitable for polyamide-based pigment masterbatches for molded articles according to embodiments include carbon black, aniline black; metal-based pigments, such as cadmium pigments (yellow, red, green, orange); chromium pigments (yellow, green); cobalt pigments (violet, blue, sky blue, yellow); copper pigments (copper blue, violet, blue, green, phthalocyanine blue, phthalocyanine green), iron oxide pigments (red oxide, ochre, Prussian blue); lead pigments (lead white, yellow, red, lead tin yellow); manganese pigments (violet, blue); mercury pigments (vermilion); titanium pigments (yellow, beige, white, black); zinc pigments (white, ferrite, yellow) and aluminum powder. Still further examples of pigments suitable for use in polyamide-based pigment masterbatches for molded articles according to embodiments include inorganic pigments such as carbon black (including rattan black, lamp black), ivory black (bone charcoal); clay pigments (iron oxide, yellow ochre, raw ochre, burnt sienna, raw umber, burnt umber); ultramarine pigments and those from biological and non-biological sources such as alizarin (synthetic), alizarin crimson (synthetic), gamboge, cochineal, rose madder, indigo, Indian yellow, Tyrian purple, quinacridone, fuchsin, phthalocyanine green, phthalocyanine blue, pigment red 170, and diarylide yellow.

[0039] Further examples of pigments suitable for the polyamide-based pigment masterbatch of the molded article according to the embodiment include organic or inorganic pigments such as perylene, perinone, quinacridone, quinacridonequinone, anthraquinone, anthrone, benzimidazolone, diazo condensation compounds, azo compounds, indanthrone, phthalocyanine, triarylcarbonium, dioxazine, triphenodioxazine, aminoanthraquinone, diketopyrrolopyrrole, indigo, thioindigo, Indigo blue, thiazine indigo, isoindoline, isoindolinone, pyranthrone, isoviranthrone, flavonanthrone, anthrapyridine or carbon black pigment, mixed crystal or mixture thereof; or inorganic pigment, such as titanium dioxide, zinc sulfide, zinc oxide, iron oxide, chromium oxide, mixed metal oxide (such as nickel rutile yellow, chrome rutile yellow, cobalt blue, cobalt green, zinc iron brown, spinel black), cadmium, bismuth, chromate, ultramarine and iron blue pigment and mixture thereof, and mixture of organic and inorganic pigment. Other examples of the first pigment of the polyamide-based pigment masterbatch suitable for the molded article according to the embodiment include carbon black, pigment yellow 192, pigment orange 68 and pigment red 149.

[0040] According to an embodiment, in addition to the first pigment associated with the polyamide of the polyamide-based pigment masterbatch, the molded article also includes a second pigment and an oil-based carrier. The second pigment and the oil-based carrier are both derived from a liquid-based pigment masterbatch. In contrast to the first pigment that remains associated with the polyamide of the polyamide-based pigment masterbatch formulation, the second pigment and the oil-based carrier do not have to be associated with each other in the molded article. In an embodiment, the second pigment can be present in the molded article as a second secondary phase, and the oil-based carrier can be present in the molded article as a third secondary phase separated from the second phase. The second pigment and the oil-based carrier are derived from the liquid-based pigment masterbatch because when the molded article is produced, the liquid-based pigment masterbatch is added to the original neutralized acid copolymer before the molding process. During the molding process, the second pigment is dispersed throughout the copolymer material to impart a coloring effect to the entire copolymer. Nevertheless, the oil-based carrier remains in the molded article as a detectable artifact of the means of adding the second pigment, i.e., the liquid-based pigment masterbatch.

[0041] According to the molded article of the embodiment, 0.1 wt % to 5 wt %, or 0.5 wt % to 4 wt %, or 0.5 wt % to 3 wt %, or 0.5 wt % to 2.5 wt % of the second pigment derived from the liquid-based pigment masterbatch can be included by the total weight of the molded article; and 0.1 wt % to 0.7 wt %, or 0.1 wt % to 0.5 wt %, or 0.1 wt % to 0.3 wt %, or 0.1 wt % to 0.2 wt %, or 0.05 wt % to 0.2 wt % of the oil-based carrier derived from the liquid-based pigment masterbatch can be included by the total weight of the molded article. In some embodiments, the molded article can include a plurality of second pigments and oil-based carriers, each of which is derived from a separate liquid-based colorant. In such embodiments, the aforementioned weight percentages describing the second pigments and oil-based carriers in the molded article refer to the combined total weight of all second pigments and oil-based carriers in the molded article.

[0042] The liquid-based pigment masterbatch from which the second pigment and the oil-based carrier of the molded article are derived must contain the second pigment and the oil-based carrier. The liquid-based pigment masterbatch can be a colorant formulation in any liquid form that is chemically compatible with the neutralized acid copolymer and that is stable at typical temperatures of the extrusion or injection molding process. The second pigment can be any pigment that is chemically compatible with the neutralized acid copolymer and stable at typical temperatures of the extrusion or injection molding process. The oil-based carrier can be any non-polar liquid in which the second pigment is substantially soluble.

[0043] Examples of pigments suitable as the second pigment of the molded article include, but are not limited to, organic or inorganic pigments. Such organic or inorganic pigments may be selected from black pigments, yellow pigments, magenta pigments, red pigments, purple pigments, cyan pigments, blue pigments, green pigments, orange pigments, brown pigments, and white pigments. In some cases, the organic or inorganic pigments may include spot color pigments, which are formed by a combination of two or more primary color pigments in a predetermined ratio.

