A method for determining 111 crystal orientation single crystal silicon crystal line

Through chemical etching and infrared beam specular reflection technology, the process of determining single crystal silicon crystal lines is simplified, solving the problems of complexity and high cost of existing methods, achieving efficient and convenient crystal line determination, and is suitable for mass production.

CN114875495BActive Publication Date: 2024-10-15NINGXIA ZHONGJING SEMICON MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210525353.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-18
Publication Date
2024-10-15
Estimated Expiration
2042-05-18

AI Technical Summary

Technical Problem

The existing method of determining single crystal silicon crystal lines is complex, resulting in increased processing costs and inconvenience in quickly determining crystal lines, making it difficult to meet the needs of mass production.

Method used

Chemical etching reagents are used to selectively etch the surface of single crystal silicon, and the mirror reflection of infrared beams is used to determine the position of the crystal lines. It is combined with light pattern testing and infrared projection technology to simplify the process and improve efficiency.

Benefits of technology

It realizes the rapid and convenient determination of single crystal silicon crystal lines, reduces processing costs, and is suitable for large-scale production needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114875495B_ABST
    Figure CN114875495B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for determining a 111 crystal orientation single crystal silicon crystal line, comprising the following steps: pre-configuring a chemical corrosion reagent, placing the tail section of the crystal rod in the chemical corrosion reagent for corrosion, so that pits appear on the surface of the single crystal, a proportioning method of the chemical corrosion reagent, pouring sodium hydroxide and pure water into the interior of a reactor, mixing and stirring, so that sodium hydroxide and pure water are mixed to generate an alkaline solution; pouring the prepared alkaline solution into the interior of a container, placing a hollow ring at the bottom of the container, placing the container on the top of an electric furnace, controlling the electric furnace to be powered on, the electric furnace heats the container, and the container heats the alkaline solution inside. The present invention has the advantages of high efficiency and convenience, and solves the problem that the current method for determining the single crystal silicon crystal line is not convenient for quickly determining the crystal line of the single crystal silicon, the determination process is complicated, and the processing cost of the single crystal silicon is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of single crystal silicon processing, and in particular to a method for determining single crystal silicon crystal lines with a 111 crystal orientation. Background Art

[0002] Single crystal silicon is a single crystal of silicon. It is a crystal with a basically complete lattice structure. Different directions have different properties. It is a good semiconductor material. Single crystal silicon has excellent physical, chemical, mechanical and semiconductor properties. Therefore, it is widely used as a basic material in the manufacturing process of large-scale integrated circuits, semiconductor devices and photovoltaic solar cells. Single crystal silicon is drawn from high-purity polycrystalline silicon in a single crystal furnace.

[0003] Processing workpiece of single crystal silicon rod: high-purity polysilicon is placed in a quartz crucible and continuously heated by a graphite heater surrounding it. The crucible rotates with the polysilicon melt, and a seed crystal is immersed in it. The pulling rod rotates with the seed crystal in the opposite direction, and slowly and vertically pulls it upward from the silicon melt. The molten polysilicon will stick to the bottom of the seed crystal and continue to grow in the direction of the seed crystal lattice arrangement. After being pulled out and cooled, it grows into a single crystal silicon rod with the same lattice direction as the seed crystal. When it is necessary to process a single crystal silicon rod into a round wafer, the single crystal rod will be cut into appropriate sizes, then ground to remove the uneven cut marks, and then use a chemical mechanical polishing process to make at least one side as smooth as a mirror. The wafer manufacturing is completed. When cutting the single crystal rod, it is necessary to mark the crystal line in advance and select a certain direction for slicing. This will reduce the slicing fragmentation rate, reduce the warping of the silicon wafer, reduce the surface stress of the silicon wafer, improve the slicing yield of the subsequent device, and improve the finished product rate. The current marking method is to use a corrosive liquid to corrode the marking surface of the crystal rod in advance, observe the corroded surface through a microscope, and mark the lines according to the observed defects.

