A method for preparing porous biochar-based MnFe2O4 composite
By preparing porous biochar-based MnFe2O4 composites, the problem of MnFe2O4 catalysts easily agglomerating in water was solved, improving catalytic activity and antibiotic degradation efficiency, and realizing economical and efficient catalyst utilization.
Patent Information
- Application Number
- CN202210444812.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-04-26
AI Technical Summary
Existing MnFe2O4 catalysts tend to aggregate in water, have low utilization rates, and few surface active sites, making it difficult to efficiently catalyze the degradation of antibiotics.
Porous biochar was used as a carrier to prepare a porous biochar-based MnFe2O4 composite through co-pyrolysis and high-temperature and high-pressure hydrothermal reaction. The nitrogen-doped configuration of biochar was used to improve the separation efficiency of photogenerated electron and hole pairs and inhibit the aggregation of MnFe2O4.
It improves the dispersibility and catalytic activity of MnFe2O4, enhances the degradation efficiency of antibiotics, and is easy to recycle, thus reducing costs.
Smart Images

Figure CN114904536B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a MnFe2O4 composite, in particular to a method for preparing a porous biochar-based MnFe2O4 composite. Background Art
[0002] In recent years, due to the rapid development of agriculture and pharmaceutical factories, antibiotics have been frequently detected in rivers and drinking water. The latest research results show that antibiotics are difficult to degrade and can remain in the environment for a long time. Antibiotics in the water environment can cause an increase in antibiotic resistance genes in humans and animals, causing potential genetic pollution to the ecological environment. Today, the problem of antibiotic resistance has become one of the global public health issues.
[0003] Advanced oxidation technology (AOT) by activating peroxymonosulfate or peroxydisulfate has been widely used to remove antibiotics and has shown good performance. Reactive oxygen species (ROS) such as sulfate radicals and hydroxyl radicals can be formed in situ by ultraviolet light, transition metal activation, and thermal activation. Persulfate has higher stability and convenience than hydrogen peroxide in terms of storage and transportation. Although the persulfate activation method has the above advantages, persulfate-based AOT still has great disadvantages, such as high cost and possible toxicity of treated water. Sulfite, as a by-product of the flue gas desulfurization process, has been considered as a viable alternative in recent years. In addition, a variety of transition metals, including manganese, iron, and cobalt, have been applied to the activation of persulfate. Obviously, compared with cobalt, catalysts containing iron and manganese are lower in cost and toxicity, making them a better choice.
[0004] As a magnetic material, MnFe2O4 can be easily separated from aqueous solution under the action of an external magnetic field, providing an economical and effective method for practical application. However, due to the magnetic interaction between particles, magnetic nanoparticles tend to aggregate in water, which greatly reduces the catalytic activity. It is necessary to select a suitable carrier to improve the application performance of MnFe2O4.
[0005] The existing MnFe2O4 preparation method has the following disadvantages: low catalyst utilization, few surface active sites, and easy aggregation. Summary of the invention
[0006] Purpose of the invention: In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a porous biochar-based MnFe2O4 composite with a wide source and low cost.
[0007] Technical solution: The method for preparing a porous biochar-based MnFe2O4 composite according to the present invention comprises the following steps:
[0008] Step 1: washing the alfalfa with ultrapure water to remove surface impurities, drying, crushing, and sieving to obtain alfalfa powder of uniform size;
[0009] Step 2, after the alfalfa powder is mixed with the activator, it is placed in a tube furnace for co-pyrolysis reaction;
[0010] Step 3, cooling the mixture obtained in step 2 to room temperature, repeatedly washing with dilute hydrochloric acid and ultrapure water, and drying to obtain black powder biochar;
[0011] Step 4, placing the black powdered biochar in step 3 in ultrapure water for ultrasonic dispersion, then uniformly mixing it with FeCl3·6H2O and MnCl2·4H2O in a molar ratio of 2 to 4:1, adjusting the pH to alkaline, and performing a high temperature and high pressure hydrothermal reaction;
[0012] Step 5, washing the mixture after the reaction in step 4 with ultrapure water and ethanol in sequence, and vacuum drying to obtain a porous biochar-based MnFe2O4 composite.
[0013] Furthermore, in step 1, the nitrogen content of the alfalfa is 4-4.5 wt %. The drying is carried out in an oven at 80-110° C. for 12-24 hours, the grinding is carried out using a pulverizer, and the screening is carried out using a 20-40 mesh sieve.