[0044] Non-limiting examples of suitable inorganic black pigments include carbon black. Examples of carbon black pigments include those manufactured by Mitsubishi Chemical Corporation, Japan (e.g., Carbon Black No. 2300, No. 900, MCF88, No. 33, No. 40, No. 45, No. 52, MA7, MA8, MA100, and No. 2200B); A series of various carbon black pigments (e.g. 5750, 5250, 5000, 3500, 1255 and 700); manufactured by Cabot Corporation, Boston, Mass. series, Series or A series of various carbon black pigments (e.g. 400R, 330R, 660R, L. 700, 800, 880, 900, 1000, 1100, 1300 and 1400); and various black pigments manufactured by Evonik Degussa Corporation, Parsippany, NJ (e.g., Color Black FW1, Color Black FW2, Color Black FW2V, Color Black FW18, Color Black FW200, Color Black S150, Color Black S160, Color Black S170, 35. U. V. Non-limiting examples of organic black pigments include aniline black, such as CI Pigment Black 1.

[0045] Non-limiting examples of suitable yellow pigments include CI Pigment Yellow 1, CI Pigment Yellow 2, CI Pigment Yellow 3, CI Pigment Yellow 4, CI Pigment Yellow 5, CI Pigment Yellow 6, CI Pigment Yellow 7, CI Pigment Yellow 10, CI Pigment Yellow 11, CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Yellow 14, CI Pigment Yellow 16, CI Pigment Yellow 17, CI Pigment Yellow 24, CI Pigment Yellow 34, CI Pigment Yellow 35, CI Pigment Yellow 37, CI Pigment Yellow 53, CI Pigment Yellow 55, CI Pigment Yellow 65, CI Pigment Yellow 73, CI Pigment Yellow 74, CI Pigment Yellow 75, CI Pigment Yellow 81, CI Pigment Yellow 83, CI Pigment Yellow 93, CI Pigment Yellow 94, CI Pigment Yellow 95, CI Pigment Yellow 100, CI Pigment Yellow 101, CI Pigment Yellow 102, CI Pigment Yellow 103, CI Pigment Yellow 104, CI Pigment Yellow 105, CI Pigment Yellow 106, CI Pigment Yellow 107, CI Pigment Yellow 108, CI Pigment Yellow 109, CI Pigment Yellow 110 CI Pigment Yellow 94, CI Pigment Yellow 95, CI Pigment Yellow 97, CI Pigment Yellow 98, CI Pigment Yellow 99, CI Pigment Yellow 108, CI Pigment Yellow 109, CI Pigment Yellow 110, CI Pigment Yellow 113, CI Pigment Yellow 114, CI Pigment Yellow 117, CI Pigment Yellow 120, CI Pigment Yellow 124, CI Pigment Yellow 128, CI Pigment Yellow 129, CI Pigment Yellow 133, CI Pigment Yellow 138, CI Pigment Yellow 139, CI Pigment Yellow 147, CI Pigment Yellow 151, CI Pigment Yellow 153, CI Pigment Yellow 154, Pigment Yellow 155, CI Pigment Yellow 167, CI Pigment Yellow 172, and CI Pigment Yellow 180.

[0046] Non-limiting examples of suitable magenta or red or violet organic pigments include CI Pigment Red 1, CI Pigment Red 2, CI Pigment Red 3, CI Pigment Red 4, CI Pigment Red 5, CI Pigment Red 6, CI Pigment Red 7, CI Pigment Red 8, CI Pigment Red 9, CI Pigment Red 10, CI Pigment Red 11, CI Pigment Red 12, CI Pigment Red 14, CI Pigment Red 15, CI Pigment Red 16, CI Pigment Red 17, CI Pigment Red 18, CI Pigment Red 19, CI Pigment Red 21, CI Pigment Red 22, CI Pigment Red 23, CI Pigment Red 30, CI Pigment Red 31, CI Pigment Red 32, CI Pigment Red 37, CI Pigment Red 38, CI Pigment Red 40, CI Pigment Red 41, CI Pigment Red 42, CI Pigment Red 48 (Ca), CI Pigment Red 48 (Mn), CI Pigment Red 57 (Ca), CI Pigment Red 57 ... CI Pigment Red 88, CI Pigment Red 112, CI Pigment Red 114, CI Pigment Red 122, CI Pigment Red 123, CI Pigment Red 144, CI Pigment Red 146, CI Pigment Red 149, CI Pigment Red 150, CI Pigment Red 166, CI Pigment Red 168, CI Pigment Red 170, CI Pigment Red 171, CI Pigment Red 175, CI Pigment Red 176, CI Pigment Red 177, CI Pigment Red 178, CI Pigment Red 179, CI Pigment Red 184, CI Pigment Red 185, CI Pigment Red 187, CI Pigment Red 202, CI Pigment Red 209, CI Pigment Red 219, CI Pigment Red 224, CI Pigment Red 245, CI Pigment Violet 19, CI Pigment Violet 23, CI Pigment Violet 32, CI Pigment Violet 33, CI Pigment Violet 36, CI Pigment Violet 38, CI Pigment Violet 43, and CI Pigment Violet 50.

[0047] Non-limiting examples of blue or cyan organic pigments include CI Pigment Blue 1, CI Pigment Blue 2, CI Pigment Blue 3, CI Pigment Blue 15, CI Pigment Blue 15:3, CI Pigment Blue 15:34, CI Pigment Blue 15:4, CI Pigment Blue 16, CI Pigment Blue 18, CI Pigment Blue 22, CI Pigment Blue 25, CI Pigment Blue 60, CI Pigment Blue 65, CI Pigment Blue 66, CI Vat Blue 4, CI Vat Blue 60.

