NiO / SiO2 catalyst and its preparation method and application

By preparing NiO/SiO2 catalyst, the problem of sintering active components of Ni/SiO2 catalyst at high temperature was solved, the catalytic activity and methane conversion rate were improved, and the stable and efficient catalytic effect was achieved at high temperature.

CN114789054BActive Publication Date: 2024-11-26PETROCHINA CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202110100054.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-25
Publication Date
2024-11-26
Estimated Expiration
2041-01-25

AI Technical Summary

Technical Problem

When the existing Ni/SiO2 catalysts catalyze the reforming reaction between methane and carbon dioxide, the active component Ni is prone to sintering, resulting in a reduced catalytic activity and a lower methane conversion rate.

Method used

Using the preparation method of NiO/SiO2 catalyst, NiO/SiO2 catalyst is formed by adding silica sol to the nickel ammonia complex solution, and after distillation, drying and calcining, NiO/SiO2 catalyst is formed, and the reaction conditions such as stirring time, pH value, temperature and calcining are optimized. time to improve catalytic activity and stability.

Benefits of technology

The catalytic activity is improved, ensuring that the active components are not easy to sinter, and the methane conversion rate is significantly improved, especially maintaining stable high catalytic activity at high temperatures, and the methane conversion rate is increased by 5% to 36%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114789054B_ABST
    Figure CN114789054B_ABST
Patent Text Reader

Abstract

The present invention provides a NiO / SiO 2 Catalyst and its preparation method and application. The preparation method comprises: S1, adding ammonia water to nickel nitrate solution to form a nickel ammonia complex solution; S2, adding silica sol to the nickel ammonia complex solution, stirring the reaction to obtain a suspension; S3, subjecting the suspension to ammonia evaporation and drying treatment in sequence to obtain a reaction product Ni 3 Si 2 O 5 (OH) 4 / SiO 2 The reaction product is calcined to obtain NiO / SiO 2 Catalyst. The NiO / SiO prepared by the present invention 2 When the catalyst is used to catalyze the reforming reaction of methane and carbon dioxide, the catalytic activity is higher, especially the stability is better, the active component is not easy to sinter, and thus the high and stable catalytic activity can be always maintained in the reforming reaction, so that the conversion rate of methane in the reforming reaction is greatly improved. Moreover, the preparation method of the present invention has simpler preparation conditions and the process is easier to control.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalysts, and in particular to a NiO / SiO2 catalyst and a preparation method and application thereof. Background Art

[0002] In 2005, JP2005254091A disclosed a Ni / SiO2 catalyst and a production method thereof. The method provides a highly active catalyst having both macropores and fine pores, excellent material transfer capability and high Ni specific surface area. However, the dispersion of the catalyst Ni component is not high, resulting in insufficient catalytic properties. CN102500380A discloses a method for preparing nano Ni catalyst particles on a Si substrate. The Si substrate is first cleaned, and then the cleaned Si substrate is placed in a nickel nitrate ethanol solution for ultrasonic vibration and then placed in a muffle furnace for drying to obtain a Si substrate coated with a Ni film. The prepared Si substrate coated with a Ni film is placed in a quartz boat, placed in a high-temperature tubular atmosphere furnace, N2 is introduced to remove the air in the tubular furnace, and then the temperature is raised to prepare nano catalyst particles on the substrate using a high-temperature ammonia etching method. Finally, N2 is introduced to remove NH3 in the tubular furnace, and the nano Ni catalyst particles prepared on the Si substrate are completed. CN104511279A discloses a high-efficiency methane carbon dioxide reforming Ni / SiO2 catalyst and its electrostatic spinning preparation method. By electrostatic spinning technology, a high-efficiency catalyst of silicon dioxide nanofiber loaded with nickel nanoparticles is prepared. Its preparation steps first prepare a spinning precursor solution, then electrostatic spinning, and finally dry and roast to obtain a finished product. CN105363452A provides a method for preparing a double mesoporous structure Ni / SiO2-ZrO2 catalyst for partial oxidation of methane. The invention prepares a double mesoporous structure Ni / SiO2-ZrO2 catalyst loaded with active component nickel by impregnation. CN108579750A discloses a copper-doped nanocomposite Ni / SiO2 catalyst and its preparation method. The nanocomposite catalyst is made of nickel nitrate, sodium silicate and dilute nitric acid as raw materials, and is prepared by precipitation method, aging, filtering, washing, drying, grinding and reduction.