[0014] Furthermore, in step 2, the activator is one or more of potassium hydroxide, calcium hydroxide, and sodium hydroxide. The activator is preferably a mixture of potassium hydroxide and calcium hydroxide, and the mass ratio thereof is 1 to 3:1, preferably 1:1. The mass ratio of alfalfa powder to the activator is 1:1 to 3. The co-pyrolysis reaction is carried out in a tubular furnace, the reaction atmosphere is nitrogen, the temperature is 500 to 800°C, the heating rate is 1 to 10°C / min, and the time is 1 to 10h.
[0015] Furthermore, in step 4, the ultrasonic dispersion time is 10 to 60 minutes, and the pH is adjusted to 11 to 13 with a 1M sodium hydroxide solution, preferably 12. The high temperature and high pressure hydrothermal reaction is carried out in a high temperature and high pressure autoclave, the reaction temperature is 150 to 200° C., and the reaction time is 2 to 24 hours.
[0016] Furthermore, in step 5, the drying temperature is 80-120°C and the drying time is 12-24 hours. The specific surface area of the porous biochar-based MnFe2O4 composite is 655-660m 2 / g, total pore volume is 0.7~0.8cm 3 / g.
[0017] Reaction principle: Mn, Fe, and O are easy to aggregate during the reaction process. Through the treatment of steps 2 to 4 of this application, they can be evenly dispersed. In the synergistic process of advanced oxidation and photocatalysis, the separation efficiency of photogenerated electrons and hole pairs is improved due to the presence of a large amount of nitrogen-doped configurations in biochar. Due to the pore size on the surface of biochar and the interface interaction between biochar and metal, it is not easy to aggregate.
[0018] Beneficial effects: Compared with the prior art, the present invention has the following significant features:
[0019] 1. The raw material for preparation is alfalfa, an agricultural waste, which has a wide source and low cost, and can fully reuse the waste. The co-activation of two different types of alkali is conducive to the generation of pores of different sizes, which is conducive to the mass transfer and adsorption of tetracycline;
[0020] 2. It is beneficial to improve the added value of alfalfa. By taking advantage of its rich nitrogen content, the biochar produced generates nitrogen-doped structures in situ, has a large specific surface area, graphite-like structure and hierarchical porous structure, and has a large adsorption capacity;
[0021] 3. The manganese and iron elements in MnFe2O4 can catalyze the persulfate reaction and be used to degrade antibiotics in wastewater; and MnFe2O4 is a magnetic material, which is easy to separate under the action of an external magnetic field and is easy to recycle and reuse;
[0022] 4. As a carrier of MnFe2O4, biochar can inhibit the aggregation of magnetic MnFe2O4, improve its dispersibility, accelerate the contact between pollutants and active sites, and improve the degradation efficiency. In the synergistic process of advanced oxidation and photocatalysis, the separation efficiency of photogenerated electrons and hole pairs is improved due to the presence of a large amount of nitrogen-doped configuration in biochar. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is the XRD spectrum of the present invention;
[0024] Figure 2 is a scanning electron microscope image of NBCs of Example 4 of the present invention;
[0025] Figure 3 This is a scanning electron microscope image of MnFe2O4;
[0026] Figure 4 is a scanning electron microscope image of the product obtained in Example 5 of the present invention;
[0027] Figure 5 is a N2 adsorption-desorption isotherm diagram of the products obtained in Examples 4 and 5 of the present invention;
[0028] Figure 6 is a pore size distribution diagram of the products obtained in Examples 4 and 5 of the present invention;
[0029] Figure 7 is a FTIR comparison chart of the material of Example 8 of the present invention before and after the adsorption of tetracycline, wherein a is the product obtained in Example 4, b is the product obtained in Example 6, c is the product obtained in Example 7, and d is the product obtained in Example 5;
[0030] Figure 8 is the adsorption kinetic curve of tetracycline by the material of Example 8 of the present invention, wherein a is the product obtained in Example 4, b is the product obtained in Example 6, c is the product obtained in Example 7, and d is the product obtained in Example 5;
[0031] Fig. 9 is the degradation kinetic curve of the material in Example 9 of the present invention and its control sample;
[0032] Fig.10 It is a comparison chart of pseudo-first-order degradation rate constants of the materials in Example 9 of the present invention. DETAILED DESCRIPTION
[0033] In the following examples, the nitrogen content of alfalfa is 4-4.5 wt%.