[0048] Non-limiting examples of green organic pigments include CI Pigment Green 1, CI Pigment Green 2, CI Pigment Green 4, CI Pigment Green 7, CI Pigment Green 8, CI Pigment Green 10, CI Pigment Green 36, and CI Pigment Green 45.

[0049] Non-limiting examples of brown organic pigments include CI Pigment Brown 1, CI Pigment Brown 5, CI Pigment Brown 22, CI Pigment Brown 23, CI Pigment Brown 25, CI Pigment Brown, CI Pigment Brown 41, and CI Pigment Brown 42.

[0050] Non-limiting examples of orange organic pigments include CI Pigment Orange 1, CI Pigment Orange 2, CI Pigment Orange 5, CI Pigment Orange 7, CI Pigment Orange 13, CI Pigment Orange 15, CI Pigment Orange 16, CI Pigment Orange 17, CI Pigment Orange 19, CI Pigment Orange 24, CI Pigment Orange 34, CI Pigment Orange 36, CI Pigment Orange 38, CI Pigment Orange 40, CI Pigment Orange 43, and CI Pigment Orange 66.

[0051] Organic pigments suitable as the second pigment may include, for example, azo compounds, azomethines, methenamines, anthraquinones, phthalocyanines, perylenes, perylenes, diketopyrrolopyrroles, thioindigos, iminoisoindolines, dioxazines, iminoisoindolones, quinacridones, flavones, indanthrone, anthrapyridines and quinophthalone pigments, or mixtures or solutions thereof.

[0052] Suitable inorganic pigments for the second pigment of the molded article according to the embodiment may include, for example, carbon black, metal oxides, mixed metal oxides, antimony yellow, lead chromate, lead chromate sulfate, lead molybdate, ultramarine blue, cobalt blue, manganese blue, chromium oxide green, hydrated chromium oxide green, cobalt green, metal sulfides, cadmium selenide sulfide, zinc ferrite and bismuth vanadate, or mixtures thereof.

[0053] The oil-based carrier of liquid-based pigment masterbatch can be any fluid carrier compatible with the second pigment chemistry.The example of oil-based carrier comprises mineral oil, cyclopentasiloxane, cyclohexasiloxane, isoparaffin fluid, polyethylene glycol and polyisobutylene, or these mixtures.In specific example embodiment, the oil-based carrier of liquid-based pigment masterbatch is mineral oil.In further specific example embodiment, the oil-based carrier of liquid-based pigment masterbatch is polyisobutylene.In further specific example embodiment, the oil-based carrier of liquid-based pigment masterbatch is the mixture of mineral oil and polyisobutylene.In further specific example embodiment, the oil-based carrier of liquid-based pigment masterbatch is the mixture of polyethylene glycol and polyisobutylene.In further specific example embodiment, the oil-based carrier of liquid-based pigment masterbatch is the mixture of polyethylene glycol and mineral oil.

[0054] Examples of liquid-based pigment masterbatches may include 5 wt % to 60 wt %, or 10 wt % to 60 wt %, or 15 wt % to 60 wt %, or 20 wt % to 60 wt % of the second pigment, based on the total weight of the liquid-based pigment masterbatch; and 40 wt % to 95 wt %, or 40 wt % to 90 wt %, or 40 wt % to 85 wt %, or 40 wt % to 80 wt % of the oil-based carrier, based on the total weight of the liquid-based pigment masterbatch.

[0055] In some example embodiments of the molded article, the second pigment is a metallic pigment, is a metallic colorant, or includes metallic flakes, and the oil-based carrier is a mixture of polyisobutylene and mineral oil. In such embodiments, the second pigment and the oil-based carrier can be derived from a liquid-based pigment masterbatch, wherein the oil-based carrier comprises 30 wt % to 70 wt % of polyisobutylene based on the total weight of the oil-based carrier; and 30 wt % to 70 wt % of mineral oil based on the total weight of the oil-based carrier.

[0056] In some example embodiments of the molded article, the second pigment is a non-metallic colorant and the oil-based carrier is a mixture of polyethylene glycol and mineral oil. In such embodiments, the second pigment and the oil-based carrier can be derived from a liquid-based pigment masterbatch, wherein the oil-based carrier comprises 10 wt % to 30 wt % of polyethylene glycol based on the total weight of the oil-based carrier; and 70 wt % to 90 wt % of mineral oil based on the total weight of the oil-based carrier.

[0057] The molded article according to the embodiments may have any shape or size.In some embodiments, the molded article may be a bottle or a cap for a bottle intended for use in the cosmetics industry or for purposes that may require a decorative effect imparted by the first pigment and the second pigment.

[0058] Having described embodiments of molded articles, embodiments of methods for preparing molded articles will now be described. The method for preparing a molded article according to any of the foregoing embodiments may include dry blending a neutralized acid copolymer, a nylon-based pigment masterbatch, and a liquid-based pigment masterbatch to form an initial mixture. The neutralized acid copolymer and the nylon-based pigment masterbatch may be in bulk form, such as pellets or powders. The liquid-based pigment masterbatch may be added in liquid form to the combination of the neutralized acid copolymer and the nylon-based pigment masterbatch prior to dry blending to produce the initial mixture.

[0059] In the method for preparing a molded article, the initial mixture can be fed into a molding device such as an injection molding device. The initial mixture is molded in the molding device to form a molded article by any suitable molding technique under standard process conditions.