[0003] However, after the Ni / SiO2 catalyst existing in the prior art is reduced and activated, when it is used to catalyze the reforming reaction of methane and carbon dioxide (temperature as high as 700-850°C), the active component Ni is easily sintered, which leads to a decrease in the catalytic activity of the catalyst and a low methane conversion rate. Summary of the invention

[0004] The main purpose of the present invention is to provide a NiO / SiO2 catalyst and a preparation method and application thereof, so as to solve the problem in the prior art that when the Ni / SiO2 catalyst is used to catalyze the reforming reaction of methane and carbon dioxide, the active component Ni is easily sintered, resulting in poor catalytic effect of the catalyst and low methane conversion rate.

[0005] In order to achieve the above-mentioned object, according to one aspect of the present invention, a method for preparing a NiO / SiO2 catalyst is provided. The preparation method comprises the following steps: S1, adding ammonia water to a nickel nitrate solution to form a nickel ammonia complex solution; S2, adding silica sol to the nickel ammonia complex solution, and stirring the reaction to obtain a suspension; S3, subjecting the suspension to ammonia evaporation and drying treatment in sequence to obtain a reaction product Ni3Si2O5(OH)4 / SiO2, and subjecting the reaction product Ni3Si2O5(OH)4 / SiO2 to a calcination treatment to obtain a NiO / SiO2 catalyst.

[0006] Furthermore, the weight ratio of nickel nitrate to silica sol is 1:(8.5-16.5).

[0007] Furthermore, the mass concentration of SiO2 in the silica sol is 20% to 30%.

[0008] Furthermore, the pH value of the nickel ammine complex solution is 10-12.

[0009] Furthermore, in step S2, the stirring reaction time is 6 to 12 hours.

[0010] Furthermore, during the ammonia evaporation treatment, the temperature is 80°C to 95°C, and the pH value of the suspension after the ammonia evaporation treatment is 6 to 7. Preferably, during the drying treatment, the temperature is 100°C to 160°C, and the time is 8 to 16 hours. Preferably, before the drying treatment, step S2 also includes the step of washing the suspension after the ammonia evaporation treatment. Preferably, during the roasting treatment, the temperature is 700 to 900°C, and the time is 2 to 8 hours.

[0011] In order to achieve the above object, according to one aspect of the present invention, a NiO / SiO2 catalyst is provided. The NiO / SiO2 catalyst is prepared by the above-mentioned method for preparing the NiO / SiO2 catalyst.

[0012] Furthermore, the particle size of the NiO / SiO2 catalyst is 20-40 meshes.

[0013] According to another aspect of the present invention, there is provided an application of a NiO / SiO2 catalyst in a reforming reaction of methane and carbon dioxide. The NiO / SiO2 catalyst is prepared by the above-mentioned preparation method, or the above-mentioned NiO / SiO2 catalyst is subjected to hydrogen reduction activation treatment to obtain an activated catalyst; and the activated catalyst is used to catalyze the reforming reaction of methane and carbon dioxide.

[0014] Furthermore, during the reforming reaction, the reaction temperature is 700-850°C, and the mass space velocity of methane and carbon dioxide is independently 1.0-4.0h -1 , the molar ratio of methane and carbon dioxide is 1:(1.0~1.2).