[0034] Example 1
[0035] A method for preparing a porous biochar-based MnFe2O4 composite comprises the following steps:
[0036] (1) The alfalfa was washed with ultrapure water to remove surface impurities, dried in an oven at 80° C. for 12 h, crushed with a grinder, and sieved with a 20-mesh sieve to obtain alfalfa powder of uniform size;
[0037] (2) 10 g of alfalfa powder was mixed with 10 g of activator potassium hydroxide, and then placed in a tube furnace for co-pyrolysis reaction for 1 h. The reaction atmosphere was nitrogen, the temperature was 500 °C, and the heating rate was 1 °C / min;
[0038] (3) cooling the mixture obtained in step (2) to room temperature, repeatedly washing with dilute hydrochloric acid and ultrapure water, and drying to obtain black powdered biochar;
[0039] (4) 0.05893 g of the black powdered biochar in step (3) was ultrasonically dispersed in ultrapure water for 10 to 60 minutes, then uniformly mixed with 0.1081 g of FeCl3·6H2O and 0.0396 g of MnCl2·4H2O, the pH was adjusted to 11 with a 1 M sodium hydroxide solution, and a high-pressure hydrothermal reaction was carried out in a high-temperature autoclave at 150° C. for 2 hours;
[0040] (5) The mixture after the reaction in step (4) was rinsed with ultrapure water and ethanol in sequence, and vacuum dried at 80-120° C. for 12 h to obtain a porous biochar-based MnFe2O4 composite.
[0041] The specific surface area of the porous biochar-based MnFe2O4 composite was 655.36 m 2 / g, and the total pore volume is 0.72cm 3 / g.
[0042] Example 2
[0043] A method for preparing a porous biochar-based MnFe2O4 composite comprises the following steps:
[0044] (1) The alfalfa was washed with ultrapure water to remove surface impurities, dried in an oven at 110° C. for 24 h, crushed with a grinder, and sieved with a 40-mesh sieve to obtain alfalfa powder of uniform size;
[0045] (2) 10 g of alfalfa powder was mixed with 30 g of an activator, which was 15 g of potassium hydroxide and 15 g of sodium hydroxide, and placed in a tubular furnace for co-pyrolysis reaction for 10 h in a nitrogen atmosphere at a temperature of 800 °C and a heating rate of 10 °C / min;
[0046] (3) cooling the mixture obtained in step (2) to room temperature, repeatedly washing with dilute hydrochloric acid and ultrapure water, and drying to obtain black powdered biochar;
[0047] (4) The black powdered biochar prepared in step (3) was ultrasonically dispersed in ultrapure water for 10 to 60 minutes, and then uniformly mixed with 0.2162 g of FeCl3·6H2O and 0.0396 g of MnCl2·4H2O, and the pH was adjusted to 13 with a 1 M sodium hydroxide solution, and a high pressure hydrothermal reaction was carried out at 200° C. in a high temperature autoclave for 24 hours;
[0048] (5) The mixture after the reaction in step (4) was rinsed with ultrapure water and ethanol in sequence, and vacuum dried at 80-120° C. for 24 h to obtain a porous biochar-based MnFe2O4 composite.
[0049] The specific surface area of the porous biochar-based MnFe2O4 composite was 659.76 m 2 / g, and the total pore volume is 0.79 cm 3 / g.
[0050] Example 3
[0051] A method for preparing a porous biochar-based MnFe2O4 composite comprises the following steps:
[0052] (1) The alfalfa was washed with ultrapure water to remove surface impurities, dried in an oven at 95°C for 18 h, crushed with a grinder, and sieved with a 40-mesh sieve to obtain alfalfa powder of uniform size;
[0053] (2) 10 g of alfalfa powder was mixed with 20 g of activator sodium hydroxide and placed in a tube furnace for co-pyrolysis reaction for 5 h in a nitrogen atmosphere at a temperature of 650 °C and a heating rate of 5 °C / min;
[0054] (3) cooling the mixture obtained in step (2) to room temperature, repeatedly washing with dilute hydrochloric acid and ultrapure water, and drying to obtain black powdered biochar;
[0055] (4) The black powdered biochar in step (3) was ultrasonically dispersed in ultrapure water for 10 to 60 minutes, then uniformly mixed with 0.1081 g of FeCl3·6H2O and 0.0396 g of MnCl2·4H2O, the pH was adjusted to 12 with a 1 M sodium hydroxide solution, and a high pressure hydrothermal reaction was carried out at 180° C. in a high temperature autoclave for 13 hours;
[0056] (5) The mixture after the reaction in step (4) was rinsed with ultrapure water and ethanol in sequence, and vacuum dried at 80-120° C. for 1 h to obtain a porous biochar-based MnFe2O4 composite.