[0004] The present invention uses a chemical etching agent to preferentially corrode the surface of the crystal, so that pits appear on the surface of the single crystal, and uses the mirror reflection of the laser beam to determine the position of the crystal line. The process is simple, the time is short, and the cost is low. In particular, the crystal line can be accurately found for the rolled crystal rod, thereby meeting the needs of large-scale production. Summary of the invention

[0005] The purpose of the present invention is to provide a method for determining the crystal lines of single crystal silicon with a 111 crystal orientation, which has the advantages of being efficient and convenient, and solves the problem that the current method for determining the crystal lines of single crystal silicon is not convenient for quickly determining the crystal lines of single crystal silicon, the determination process is complicated, and the processing cost of single crystal silicon is increased.

[0006] To achieve the above object, the present invention provides the following technical solution: a method for determining a 111 crystal orientation single crystal silicon crystal line, comprising the following steps:

[0007] 1) Pre-prepare a chemical etching reagent, place the tail section of the crystal rod in the chemical etching reagent for etching, so that pits appear on the surface of the single crystal, and mix the chemical etching reagent in a ratio of sodium hydroxide and pure water into a reactor, mix and stir, and mix the sodium hydroxide and pure water to generate an alkaline solution;

[0008] 2) pouring the prepared alkaline solution into the container, placing a hollow ring at the bottom of the container, placing the container on top of an electric furnace, controlling the electric furnace to be powered on, the electric furnace heats the container, and the container heats the alkaline solution inside;

[0009] 3) After heating is completed, the tail of the crystal rod is placed on a hollow ring, and the bottom of the crystal rod is immersed in the alkaline solution for 2 mm. The bottom of the crystal rod undergoes a chemical reaction in the alkaline solution. When bubbles are generated at the bottom of the crystal rod, the temperature is measured. The temperature of the alkaline solution and the temperature of the crystal rod head are measured using a temperature measuring gun. When the temperature of the alkaline solution is 105-115 degrees and the temperature of the crystal rod head is 60-70 degrees, the timing heating is started;

[0010] 4) After the heating time is up, take out the crystal rod from the container and observe the corrosion degree of the cross section at the bottom of the crystal rod. When the cross section becomes a micro-mirror surface, clean the alkali solution at the bottom of the crystal rod. When the cross section is not a micro-mirror surface, put it back into the container and continue to etch.

[0011] 5) After cleaning, the crystal direction and crystal deviation of the surface crystal rod are tested by optical imaging to accurately find the position of the crystal line. The observation requirement of the crystal line of the crystal rod is that there is no light in the room and the wall is bright and reflected. The crystal rod is fixed on the support frame, and the tail of the crystal rod is aligned with the infrared transmitter. The infrared transmitter is used to emit infrared rays for crystal line detection;

[0012] 6) When red light appears on the wall, observe the red light and observe the triangle based on infrared projection. The three vertices of the infrared projection triangle correspond to the three crystal lines of the crystal rod. Draw the crystal lines on the crystal rod, correspond the crystal lines at the tail of the crystal rod to the corresponding positions of the head of the crystal rod according to the markings, and draw the positions of the crystal lines on the head.

[0013] In order to facilitate uniform mixing of sodium hydroxide and pure water, as a method for determining 111 crystal orientation single crystal silicon crystal lines of the present invention, preferably, the mixing time in step 1) is 10-30 minutes.

[0014] In order to facilitate the control of the pH value of the alkaline solution, as a preferred method for determining 111 crystal orientation single crystal silicon crystal lines of the present invention, the ratio of sodium hydroxide to pure water in step 1) is 1:2.

[0015] In order to prevent the container and the hollow ring from being corroded by the alkaline solution, as a preferred method for determining 111 crystal orientation single crystal silicon crystal lines of the present invention, the materials of the container and the hollow ring in step 2) are both stainless steel.

[0016] In order to facilitate the alkaline solution to corrode the crystal rod, as a preferred method for determining 111 crystal orientation single crystal silicon crystal lines of the present invention, the heating temperature of the alkaline solution in step 2) is 400-500°C.