[0015] The NiO / SiO2 catalyst prepared by the present invention has higher catalytic activity, especially better stability, when used to catalyze the reforming reaction of methane and carbon dioxide (reaction temperature is as high as 700-850°C), and the active components are not easy to sinter, so that the high catalytic activity can be maintained stably in the reforming reaction, and the conversion rate of methane in the reforming reaction is greatly improved. Moreover, the preparation method of the present invention has simpler preparation conditions and the process is easier to control. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0017] Figure 1 shows the XRD spectrum of the reaction product Ni3Si2O5(OH)4 / SiO2 in Example 1 of the present invention; and

[0018] Figure 2 The XRD spectrum of the NiO / SiO2 catalyst in Example 1 of the present invention is shown. DETAILED DESCRIPTION

[0019] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0020] As described in the background technology section, when Ni / SiO2 catalysts in the prior art are used to catalyze the reforming reaction of methane and carbon dioxide, the active component Ni is easily sintered, resulting in poor catalytic effect of the catalyst and low methane conversion rate.

[0021] In order to solve this problem, the present invention provides a method for preparing a NiO / SiO2 catalyst. The preparation method comprises the following steps: S1, adding ammonia water to a nickel nitrate solution to form a nickel ammonia complex solution; S2, adding silica sol to the nickel ammonia complex solution, and stirring the reaction to obtain a suspension; S3, subjecting the suspension to ammonia evaporation and drying treatment in sequence to obtain a reaction product Ni3Si2O5(OH)4 / SiO2, and subjecting the reaction product to a calcination treatment to obtain a NiO / SiO2 catalyst.

[0022] The present invention adopts the method of adding silica sol to a nickel-ammine complex solution, and then sequentially evaporating ammonia, drying and calcining to form a NiO / SiO2 catalyst. The NiO / SiO2 catalyst prepared by the above operation has higher catalytic activity. The NiO / SiO2 catalyst prepared by the present invention has higher catalytic activity when used to catalyze the reforming reaction of methane and carbon dioxide (reaction temperature is as high as 700-850°C), so that the conversion rate of methane in the reforming reaction is greatly improved. In particular, compared with the catalyst prepared by the impregnation method and the precipitation method, the NiO / SiO2 catalyst obtained by the preparation method of the present invention can promote the methane conversion rate in the reforming reaction to increase by 5% to 36%. Moreover, the preparation conditions of the preparation method of the present invention are simpler and the process is easier to control.

[0023] Preferably, the weight ratio of nickel nitrate to silica sol (water-soluble silica sol) is 1:(8.5-16.5). Within this range, the generated reaction product Ni3Si2O5(OH)4 / SiO2 has a more stable structure, better high-temperature sintering resistance after subsequent calcination, and can better meet the demand for high catalytic activity. When applied to catalytic reforming reactions, it can further promote a significant increase in the conversion rate of methane in the reforming reaction. In a preferred embodiment, the mass concentration of SiO2 in the silica sol is 20%-30%.

[0024] For the purpose of promoting a more complete and more stable reaction after adding silica sol into the nickel-ammine complex solution, the pH value of the nickel-ammine complex solution is 10-12.

[0025] Preferably, in step S2, the stirring reaction time is 6 to 12 hours. In this way, the completeness and stability of the reaction after adding silica sol to the nickel-ammine complex solution can be further improved, thereby making the structure of the reaction product Ni3Si2O5(OH)4 / SiO2 more stable, and better high-temperature stability can be obtained after subsequent calcination.

[0026] Based on the purpose of promoting better deamination effect after the reaction and obtaining a higher purity of the product Ni3Si2O5(OH)4 / SiO2, the temperature during the ammonia evaporation treatment is preferably 80°C to 95°C, and the pH value of the suspension after the ammonia evaporation treatment is 6 to 7. Based on the purpose of promoting better dehydration effect of the suspension after the reaction, the temperature during the drying treatment is preferably 100°C to 160°C and the time is 8 to 16 hours. In a preferred embodiment, before the drying treatment, step S2 also includes the step of washing the suspension after the ammonia evaporation treatment, and the suspension is washed three times with deionized water. This operation can further remove impurities in the suspension, and promote the Ni3Si2O5(OH)4 / SiO2 catalyst generated by the reaction to have a higher purity and a higher yield. The reaction product Ni3Si2O5(OH)4 / SiO2 is calcined to obtain a NiO / SiO2 catalyst, and the temperature during the calcination treatment is preferably 700 to 900°C and the time is 2 to 8 hours.