[0057] The specific surface area of the porous biochar-based MnFe2O4 composite was 657.18 m 2 / g, with a total pore volume of 0.75 cm 3 / g.
[0058] Example 4
[0059] A method for preparing a porous biochar-based MnFe2O4 composite comprises the following steps:
[0060] (1) The alfalfa was washed with ultrapure water to remove surface impurities, dried in an oven at 100° C. for 12 h, crushed with a grinder, and sieved with a 20-mesh sieve to obtain alfalfa powder of uniform size;
[0061] (2) 10 g of alfalfa powder was mixed with 20 g of an activator, which was a mixture of 10 g of potassium hydroxide and 10 g of calcium hydroxide, and placed in a tube furnace for co-pyrolysis reaction for 1 h in a nitrogen atmosphere at a temperature of 700 °C and a heating rate of 8 °C / min;
[0062] (3) The mixture obtained in step (2) is cooled to room temperature, repeatedly washed with dilute hydrochloric acid and ultrapure water, and dried to obtain black powdered biochar, which is recorded as NBCs.
[0063] Depend on Figure 2It can be seen that NBCs have a smooth surface, many defect sites, and a well-developed pore structure.
[0064] Example 5
[0065] A method for preparing a porous biochar-based MnFe2O4 composite comprises the following steps:
[0066] (1) The alfalfa was washed with ultrapure water to remove surface impurities, dried in an oven at 100° C. for 12 h, crushed with a grinder, and sieved with a 20-mesh sieve to obtain alfalfa powder of uniform size;
[0067] (2) 10 g of alfalfa powder was mixed with 20 g of an activator, which was a mixture of 10 g of potassium hydroxide and 10 g of calcium hydroxide, and placed in a tube furnace for co-pyrolysis reaction for 1 h in a nitrogen atmosphere at a temperature of 700 °C and a heating rate of 8 °C / min;
[0068] (3) cooling the mixture obtained in step (2) to room temperature, repeatedly washing with dilute hydrochloric acid and ultrapure water, and drying to obtain black powdered biochar, denoted as NBCs;
[0069] (4) 0.117852 g of the black powdered biochar (NBCs) in step (3) was ultrasonically dispersed in ultrapure water for 20 minutes, then uniformly mixed with 0.10812 g of FeCl3·6H2O and 0.0396 g of MnCl2·4H2O, the pH was adjusted to 12 with a 1 M sodium hydroxide solution, and a high-pressure hydrothermal reaction was carried out at 180° C. in a high-temperature autoclave for 6 hours;
[0070] (5) The mixture after the reaction in step (4) was rinsed with ultrapure water and ethanol in sequence, and vacuum dried at 100° C. for 18 h to obtain a porous biochar-based MnFe2O4 composite, which was recorded as NBCs / MnFe2O4-2:1.
[0071] Figure 3 This is a scanning electron microscope image of conventional MnFe2O4, which is quasi-spherical with a small amount of rod-like and plate-like structures, with a diameter of 50-200nm. Figure 4 is a scanning electron microscope image of the MnFe2O4 composite obtained in this example. Figure 4 It can be seen that the final MnFe2O4 composite is a porous structure, NBCs are used as a carrier to load small-sized MnFe2O4 nanoparticles, and in NBCs / MnFe2O4, the morphology of NBCs and MnFe2O4 does not change significantly.
[0072] Figure 5 is the N2 adsorption-desorption isotherm diagram of the products obtained in Example 4 and Example 5. Figure 5It can be seen that: According to the IUPAC classification, both NBCs and NBCs / MnFe2O4 have type IV adsorption isotherms with obvious hysteresis loops, which proves that the prepared samples contain mesopores, which are conducive to the mass transfer of pollutants. When the relative pressure is less than 0.01, the adsorption volume increases sharply due to the presence of micropores in the sample.