[0060] In the method for preparing molded articles, the initial mixture can include at least 75 wt % or at least 80 wt % or at least 85 wt % or at least 90 wt % or at least 95 wt % of the neutralized acid copolymer by the total weight of the initial mixture. The initial mixture can also include 0.1 wt % to 5 wt %, 0.1 wt % to 0.4 wt %, 0.1 wt % to 0.3 wt % or 0.1 wt % to 0.2 wt % of the pigment masterbatch based on polyamide by the total weight of the initial mixture. In certain embodiments, the initial mixture can include multiple pigment masterbatch based on polyamide. In such embodiments, the initial mixture can include all pigment masterbatch based on polyamide of 0.1 combination weight % to 5 combination weight %, 0.1 combination weight % to 0.4 combination weight %, 0.1 combination weight % to 0.3 combination weight % or 0.1 combination weight % to 0.2 combination weight % in total by the total weight of the initial mixture.

[0061] In the method for preparing molded articles, the initial mixture can also include 0.2% by weight to 5.7% by weight, or 0.2% by weight to 5% by weight, or 0.2% by weight to 4% by weight, or 0.2% by weight to 3% by weight, or 0.2% by weight to 2% by weight, or 0.2% by weight to 1.5% by weight, or 0.2% by weight to 1% by weight of a liquid-based pigment masterbatch. In certain embodiments, the initial mixture can include multiple liquid-based pigment masterbatches. In such embodiments, the initial mixture can include all polyamide-based pigment masterbatches of 0.2% by weight to 5.7% by weight, or 0.2% by weight to 5% by weight, or 0.2% by weight to 4% by weight, or 0.2% by weight to 3% by weight, or 0.2% by weight to 2% by weight, or 0.2% by weight to 1.5% by weight, or 0.2% by weight to 1% by weight, by the total weight of the initial mixture.

[0062] The neutralized acid copolymer, the polyamide-based pigment masterbatch (comprising a first pigment and a polyamide), and the liquid-based pigment masterbatch (comprising a second pigment and an oil-based carrier) have all been described above in connection with the examples of molded articles.

[0063] As the component of initial mixture, the pigment masterbatch based on polyamide can include 30 wt % to 95 wt % of polyamide by the total weight of the pigment masterbatch based on polyamide, and 5 wt % to 70 wt % of the first pigment associated with polyamide by the total weight of nylon-based pigment masterbatch.As the component of initial mixture, the liquid-based pigment masterbatch can include 5 wt % to 60 wt % of the second pigment by the total weight of the liquid-based pigment masterbatch, and 40 wt % to 95 wt % of the oil-based carrier by the total weight of the liquid-based pigment masterbatch.In an embodiment, the initial mixture as a whole can include 0.1 wt % to 5 wt % of the second pigment by the total weight of the initial mixture and 0.1 wt % to 0.7 wt %, or 0.1 wt % to 0.6 wt %, or 0.1 wt % to 0.5 wt %, or 0.1 wt % to 0.4 wt % of the oil-based carrier. Without wishing to be bound by theory, it is believed that an excess of oil-based carrier in the initial mixture may result in undesirable viscosity characteristics of the initial mixture, which may, in some cases, render the initial mixture unsuitable for forming molded articles by injection molding.

[0064] Embodiments of molded articles according to the present disclosure are understood to include embodiments of molded articles prepared by embodiments of methods according to the present disclosure or by any other suitable method that produces a molded article as described herein.

[0065] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art of molded articles or molding technology. The terms used in the specification herein are only for describing specific embodiments and are not intended to be limiting. As used in the specification and the appended claims, the singular forms "a / an" and "the" are also intended to include the plural forms unless the context clearly indicates otherwise.

[0066] Example

[0067] Embodiments of molded articles and related methods of making the same will be better understood by reference to the following examples, which are provided by way of illustration and those skilled in the art of molded articles or molding technology will recognize that these embodiments are not meant to be limiting.

[0068] General injection molding process

[0069] In order to verify the various decorative effects that can be obtained in molded articles, an initial mixture is prepared according to a predetermined decorative design by dry blending a mixture of an ionomer resin, at least one polyamide-based pigment masterbatch and at least one liquid-based pigment masterbatch. The dry blended mixture is then fed into an injection molding device to evaluate whether the formulated initial mixture is suitable for producing molded articles.

[0070] The ionomer resins of all the following examples are ethylene acid copolymers containing from about 15 wt% to about 30 wt% copolymerized units of acrylic acid or methacrylic acid, based on the total weight of the parent acid copolymer. The melt flow rate of the ionomer is about 4.5 g / 10 min, measured at 190° C. and 2160 g load according to ASTM D1238. In the ionomer, from about 40% to about 70% of the total carboxylic acid groups of the copolymer are neutralized to carboxylate salts containing sodium cations.

[0071] The polyamide-based pigment masterbatch in the embodiment is a commercially available formulation comprising nylon 6 as a polyamide component. The liquid-based pigment masterbatch in the embodiment is a commercially available formulation comprising a pigment and an oil-based carrier. The oil-based carrier in the liquid-based pigment masterbatch comprises one or more of polyethylene glycol, mineral oil and polyisobutylene, and one or more additional additives. The additional ingredients in the initial mixture are described in more detail by their respective embodiments.