[0027] The present invention also provides a NiO / SiO2 catalyst, which is prepared by the above-mentioned method for preparing the NiO / SiO2 catalyst.

[0028] Based on the above reasons, the NiO / SiO2 catalyst of the present invention has higher catalytic activity. When the NiO / SiO2 catalyst prepared by the present invention is used to catalyze the reforming reaction of methane and carbon dioxide (reaction temperature is as high as 700-850°C), the catalytic activity is higher, and the conversion rate of methane in the reforming reaction can be greatly improved. In a preferred embodiment, the particle size of the NiO / SiO2 catalyst is 20-40 meshes.

[0029] The present invention also provides an application of a NiO / SiO2 catalyst in a reforming reaction of methane and carbon dioxide, wherein the NiO / SiO2 catalyst prepared by the above preparation method or the above NiO / SiO2 catalyst is subjected to hydrogen reduction activation treatment to obtain an activated catalyst, and then the activated catalyst is used to catalyze the reforming reaction of methane and carbon dioxide. In the reforming reaction, the reaction temperature is 700-850°C, and the mass space velocity of methane and carbon dioxide is independently 1.0-4.0h -1 , the molar ratio of methane and carbon dioxide is 1:(1.0~1.2).

[0030] Based on the above reasons, the NiO / SiO2 catalyst prepared by the present invention has a higher catalytic activity when used to catalyze the reforming reaction of methane and carbon dioxide (reaction temperature is as high as 700-850°C), which can greatly improve the conversion rate of methane in the reforming reaction. More preferably, the NiO / SiO2 catalyst prepared by the present invention is crushed to obtain a NiO / SiO2 catalyst with a particle size of 20-40 mesh, which is then used to catalyze the reforming reaction of methane and carbon dioxide, and the effect is better.

[0031] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0032] Example 1

[0033] 10.0g Ni(NO3)2·6H2O was dissolved in deionized water to obtain a nickel nitrate solution, and then ammonia water was added to form a nickel ammonia complex solution with a pH value of 11. 72.0g silica sol (SiO2 mass fraction 25%) was added to the nickel ammonia complex solution, and the suspension was stirred for 8 hours to obtain a suspension. The suspension was placed in a 90°C water bath for ammonia evaporation treatment, and the pH value of the suspension after ammonia evaporation treatment was 6. The suspension was washed three times with deionized water, and the suspension was placed at 120°C for 12 hours to obtain the reaction product Ni3Si2O5(OH)4 / SiO2. The reaction product Ni3Si2O5(OH)4 / SiO2 was calcined at 800°C for 4h to obtain a NiO / SiO2 catalyst. Among them, the weight ratio of Ni(NO3)2·6H2O and silica sol was 1:7.2.

[0034] Example 2

[0035] The only difference from Example 1 is that the amount of Ni(NO3)2·6H2O used is 7.0 g, and the weight ratio of Ni(NO3)2·6H2O to silica sol is 1:10.

[0036] Example 3

[0037] The only difference from Example 1 is that the amount of Ni(NO3)2·6H2O used is 13.0 g, and the weight ratio of Ni(NO3)2·6H2O to silica sol is 1:5.5.

[0038] Example 4

[0039] The only difference from Example 1 is that aqueous ammonia is added to form a nickel ammine complex solution with a pH value of 10.

[0040] Example 5

[0041] The only difference from Example 1 is that aqueous ammonia is added to form a nickel ammine complex solution with a pH value of 12.