[0073] Figure 6 is the pore size distribution diagram of the products obtained in Example 4 and Example 5. Figure 6 It can be seen that the sample contains both micropores and mesopores, which is consistent with the results of adsorption isotherm analysis.
[0074] Example 6
[0075] A method for preparing a porous biochar-based MnFe2O4 composite comprises the following steps:
[0076] (1) The alfalfa was washed with ultrapure water to remove surface impurities, dried in an oven at 100° C. for 12 h, crushed with a grinder, and sieved with a 20-mesh sieve to obtain alfalfa powder of uniform size;
[0077] (2) 10 g of alfalfa powder was mixed with 20 g of an activator, which was a mixture of 10 g of potassium hydroxide and 10 g of calcium hydroxide, and placed in a tube furnace for co-pyrolysis reaction for 1 h in a nitrogen atmosphere at a temperature of 700 °C and a heating rate of 8 °C / min;
[0078] (3) cooling the mixture obtained in step (2) to room temperature, repeatedly washing with dilute hydrochloric acid and ultrapure water, and drying to obtain black powdered biochar, denoted as NBCs;
[0079] (4) 0.058926 g of the black powdered biochar (NBCs) in step (3) was ultrasonically dispersed in ultrapure water for 20 minutes, then uniformly mixed with 0.10812 g of FeCl3·6H2O and 0.0396 g of MnCl2·4H2O, the pH was adjusted to 12 with a 1 M sodium hydroxide solution, and a high-pressure hydrothermal reaction was carried out at 180° C. in a high-temperature autoclave for 6 hours;
[0080] (5) The mixture after the reaction in step (4) was rinsed with ultrapure water and ethanol in sequence, and vacuum dried at 100° C. for 18 h to obtain a porous biochar-based MnFe2O4 composite, which was recorded as NBCs / MnFe2O4-1:1.
[0081] Example 7
[0082] A method for preparing a porous biochar-based MnFe2O4 composite comprises the following steps:
[0083] (1) The alfalfa was washed with ultrapure water to remove surface impurities, dried in an oven at 100° C. for 12 h, crushed with a grinder, and sieved with a 20-mesh sieve to obtain alfalfa powder of uniform size;
[0084] (2) 10 g of alfalfa powder was mixed with 20 g of an activator, which was a mixture of 10 g of potassium hydroxide and 10 g of calcium hydroxide, and placed in a tube furnace for co-pyrolysis reaction for 1 h in a nitrogen atmosphere at a temperature of 700 °C and a heating rate of 8 °C / min;
[0085] (3) cooling the mixture obtained in step (2) to room temperature, repeatedly washing with dilute hydrochloric acid and ultrapure water, and drying to obtain black powdered biochar, denoted as NBCs;
[0086] (4) 0.029463 g of the black powdered biochar (NBCs) in step (3) was ultrasonically dispersed in ultrapure water for 20 minutes, then uniformly mixed with 0.10812 g of FeCl3·6H2O and 0.0396 g of MnCl2·4H2O, the pH was adjusted to 12 with a 1 M sodium hydroxide solution, and a high-pressure hydrothermal reaction was carried out at 180° C. in a high-temperature autoclave for 6 hours;
[0087] (5) The mixture after the reaction in step (4) was rinsed with ultrapure water and ethanol in sequence, and vacuum dried at 100° C. for 18 h to obtain a porous biochar-based MnFe2O4 composite, which was recorded as NBCs / MnFe2O4-1:2.
[0088] The NBCs, NBCs / MnFe2O4-1:1, NBCs / MnFe2O4-1:2, and NBCs / MnFe2O4-2:1 obtained in Examples 4 to 7 were subjected to XRD tests, respectively. Figure 1 , it can be seen that the typical diffraction peak of pure MnFe2O4 is spinel phase, with high crystallinity, and no impurities are generated during the preparation process. For NBCs, there are characteristic diffraction peaks at 2θ=26.46° and 42.42°, which belong to the (0 0 2) plane and (1 0 0) plane of graphite, respectively. In addition, in the XRD spectrum of NBCs / MnFe2O4-2:1, the characteristic diffraction peaks of MnFe2O4 are located at 35.25° and 62.46°, respectively. These results show that NBCs / MnFe2O4 was successfully prepared.