[0017] In order to facilitate etching the bottom of the crystal rod into a micro-mirror surface, as a preferred method for determining a 111 crystal orientation single crystal silicon crystal line of the present invention, the time for timing heating in the step 3) is 5-6 minutes.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The present invention determines the crystal lines of monocrystalline silicon by infrared rays, and has the advantages of being efficient and convenient, and solves the problem that the current method for determining the crystal lines of monocrystalline silicon is not convenient for rapid determination of the crystal lines of monocrystalline silicon, the determination process is complicated, and the processing cost of monocrystalline silicon is increased. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a schematic diagram of three crystal lines of a crystal rod displayed by infrared light of the present invention;

[0021] Figure 2 This is a schematic diagram of the crystal line marking at the tail of the crystal rod of the present invention. DETAILED DESCRIPTION

[0022] Example:

[0023] A method for determining a 111 crystal orientation single crystal silicon crystal line comprises the following steps:

[0024] 1) Pre-prepare a chemical etching reagent, place the tail section of the crystal rod in the chemical etching reagent for etching, so that pits appear on the surface of the single crystal, and mix the chemical etching reagent in a ratio of sodium hydroxide and pure water into a reactor, mix and stir, and mix the sodium hydroxide and pure water to generate an alkaline solution;

[0025] 2) pouring the prepared alkaline solution into the container, placing a hollow ring at the bottom of the container, placing the container on top of an electric furnace, controlling the electric furnace to be powered on, the electric furnace heats the container, and the container heats the alkaline solution inside;

[0026] 3) After heating is completed, the tail of the crystal rod is placed on a hollow ring, and the bottom of the crystal rod is immersed in the alkaline solution for 2 mm. The bottom of the crystal rod undergoes a chemical reaction in the alkaline solution. When bubbles are generated at the bottom of the crystal rod, the temperature is measured. The temperature of the alkaline solution and the temperature of the crystal rod head are measured using a temperature measuring gun. When the temperature of the alkaline solution is 105-115 degrees and the temperature of the crystal rod head is 60-70 degrees, the timing heating is started;

[0027] 4) After the heating time is up, take out the crystal rod from the container and observe the corrosion degree of the cross section at the bottom of the crystal rod. When the cross section becomes a micro-mirror surface, clean the alkali solution at the bottom of the crystal rod. When the cross section is not a micro-mirror surface, put it back into the container and continue to etch.

[0028] 5) After cleaning, the crystal direction and crystal deviation of the surface crystal rod are tested by optical imaging to accurately find the position of the crystal line. The observation requirement of the crystal line of the crystal rod is that there is no light in the room and the wall is bright and reflected. The crystal rod is fixed on the support frame, and the tail of the crystal rod is aligned with the infrared transmitter. The infrared transmitter is used to emit infrared rays for crystal line detection;

[0029] 6) When red light appears on the wall, observe the red light and observe the triangle based on infrared projection. The three vertices of the infrared projection triangle correspond to the three crystal lines of the crystal rod. Draw the crystal lines on the crystal rod, correspond the crystal lines at the tail of the crystal rod to the corresponding positions of the head of the crystal rod according to the markings, and draw the positions of the crystal lines on the head.

[0030] In this embodiment: the single crystal rod is corroded by a proportioned chemical etching solution, and the bottom of the single crystal rod is heated to make the bottom etching layer of the single crystal rod micro-mirror, which is convenient for subsequent light image testing. After the etching is completed, the single crystal rod is fixed, and the infrared generator is aimed at the tail of the single crystal rod to emit infrared rays, which can pass through the single crystal rod and be projected onto the wall. The three crystal lines of the single crystal rod are marked by the projected triangular picture.

[0031] As a technical optimization solution of the present invention, the mixing time in step 1) is 10-30 minutes.

[0032] In this embodiment, the mixing time of sodium hydroxide and pure water is 10-30 minutes, which can make the sodium hydroxide and pure water mix evenly.