[0042] Example 6

[0043] The only difference from Example 1 is that the amount of silica sol (SiO2 mass fraction 20%) used is 90.0 g, and the weight ratio of Ni(NO3)2·6H2O to silica sol is 1:9.

[0044] Example 7

[0045] The only difference from Example 1 is that the amount of silica sol (SiO2 mass fraction 30%) used is 60.0 g, and the weight ratio of Ni(NO3)2·6H2O to silica sol is 1:6.

[0046] Example 8

[0047] The only difference from Example 1 is that the drying time is 8 hours.

[0048] Example 9

[0049] The only difference from Example 1 is that the drying time is 16 h.

[0050] Example 10

[0051] The only difference from Example 1 is that the ammonia evaporation treatment temperature is 80° C. and the pH value of the suspension after the ammonia evaporation treatment is 7.

[0052] Embodiment 11

[0053] The only difference from Example 1 is that the ammonia evaporation treatment temperature is 95° C. and the pH value of the suspension after the ammonia evaporation treatment is 6.

[0054] Example 12

[0055] The only difference from Example 1 is that the drying temperature is 100°C.

[0056] Example 13

[0057] The only difference from Example 1 is that the calcination condition is 700° C. for 8 h.

[0058] Embodiment 14

[0059] The only difference from Example 1 is that the calcination condition is 900° C. for 2 h.

[0060] Embodiment 15

[0061] The only difference from Example 1 is that the amount of Ni(NO3)2·6H2O used is 20.0 g, and the weight ratio of Ni(NO3)2·6H2O to silica sol is 1:3.6.

[0062] Example 16

[0063] The only difference from Example 1 is the silica sol (SiO2 mass fraction is 40%).

[0064] Comparative Example 1

[0065] 10.0 g Ni(NO3)2·6H2O was dissolved in deionized water to form a nickel nitrate solution, which was then impregnated onto the carrier SiO2 by an equal volume impregnation method. After stirring, air drying, and drying at 120°C, the NiO / SiO2 catalyst was obtained by calcination.

[0066] Comparative Example 2

[0067] 10.0g Ni(NO3)2·6H2O was dissolved in deionized water to form a nickel nitrate solution, and then 72.0g silica sol (SiO2 mass fraction 25%) was added, and then 0.1mol / L NaOH solution was slowly added to the mixed liquid until the nickel nitrate was completely precipitated. The solution was washed with deionized water, dried at 120°C, and calcined to obtain a NiO / SiO2 catalyst.

[0068] Performance characterization:

[0069] Test method: The catalyst phase analysis was performed using a Shimadzu XRD-6000 rotating target X-ray diffractometer with a CuKα target, a voltage of 40 kV, a current of 30 mA, a scanning rate of 2° / min, and a scanning range of 10° to 70°.

[0070] Figure 1 The XRD spectrum of the reaction product Ni3Si2O5(OH)4 / SiO2 in Example 1 of the present invention is shown;

[0071] Figure 2 The XRD spectrum of the NiO / SiO2 catalyst in Example 1 of the present invention is shown.

[0072] The catalysts prepared in Examples 1 to 14 and Comparative Examples 1 and 2 were crushed into 20-40 meshes, and activated by hydrogen reduction to catalyze the reforming reaction of methane and carbon dioxide. The reaction temperature was 700-850°C, the reaction pressure was atmospheric pressure, and the mass space velocity of methane and carbon dioxide was 1.0-4.0h. -1 , the molar ratio of methane to carbon dioxide is 1:(1.0-1.2). The conversion rate of methane for each catalyst is listed in Table 1.

