A method for preparing a ZnO flexible film with high optical performance
By growing zinc oxide nanofilms on carbon fiber cloth using a two-step method, the problem of insufficient photoelectric performance of traditional zinc oxide films is solved, and high photoelectric response and stability are achieved, making it suitable for industrial applications.
Patent Information
- Application Number
- CN202210530642.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-16
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-05-16
AI Technical Summary
The photoelectric properties of traditional zinc oxide films are weak and need to be doped with other metal ions, which increases the cost and preparation complexity and limits large-scale production.
ZnO nanofilms rich in oxygen vacancies are grown on carbon fiber cloth through a two-step method. The first step is to calcine in a vacuum environment to form a seed layer. The second step is to grow the film under constant temperature hydrothermal conditions and adjust the oxygen vacancy concentration to improve photoelectrochemistry. performance.
The photocurrent, carrier concentration and light absorption are significantly increased, the electrochemical impedance is reduced, and a pure ZnO nanofilm with high photoelectric response and stability is formed, which is suitable for industrial production.
Smart Images

Figure CN114887614B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of optoelectronic functional materials, and in particular to a method for preparing a ZnO flexible film with high optical performance. Background Art
[0002] In recent years, nano zinc oxide materials have attracted widespread attention due to their non-toxic, high efficiency, and wide sources. Nano zinc oxide has high catalytic properties and is an important semiconductor photocatalyst. Zinc oxide thin films have both visible light transmittance and electrical conductivity. Traditional zinc oxide thin films have weak optoelectronic properties, so they usually need to be doped with other metal ions, but this undoubtedly increases the cost and the preparation process is also cumbersome, which is not conducive to large-scale production. Summary of the invention
[0003] In view of the shortcomings of the prior art, the present invention grows a ZnO nanofilm rich in oxygen vacancies on a carbon fiber cloth through a two-step method, has stronger photoelectrochemical properties, and has a simple preparation method.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] A method for preparing a ZnO flexible film with high optical performance comprises the following steps:
[0006] S1: Preparation of precursor solution
[0007] Weigh zinc acetate powder and dissolve it in a mixed solution of ethanol and ethanolamine; place it in a sealed beaker and heat it in a 60°C water bath with magnetic stirring for 3 hours, then take out the beaker and cool it to room temperature;
[0008] S2: Preparation of growth solution
[0009] Weigh zinc acetate powder, hexamethylenetetramine powder, and trisodium citrate dihydrate powder and dissolve them in deionized water until they are completely dissolved;
[0010] S3: immersing the carbon cloth washed with acetone in the precursor solution for 10 seconds and then pulling it out, and then calcining it at 200° C. for 2 hours in a vacuum environment to obtain a seed layer;
[0011] S4: placing the seed layer in the growth solution and growing it at a constant temperature of 95-100° C. for 3 hours to obtain a final product.
[0012] Furthermore, the mass volume ratio of zinc acetate powder, ethanol and ethanolamine in S1 is 1g:5ml:1ml.
[0013] Furthermore, the mass volume ratio of zinc acetate powder, hexamethylenetetramine powder, trisodium citrate dihydrate and deionized water in S2 is 2g:1.2-1.3g:0.1g:100ml.
[0014] In this paper, ultrathin ZnO nanosheets were synthesized on a flexible carbon cloth substrate by a two-step method. The oxygen vacancy concentration of the final ZnO sample was changed by the different annealing atmospheres of the seed layer in the first step. After 2h of hydrothermal growth in the second step, a high oxygen vacancy concentration of 286.5uA / cm 2 Photovoltaic properties. Compared with the traditional air seed layer annealing strategy, the photocurrent is significantly enhanced, up to 4.37 times. Compared with the hydrothermal growth of pure ZnO and the composite heterojunction containing ZnO under the same conditions (0V bias and 0.1M Na2SO4 concentration), the photocurrent value in this case is more significant. Due to the more oxygen vacancies, it has correspondingly stronger photoelectrochemical properties, and the photocurrent, carrier concentration, active catalytic area, and light absorption are significantly improved, the electrochemical impedance is reduced, and the migration of charge carriers is promoted.
[0015] The beneficial effects of the present invention are as follows: the present invention synthesizes a pure ZnO nanofilm with high photoelectric response and excellent stability, the raw materials are non-toxic and cheap, the preparation process is simple, the synthesis temperature is low, the preparation efficiency is high, the amount of the prepared product is large, and it is suitable for industrial production; the sample has a large specific surface area, has good photoelectric response performance under visible light, and the photocurrent continues to rise after illumination, and has broad prospects in industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 These are morphology pictures of the seed layer obtained in Examples 1 and 2 of the present invention and the final samples (a, A-ZnO-2h; b, V-ZnO-2h; c, ASL-2h; d, VSL-2h).
[0018] Figure 2 PL spectra of the final samples obtained in Examples 1 and 2 of the present invention.