[0072] Table 1 below summarizes the parameters of the injection molding process applied in all examples:

[0073] Table 1: General injection molding parameters of the examples

[0074]

[0075] Example 1

[0076] An initial mixture was prepared, which contained 98.6 wt% of ionomer resin, 0.4 wt% of a polyamide-based pigment masterbatch having a light brown first pigment, and 1.0 wt% of a liquid-based pigment masterbatch having a white second pigment. The polyamide-based pigment masterbatch contained nylon 6 as the polyamide and a light brown first pigment. The colorant density of the liquid-based pigment was 2.26 g / cm 3 , and contains about 87.1% by weight of the second pigment and about 12.9% by weight of the oil-based carrier. The oil-based carrier contains about 20% by weight of polyethylene glycol and about 80% by weight of mineral oil. Therefore, the initial mixture contains 98.6% by weight of the ionomer resin, 0.4% by weight of the light brown first pigment based on polyamide, 0.87% by weight of the white second pigment and 0.13% by weight of the oil-based carrier.

[0077] The molded article was successfully prepared by subjecting the initial mixture to an injection molding process according to the general injection molding procedure described previously. The molded article appeared pure white with light brown streaks similar to white marble.

[0078] Example 2

[0079] An initial mixture is prepared, which contains 98.7 wt% of an ionomer resin, 0.15 wt% of a polyamide-based pigment masterbatch having a light brown first pigment, 0.15 wt% of a polyamide-based pigment masterbatch having a white first pigment, and 1.0 wt% of a liquid-based pigment masterbatch having a black second pigment. The light brown polyamide-based pigment masterbatch contains nylon 6 as the polyamide and the light brown first pigment. The white polyamide-based pigment masterbatch contains nylon 6 as the polyamide and the white first pigment, and contains 55 wt% to 65 wt% of polyamide and about 35 wt% to 45 wt% of titanium dioxide (TiO 2 ) as a white pigment. Thus, the initial mixture contained 98.6 wt % of the ionomer resin, a total of 0.6 wt % of the polyamide-based first pigment, and 1.0 wt % of the second pigment in an oil-based carrier.

[0080] The molded articles having the weight proportions of the initial mixture were successfully prepared by subjecting the initial mixture to an injection molding process according to the previously described general injection molding procedure. The molded articles appeared pure black with white and light brown streaks similar to black marble.

[0081] Example 3

[0082] An initial mixture is prepared, which contains 98.8% by weight of ionomer resin, 0.2% by weight of a polyamide-based pigment masterbatch with a black first pigment, and 1.0% by weight of a liquid-based pigment masterbatch with a white second pigment. The polyamide-based pigment masterbatch contains about 88% by weight to about 92% by weight of nylon 6 as a polyamide and about 8% by weight to about 12% by weight of carbon black as a black first pigment. The colorant density of the liquid-based pigment is 2.26, and contains about 87.1% by weight of a second pigment and about 12.9% by weight of an oil-based carrier. The oil-based carrier contains about 20% by weight of polyethylene glycol and about 80% by weight of mineral oil. Therefore, the initial mixture contains 98.8% by weight of ionomer resin, 0.2% by weight of a polyamide-based black first pigment, 0.87% by weight of a white second pigment, and 0.13% by weight of an oil-based carrier.

[0083] The molded articles having the weight proportions of the initial mixture were successfully prepared by subjecting the initial mixture to an injection molding process according to the previously described general injection molding procedure. The molded articles appeared pure white with black streaks similar to white marble with dark veins.

[0084] Example 4

[0085] An initial mixture was prepared, which contained 98.5 wt% of an ionomer resin, 0.2 wt% of a polyamide-based pigment masterbatch having a light brown first pigment, 0.3 wt% of a polyamide-based pigment masterbatch having a black first pigment, and 1 wt% of a liquid-based pigment masterbatch having a metallic copper second pigment. The light brown polyamide-based pigment masterbatch contained nylon 6 as the polyamide and a light brown first pigment. The black polyamide-based pigment masterbatch contained about 88 wt% to about 92 wt% of nylon 6 as the polyamide and about 8 wt% to about 12 wt% of carbon black as the black first pigment. The colorant density of the liquid-based pigment was 1.12 g / cm 3 , and contains about 60.8 weight percent of the second pigment and about 39.2 weight percent of the oil-based carrier. The oil-based carrier contains about 50 weight percent of polyisobutylene and about 50 weight percent of mineral oil. Therefore, the initial mixture contains 98.5 weight percent of the ionomer resin, a total of 0.5 weight percent of the light brown and black first pigment based on polyamide, 0.61 weight percent of the metallic copper second pigment, and 0.39 weight percent of the oil-based carrier.

[0086] The molded articles having the weight proportions of the initial mixture were successfully prepared by subjecting the initial mixture to the injection molding process of the previously described general injection molding procedure. The molded articles exhibited a metal decorative effect similar to antique brass, in which fine black and brown stripes were present on the brass-like metal template.

[0087] Example 5

[0088] An initial mixture was prepared, which contained 98.3 wt% of an ionomer resin, 0.2 wt% of a polyamide-based pigment masterbatch having a light brown first pigment, 0.2 wt% of a polyamide-based pigment masterbatch having a black first pigment, and 1.3 wt% of a liquid-based pigment masterbatch having a metallic copper second pigment. The light brown polyamide-based pigment masterbatch contained nylon 6 as the polyamide and a light brown first pigment. The black polyamide-based pigment masterbatch contained about 88 wt% to about 92 wt% of nylon 6 as the polyamide and about 8 wt% to about 12 wt% of carbon black as the black first pigment. The colorant density of the liquid-based pigment was 0.94 g / cm 3 , and contains about 24.2% by weight of the second pigment and about 75.8% by weight of the oil-based carrier. The oil-based carrier contains about 20% by weight of polyethylene glycol and about 80% by weight of mineral oil. Therefore, the initial mixture contains 98.3% by weight of the ionomer resin, a total of 0.4% by weight of the light brown and black first pigment based on polyamide, 0.79% by weight of the metallic copper second pigment and 0.51% by weight of the oil-based carrier.