[0073] Table 1

[0074]

[0075]

[0076] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0077] It can be seen from the data of Examples 1 to 16 and Comparative Examples 1 and 2 that the NiO / SiO2 catalyst obtained by the preparation method of the present invention has better catalytic performance. The NiO / SiO2 catalyst prepared by the present invention has higher catalytic activity when used to catalyze the reforming reaction of methane and carbon dioxide (reaction temperature is as high as 700-850°C), and can always maintain a stable high catalytic activity in the reforming reaction, thereby greatly improving the conversion rate of methane in the reforming reaction. In particular, compared with the catalysts prepared by the impregnation method and the precipitation method in Comparative Examples 1 and 2, the NiO / SiO2 catalyst obtained by the preparation method of the present invention has a better catalytic effect, which can increase the methane conversion rate in the reforming reaction by 5% to 36%.

[0078] In particular, from the data comparison of Example 15 and Example 16 and Example 1, it can be seen that the weight ratio of nickel nitrate to silica sol (water-soluble silica sol) is 1: (8.5-16.5), and the mass concentration of SiO2 in silica sol is 20%-30%. Within this range, the generated reaction product Ni3Si2O5(OH)4 / SiO2 has a more stable structure, better high-temperature sintering resistance after subsequent calcination, and can better meet the needs of high catalytic activity. When applied to catalytic reforming reactions, it can further promote a significant increase in the conversion rate of methane in the reforming reaction.

[0079] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. Application of a NiO / SiO2 catalyst in the reforming reaction of methane and carbon dioxide, characterized in that: The NiO / SiO2 catalyst is subjected to hydrogen reduction activation treatment to obtain an activated catalyst; the activated catalyst is used to catalyze the reforming reaction of methane and carbon dioxide; wherein the NiO / SiO2 catalyst preparation method comprises the following steps: S1, adding ammonia water to the nickel nitrate solution to form a nickel ammonia complex solution; S2, adding silica sol to the nickel ammine complex solution, stirring and reacting to obtain a suspension; the weight ratio of the nickel nitrate to the silica sol is 1:(8.5-16.5); the mass concentration of SiO2 in the silica sol is 20%-30%; S3, subjecting the suspension to ammonia evaporation and drying treatments in sequence to obtain a reaction product Ni3Si2O5(OH)4 / SiO2, and subjecting the reaction product Ni3Si2O5(OH)4 / SiO2 to calcination treatment to obtain the NiO / SiO2 catalyst.

2. The use according to claim 1, characterized in that: The pH value of the nickel ammine complex solution is 10-12.

3. The use according to claim 1, characterized in that: In step S2, the stirring reaction time is 6 to 12 hours.

4. The use according to any one of claims 1 to 3, characterized in that During the ammonia evaporation treatment, the temperature is 80° C. to 95° C., and the pH value of the suspension after the ammonia evaporation treatment is 6 to 7.

5. The use according to claim 4, characterized in that: During the drying process, the temperature is 100° C. to 160° C. and the time is 8 to 16 hours.

6. The use according to claim 4, characterized in that: Before the drying process, step S2 also includes a step of washing the suspension after the ammonia evaporation process.

7. The use according to claim 4, characterized in that: During the calcination process, the temperature is 700-900° C. and the time is 2-8 hours.

8. The use according to claim 1, characterized in that: The particle size of the NiO / SiO2 catalyst is 20-40 meshes.

9. The use according to claim 1, characterized in that: During the reforming reaction, the reaction temperature is 700-850°C, and the mass space velocity of the methane and the carbon dioxide is independently 1.0-4.0 h -1 , the molar ratio of the methane to the carbon dioxide is 1:(1.0-1.2).

Citation Information

Patent Citations

  • Method for preparing nanometer Ni catalyst particles on Si substrate

    CN102500380A

  • Efficient methane and carbon dioxide reforming Ni / SiO2 catalyst and electrostatic spinning preparation method

    CN104511279A

  • Method for preparing bimodal mesoporous structure Ni / SiO2-ZrO2 catalyst used for partial oxidation of methane

    CN105363452A

  • Copper doped Ni / SiO2 nanocomposite catalyst and preparation method thereof