[0019] Figure 3 This is the photocurrent diagram of the final sample obtained in Examples 1 and 2 of the present invention. DETAILED DESCRIPTION
[0020] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0022] Example 1
[0023] 1. Preparation of precursor solution
[0024] Weigh 6 g of zinc acetate powder and dissolve it in a mixed solution of 30 ml of ethanol and 6 ml of ethanolamine; place it in a sealed beaker and heat it at a constant temperature of 60°C in a water bath with magnetic stirring for 3 hours; take out the beaker and cool it to room temperature.
[0025] 2. Prepare growth medium
[0026] Weigh 2 g of zinc acetate powder, 1.26 g of hexamethylenetetramine powder, and 0.1 g of trisodium citrate dihydrate powder respectively, then dissolve all of them in 100 ml of deionized water and stir until they are completely dissolved.
[0027] 3. Preparation of ZnO flexible film
[0028] The carbon cloth was cut into a suitable size and cleaned in an ultrasonic cleaner with acetone, alcohol and deionized water for 10 minutes respectively. The cleaned carbon cloth was then dried in a constant temperature drying oven at 60°C. The dried carbon cloth was immersed in the precursor solution for 10 seconds and pulled out. The carbon cloth covered with the precursor solution was placed in a tube furnace at 200°C under vacuum conditions and calcined for 2 hours to obtain a seed layer, which was recorded as ASL-2h. After the calcination was completed, the seed layer was collected and placed in a pre-prepared growth solution, and grown at a constant temperature of 98°C for 3 hours to obtain the final sample, which was recorded as A-ZnO-2h.
[0029] Embodiment 2:
[0030] The same as Example 1, except that in step 3, the carbon coated with the precursor solution is placed in a tube furnace under air at 200° C. and calcined for 2 h to obtain a seed layer, which is denoted as VSL-2h. The final sample is calcined under the same conditions and is denoted as V-ZnO-2h.
[0031] Performance Test:
[0032] Figure 1The seed layers and final samples (a, A-ZnO-2h; b, V-ZnO-2h; c, ASL-2h; d, VSL-2h) obtained by annealing in different atmospheres in the present invention show that the morphologies of the two seed layers are not much different, and the morphologies of the final samples are not obviously different either, which shows that the difference in their photoelectric properties is not caused by the morphology.
[0033] Figure 2 The PL spectra of the two final samples obtained in the present invention are shown in Figure 1. The luminescence peak at 370 nm is caused by direct band excitation, and the luminescence intensity difference between the two is not large, while the photoluminescence peak at 580 nm is mainly caused by oxygen vacancies. It can be seen that V-ZnO-2h has a stronger luminescence peak here, indicating that it is rich in more oxygen vacancies. It can be determined that the difference in their photoelectric properties is mainly caused by the different oxygen vacancy concentrations.
[0034] Figure 3 This is the photocurrent diagram of the two final samples obtained in the present invention. It can be seen that V-ZnO-2h has a larger photocurrent, which shows that the ZnO sample rich in oxygen vacancies has better photoelectrochemical performance.
[0035] In summary, the final sample prepared by annealing the seed layer under vacuum conditions has better photoelectrochemical performance. This may be because the huge difference in photovoltaic performance is mainly due to the different Zn:O ratios at the interface between the seed and the growth layer, which leads to crystal plane mismatch. This study breaks the long-held view that the smaller the lattice mismatch between the ZnO seed layer and the growth layer, the better. From the above experimental steps, data and chart analysis, it can be seen that the present invention self-assembles pure ZnO nanofilm on a carbon cloth substrate through simple preparation steps. The nanofilm has good photoelectric response performance under visible light and stable performance, and is suitable for industrial applications.
[0036] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A method for preparing a ZnO flexible film with high optical performance, characterized in that: The steps include: S1: Preparation of precursor solution Weigh zinc acetate powder and dissolve it in a mixed solution of ethanol and ethanolamine; place it in a sealed beaker and heat it in a 60°C water bath with magnetic stirring for 3 hours, then take out the beaker and cool it to room temperature; S2: Preparation of growth solution Weigh zinc acetate powder, hexamethylenetetramine powder, and trisodium citrate dihydrate powder and dissolve them in deionized water until they are completely dissolved; S3: immersing the carbon cloth washed with acetone in the precursor solution for 10 seconds and then pulling it out, and then calcining it at 200° C. for 2 hours in a vacuum environment to obtain a seed layer; S4: placing the seed layer in the growth solution and growing it at a constant temperature of 95-100° C. for 3 hours to obtain a final product; Among them, the mass volume ratio of zinc acetate powder, ethanol and ethanolamine in S1 is 1g:5mL:1mL; the mass volume ratio of zinc acetate powder, hexamethylenetetramine powder, trisodium citrate dihydrate and deionized water in S2 is 2g:1.2-1.3g:0.1g:100mL.