[0089] The molded articles having the weight proportions of the initial mixture were successfully prepared by subjecting the initial mixture to the injection molding process of the previously described general injection molding procedure. The molded articles exhibited a metal decorative effect similar to earthy copper, in which fine black and brown stripes were present on the copper-like metal template.

[0090] Comparative Example 1

[0091] An initial mixture was prepared by slightly changing the formulation of the initial mixture of Example 4 by replacing 1 wt % of the liquid-based pigment masterbatch having a metallic copper second pigment from Example 4 with 1 wt % of the alternative liquid-based pigment masterbatch having a metallic copper second pigment. Whereas the liquid-based pigment masterbatch from Example 4 contained about 60.8 wt % of the second pigment and about 39.2 wt % of an oil-based carrier composed of about 50 wt % polyisobutylene and about 50 wt % mineral oil, the alternative liquid-based pigment masterbatch contained about 24.2 wt % of the second pigment and about 75.8 wt % of an oil-based carrier composed of about 20 wt % polyethylene glycol and about 80 wt % mineral oil. Thus, like the initial mixture of Example 4, the initial mixture of this example contained equal weight parts of ionomer resin (98.5%) and total polyamide-based pigment (0.5%). However, while the initial mixture of Example 4 contained approximately 0.61 wt % of the metallic copper secondary pigment and 0.39 wt % of the oil-based carrier, the initial mixture of this Example contained 0.24 wt % of the metallic copper secondary pigment and 0.76 wt % of the oil-based carrier.

[0092] By the general injection molding procedure described previously, molded articles could not be produced from the initial mixture of this example due to screw slippage during the molding process. It is believed that the increased amount of oil-based carrier present in the initial mixture adversely affects the viscosity and flow characteristics of the initial mixture, thereby making the mixture unable to be injection molded.

[0093] Comparative Example 2

[0094] An initial mixture was prepared by slightly changing the formulation of the initial mixture of Example 5 by replacing 1.3 wt % of the liquid-based pigment masterbatch having a metallic copper second pigment from Example 5 with 1.3 wt % of the alternative liquid-based pigment masterbatch having a metallic copper second pigment. Whereas the liquid-based pigment masterbatch from Example 5 contained about 60.8 wt % of the second pigment and about 39.2 wt % of an oil-based carrier composed of about 50 wt % polyisobutylene and about 50 wt % mineral oil, the alternative liquid-based pigment masterbatch contained about 24.2 wt % of the second pigment and about 75.8 wt % of an oil-based carrier composed of about 20 wt % polyethylene glycol and about 80 wt % mineral oil. Thus, like the initial mixture of Example 5, the initial mixture of this example contained equal weight parts of ionomer resin (98.3%) and total polyamide-based pigment (0.4%). However, whereas the initial mixture of Example 5 contained approximately 0.79 wt % metallic copper secondary pigment and 0.51 wt % oil-based carrier, the initial mixture of this Example contained 0.31 wt % metallic copper secondary pigment and 0.99 wt % oil-based carrier.

[0095] By the general injection molding procedure described previously, molded articles could not be produced from the initial mixture of this example due to screw slippage during the molding process. It is believed that the increased amount of oil-based carrier present in the initial mixture adversely affects the viscosity and flow characteristics of the initial mixture, thereby making the mixture unable to be injection molded.

[0096] Analytical characterization of molded articles

[0097] The final composition of the molded articles prepared according to the foregoing description and examples can be determined by known analytical techniques. Examples of suitable analytical techniques will now be described.

[0098] Oil-based carrier assay

[0099] The oil-based carrier derived from the liquid-based pigment masterbatch can be confirmed in the neutralized acid copolymer molded article by common analytical techniques.Examples of oil-based carriers include, but are not limited to, mineral oil, polyisobutylene (PIB), polyethylene glycol (PEG), or combinations of these.

[0100] To confirm the presence of an oil-based carrier in a molded article, a sample of the molded article can be cryogenically ground and extracted into a suitable solvent (e.g., hexane or dichloromethane). The resulting solution is then concentrated by evaporating some or all of the solvent. The extracted material is then redissolved in a solvent suitable for analysis by NMR or two-dimensional gas chromatography (GC×GC).

[0101] Polyethylene glycol from an oil-based carrier can be obtained at levels below 100 ppm using standard techniques. 1Qualitative and quantitative identification is performed by H NMR. Even without cryo-grinding and extraction, the analysis can be performed directly on sample solutions prepared from the preparation. The lowest detection limits can be obtained by analyzing extracted samples. Polyethylene glycol and polyisobutylene can be determined by standard techniques. 13 C NMR qualitative and quantitative identification to a level of about 100 ppm. The analysis can be performed directly on sample solutions prepared from the preparation, even without cryo-grinding and extraction. The lowest detection limits can be obtained by analyzing extracted samples.

[0102] As described in detail in M.Biederman et al., Journal of Chromatography Volume A 1375 (2015), pp. 146-153, comprehensive two-dimensional gas chromatography (GC×GC) can distinguish mineral oil saturated hydrocarbons (MOSH) from polymer oligomeric saturated hydrocarbons (POSH). Mass spectrometry (MS) is used to identify compounds, while flame ionization detector (FID) is used for quantification. High pressure liquid chromatography fractionation can be used before GC×GC-MS analysis.