[0033] As a technical optimization solution of the present invention, the ratio of sodium hydroxide to pure water in step 1) is 1:2.

[0034] In this embodiment, the ratio of sodium hydroxide to pure water is 1:2, which can facilitate the control of the pH value of the alkaline solution.

[0035] As a technical optimization solution of the present invention, in step 2), the materials of the container and the hollow ring are both stainless steel.

[0036] In this embodiment, the container and the hollow ring are made of stainless steel, which can prevent the container and the hollow ring from being damaged by alkaline solution.

[0037] As a technical optimization solution of the present invention, the heating temperature of the alkaline solution in step 2) is 400-500°C.

[0038] In this embodiment, the heating temperature of the alkaline solution is 400-500° C., which can increase the activity of the alkaline solution and quickly corrode the bottom of the single crystal rod.

[0039] As a technical optimization solution of the present invention, the time for timing heating in step 3) is 5-6 minutes.

[0040] In this embodiment, the timed heating time is 5-6 minutes, which can cause the bottom of the single crystal rod to be corroded into a microcrystalline surface.

[0041] To sum up: the method for determining the crystal lines of single crystal silicon with 111 crystal orientation determines the crystal lines of single crystal silicon by infrared rays, and has the advantages of high efficiency and convenience. It solves the problem that the current method for determining the crystal lines of single crystal silicon is not convenient for rapid determination of the crystal lines of single crystal silicon, the determination process is complicated, and the processing cost of single crystal silicon is increased.

Claims

1. A method for determining a 111 crystal orientation single crystal silicon crystal line, characterized in that: The following steps are involved: 1) Pre-prepare a chemical etching reagent, place the tail section of the crystal rod in the chemical etching reagent for etching, so that pits appear on the surface of the single crystal, and mix the chemical etching reagent in a ratio of sodium hydroxide and pure water into a reactor, mix and stir, and mix the sodium hydroxide and pure water to generate an alkaline solution; 2) pouring the prepared alkaline solution into the container, placing a hollow ring at the bottom of the container, placing the container on top of an electric furnace, controlling the electric furnace to be powered on, the electric furnace heats the container, and the container heats the alkaline solution inside; 3) After heating is completed, the tail of the crystal rod is placed on a hollow ring, and the bottom of the crystal rod is immersed in the alkaline solution for 2 mm. The bottom of the crystal rod undergoes a chemical reaction in the alkaline solution. When bubbles are generated at the bottom of the crystal rod, the temperature is measured. The temperature of the alkaline solution and the temperature of the crystal rod head are measured using a temperature measuring gun. When the temperature of the alkaline solution is 105-115 degrees and the temperature of the crystal rod head is 60-70 degrees, the timing heating is started; 4) After the heating time is up, take out the crystal rod from the container and observe the corrosion degree of the cross section at the bottom of the crystal rod. When the cross section becomes a micro-mirror surface, clean the alkali solution at the bottom of the crystal rod. When the cross section is not a micro-mirror surface, put it back into the container and continue to etch. 5) After cleaning, the crystal direction and crystal deviation of the surface crystal rod are tested by optical imaging to accurately find the position of the crystal line. The observation requirement of the crystal line of the crystal rod is that there is no light in the room and the wall is bright and reflected. The crystal rod is fixed on the support frame, and the tail of the crystal rod is aligned with the infrared transmitter. The infrared transmitter is used to emit infrared rays for crystal line detection; 6) When red light appears on the wall, observe the red light and observe the triangle according to infrared projection. The three vertices of the infrared projection triangle correspond to the three crystal lines of the crystal rod. Draw the crystal lines on the crystal rod. Match the crystal lines at the tail of the crystal rod to the corresponding positions of the head of the crystal rod according to the marks, and draw the positions of the crystal lines on the head; The mixing time in step 1) is 10-30 min; In the step 1), the ratio of sodium hydroxide to pure water is 1:2; In the step 2), the container and the hollow ring are made of stainless steel; The heating temperature of the alkaline solution in step 2) is 400-500° C.; The heating time in step 3) is 5-6 minutes.