[0103] Pigment weight percentage in liquid-based pigment molded articles

[0104] The pigment weight percentage in a liquid-based pigment masterbatch can be determined by measuring the solid content in the masterbatch. A known weight of a liquid-based pigment masterbatch is diluted in a solvent (e.g., hexane) and centrifuged under conditions that allow the solids to be recovered and dried. The pigment weight percentage in the original masterbatch is the weight of the recovered and dried solids divided by the original weight of the masterbatch diluted in the solvent and then divided by 100.

[0105] Pigment weight percentage in molded articles

[0106] A quantitative determination of the total weight of pigment in the neutralized acid copolymer molded article relative to the total weight of the molded article can be determined by thermogravimetric analysis (TGA) of a sample of the molded article.

[0107] Qualitative and quantitative determination of pigments in molded articles

[0108] According to the neutralized acid copolymer molded articles of the present disclosure and embodiments contain a neutralized acid copolymer, a first pigment derived from a polyamide-based pigment masterbatch (e.g., a nylon-based pigment masterbatch), and a second pigment derived from a liquid-based pigment masterbatch. The presence of the two pigments in the molded article, the source of the pigment from the polyamide-based masterbatch or the liquid-based masterbatch, and its weight fraction relative to the total weight of the molded article can be determined by standard analytical techniques. In principle, the analytical technique relies on the observation that the first pigment derived from the polyamide-based pigment masterbatch remains associated with its polyamide-based carrier as a discrete phase in the molded article, and is separated or unevenly mixed with the phase containing the neutralized acid copolymer and the second pigment derived from the liquid-based pigment masterbatch. In addition, the first pigment and the second pigment themselves may be insoluble in each other in their respective carriers. For example, the first pigment may be insoluble in the oil-based carrier of the liquid-based pigment masterbatch, while the second pigment may be insoluble in or incompatible with the polyamide-based carrier of the polyamide-based pigment masterbatch.

[0109] Qualitative and quantitative determination of the first pigment and the second pigment in the neutralized acid copolymer molded article can be performed on the molded article itself without dissolving the molded article. For example, a sample of the molded article can be analyzed by scanning electron microscopy (SEM) and energy dispersive spectroscopy (EDS). The combination of microscopy and elemental analysis provides a quantitative spatial map of the elemental composition of the sample. Because in the molded article, the first pigment based on polyamide is not uniformly dispersed throughout the copolymer matrix of the molded article, the first pigment is observed in the polyamide region of the sample, independent of the second pigment in the continuous phase.

[0110] Qualitative and quantitative determination of the first pigment and the second pigment in the neutralized acid copolymer molded article can be performed on a cryogenically ground sample of the molded article. Due to the significant difference in the solubility of polyamide and vinyl copolymers, the cryogenically ground sample can be selectively dissolved with a solvent combination that separates the polyamide phase containing the first pigment from the copolymer phase containing the second pigment. The resulting solution is dried and analyzed by thermogravimetric analysis (TGA) to determine the pigment content in each phase. An example of a TGA protocol for determining the amount of carbon black pigment in a plastic, wherein the carbon black pigment is derived from a nylon-based masterbatch, can be obtained in TA Instruments Thermal Analysis Application Brief No. TA-122 entitled "Determination of Carbon Black Pigment in Nylon 66 by TGA". This TGA protocol is easily adapted to determine other pigment molecules and various molded plastics / copolymers.

[0111] Qualitative and quantitative determination of the first and second pigments in the neutralized acid copolymer molded article can be performed by elemental analysis (CHNO), according to which the weight percentage of the pigment relative to the total weight of the molded article can be determined based on only a few milligrams of sample from the molded article.

[0112] To perform elemental analysis on the first pigment from the polyamide-based pigment masterbatch, a portion of the polyamide phase of the molded article sufficient for analysis is removed from the molded article by mechanical means (such as drilling or grinding).The removed portion is subjected to conventional elemental analysis.

[0113] To perform elemental analysis of the second pigment from the liquid-based pigment masterbatch, similar techniques can be applied, except that the sample removed from the molded article is removed from the exterior of the polyamide phase, i.e., in the continuous phase of the colored acid-neutralized copolymer. However, for this analysis, the neutralized acid copolymer composition (CHNO content) must also be known so that the elemental content of the copolymer can be subtracted from the elemental analysis of the continuous phase to obtain the elemental content of the second pigment. Determination of the neutralized acid copolymer composition is accurately measured by NMR using standard techniques well known to those of ordinary skill in the art.

[0114] It should be noted that the terms "substantially" and "about" may be used herein to represent the inherent degree of uncertainty that may be attributed to any quantitative comparison, value, measurement or other representation. These terms are also used herein to represent the degree by which a quantitative representation may vary from a stated reference without resulting in a change in the basic function of the subject matter at issue.

[0115] Although specific embodiments have been illustrated and described herein, it will be appreciated that various other changes and modifications may be made without departing from the spirit and scope of the claimed subject matter. In addition, although various aspects of the claimed subject matter have been described herein, such aspects need not be utilized in combination. It is therefore contemplated that the appended claims cover all such changes and modifications within the scope of the claimed subject matter.

Claims

1. A molded product with a decorative effect, the molded product comprising: at least 75 wt % of a neutralized acid copolymer, based on the total weight of the molded article, wherein the neutralized acid copolymer is an ionomer resin; 0.1 to 5 wt % of a polyamide-based pigment masterbatch, based on the total weight of the molded article, the polyamide-based pigment masterbatch comprising 30 to 95 wt % of a polyamide, based on the total weight of the polyamide-based pigment masterbatch, and 5 to 70 wt % of a first pigment associated with the polyamide, based on the total weight of the polyamide-based pigment masterbatch; and 0.1 wt % to 5 wt % of a second pigment derived from a liquid-based pigment masterbatch, based on the total weight of the molded article, the second pigment being a metallic colorant or a non-metallic colorant; and 0.1 wt % to 0.7 wt % of an oil-based carrier derived from the liquid-based pigment masterbatch, based on the total weight of the molded article; wherein: The second pigment is a metallic colorant; and The oil-based carrier comprises: 30 to 70 wt % of polyisobutylene, based on the total weight of the oil-based carrier; and 30 wt % to 70 wt % of mineral oil based on the total weight of the oil-based carrier; or the second pigment is a non-metallic colorant; and The oil-based carrier comprises: 10 wt % to 30 wt % of polyethylene glycol based on the total weight of the oil-based carrier; and 70 to 90 wt% of mineral oil based on the total weight of the oil-based carrier.

2. The molded article according to claim 1, wherein: The neutralized acid copolymer is a continuous phase within the molded article; The polyamide-based pigment masterbatch is present as a first secondary phase within the molded article; The second pigment is present as a second secondary phase within the molded article; The oil-based carrier is present as a third secondary phase within the molded article; and The first secondary phase is not uniformly distributed within the continuous phase.

3. The molded article according to claim 1 or 2, wherein the liquid-based pigment masterbatch comprises: 5 to 60 wt % of the second pigment based on the total weight of the liquid-based pigment masterbatch; and 40 wt % to 95 wt % of the oil-based carrier based on the total weight of the liquid-based pigment masterbatch.

4. The molded article according to claim 1 or 2, wherein the neutralized acid copolymer is an ionomer resin having a melt flow index of 4 to 6 g / 10 min as measured according to ASTM D1238.

5. The molded article of claim 1 or 2, wherein the neutralized acid copolymer is an ethylene methacrylic acid copolymer, wherein the methacrylic acid groups of the copolymer are at least partially neutralized with sodium ions.

6. The molded article according to claim 1 or 2, wherein: The neutralized acid copolymer comprises 15 to 30 weight percent copolymerized units of acrylic acid or methacrylic acid and 70 to 85 weight percent copolymerized units of ethylene, based on the total weight of the neutralized acid copolymer; and 40% to 70% of the carboxylic acid groups of the neutralized acid copolymer are neutralized as carboxylate salts containing sodium cations.

7. The molded article according to claim 1 or 2, wherein the oil-based carrier comprises polyisobutylene, polyethylene glycol, mineral oil, or a combination thereof.

8. The molded article according to claim 1 or 2, wherein the first pigment is selected from the group consisting of carbon black, aniline black, metal-based pigments, cadmium pigments, chromium pigments, cobalt pigments, copper pigments, iron oxide pigments, lead pigments, manganese pigments, mercury pigments, titanium pigments, zinc pigments, aluminum powder, vine black, lamp black, ivory black, clay pigments, iron oxide, yellow ochre, raw ochre, burnt sienna, raw umber, burnt umber, ultramarine, alizarin, alizarin crimson, gamboge, cochineal, rose madder, indigo, Indian yellow, Tyrian violet, quinacridone, fuchsin, phthalocyanine green, phthalocyanine blue, pigment red 170, and diaryl yellow.

9. The molded article according to claim 1 or 2, wherein the polyamide-based pigment masterbatch is a nylon-based pigment masterbatch, and the polyamide is nylon 6.

10. The molded article according to claim 1 or 2, wherein the molded article is a decorative cap for a bottle.

11. A method for preparing a molded article, the method comprising: dry blending a neutralized acid copolymer, a polyamide-based pigment masterbatch, and a liquid-based pigment masterbatch to form an initial mixture, wherein the neutralized acid copolymer is an ionomer resin; feeding the initial mixture into an injection molding device; molding the initial mixture with the injection molding device to form the molded article, in: Based on the total weight of the initial mixture, the initial mixture comprises: at least 75% by weight of said neutralized acid copolymer; 0.1 wt% to 5 wt% of the polyamide-based pigment masterbatch; and 0.2 wt % to 5.7 wt % of the liquid-based pigment masterbatch; The polyamide-based pigment masterbatch comprises 30 to 95 wt % of a polyamide, based on the total weight of the polyamide-based pigment masterbatch, and 5 to 70 wt % of a first pigment associated with the polyamide, based on the total weight of the polyamide-based pigment masterbatch; The liquid-based pigment masterbatch comprises 5 to 60 wt % of a second pigment based on the total weight of the liquid-based pigment masterbatch, and 40 to 95 wt % of an oil-based carrier based on the total weight of the liquid-based pigment masterbatch, wherein: The second pigment is a metallic colorant; and The oil-based carrier comprises: 30 to 70 wt % of polyisobutylene, based on the total weight of the oil-based carrier; and 30 wt % to 70 wt % of mineral oil based on the total weight of the oil-based carrier; or the second pigment is a non-metallic colorant; and The oil-based carrier comprises: 10 wt % to 30 wt % of polyethylene glycol based on the total weight of the oil-based carrier; and 70 wt % to 90 wt % of mineral oil based on the total weight of the oil-based carrier.

12. The method of claim 11, wherein the initial mixture comprises 0.1 wt% to 0.7 wt% of the oil-based carrier from the liquid-based pigment masterbatch, based on the total weight of the initial mixture.

13. A molded article produced by the method according to claim 11 or 12.