[0089] Example 8
[0090] S1: Prepare 4 portions of 100 mL of 50 mg / L tetracycline solution in stoppered flasks;
[0091] S2: The NBCs, NBCs / MnFe2O4-1:1, NBCs / MnFe2O4-1:2, and NBCs / MnFe2O4-2:1 obtained in Examples 4 to 7 were placed in a magnetic water bath stirring pot at 25°C and 200 rpm under light-proof conditions, and samples were taken at specific time points (5 minutes, 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes, 80 minutes, 100 minutes, 120 minutes, 150 minutes, 180 minutes, 240 minutes, 300 minutes, 360 minutes, and 420 minutes)
[0092] S3: After sampling and centrifugation at 3000 rpm, the concentration of the supernatant was measured by UV-visible spectrophotometer.
[0093] The adsorption capacity of the material for tetracycline was calculated using the following equation:
[0094]
[0095] Where: V (L) represents the volume of tetracycline solution; C0 (mg / L) and C t (mg / L) represent the initial concentration and equilibrium concentration of tetracycline solution, respectively. m(g) represents the mass of biochar; Q t (mg / g) represents the adsorption of tetracycline by biochar. After calculating the adsorption kinetics, the pseudo-first-order kinetic model and pseudo-second-order kinetic model were used for simulation. The model equation is as follows:
[0096] Pseudo-first-order kinetic model:
[0097]
[0098] Pseudo-second-order kinetic model:
[0099]
[0100] In the formula, Q e is the equilibrium adsorption amount fitting value, unit is mg / g; Q t is the adsorption amount at time t, in mg / g; k1 is the pseudo-first-order adsorption rate constant, in min -1 ; k2 is the pseudo-secondary adsorption rate constant, unit: g·mg -1 ·min -1 .
[0101] from Figure 8 It can be seen that the pseudo-second-order kinetics can more accurately describe the adsorption kinetics experimental data, which means that the adsorption of TC on NBCs and NBCs / MnFe2O4 follows the chemical adsorption mechanism.
[0102] Example 9
[0103] S1: Prepare 7 portions of 30 mg / L tetracycline solution (100 mL) in stoppered flasks, and add 3 mmol of Na2SO3 to flasks No. 1, 2, 3, 4, 6, and 7;
[0104] S2: 10 mg of NBCs / MnFe2O4-1:1, NBCs / MnFe2O4-1:2, and NBCs / MnFe2O4-2:1 obtained in Examples 2-4 were placed in flasks 1-3 configured in S1, and 10 mg of MnFe2O4 was added to flasks 4 and 5. The mixture was placed in a magnetic water bath stirring pot at 25°C and 200 rpm, and flasks 1-6 were irradiated with ultraviolet light of 254 nm using a low-pressure mercury lamp. Samples were taken at specific time points (5 minutes, 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes, 80 minutes, 100 minutes, 120 minutes, 150 minutes, 180 minutes, 240 minutes, 300 minutes, 360 minutes, and 420 minutes).
[0105] S3: After sampling and centrifugation at 3000 rpm, the concentration of the supernatant was measured by UV-visible spectrophotometer.
[0106] from Figures 9-10 It can be seen that NBCs / MnFe2O4-2:1 has the best catalytic degradation effect on TC, and its rate constant is larger.
Claims
1. Application of a porous biochar-based MnFe2O4 composite in degrading tetracycline in wastewater, characterized in that: Prepare 100 mL of 30 mg / L tetracycline solution in a stoppered flask, add 3 mmol of Na2SO3 into the flask, take 10 mg of porous biochar-based MnFe2O4 composite into the flask, place it in a magnetic water bath stirring pot at 25 °C and 200 rpm, and use a low-pressure mercury lamp to irradiate the flask with ultraviolet light of a wavelength of 254 nm for degradation; The method for preparing the porous biochar-based MnFe2O4 composite comprises the following steps: Step 1: washing alfalfa with ultrapure water, drying, crushing, and sieving to obtain alfalfa powder of uniform size; the nitrogen content of the alfalfa is 4-4.5wt%; Step 2: After the alfalfa powder is mixed with an activator, a co-pyrolysis reaction is carried out; the activator is a mixture of potassium hydroxide and calcium hydroxide, and the mass ratio thereof is 1:1; the mass ratio of the alfalfa powder to the activator is 1:2; Step 3, cooling the mixture obtained in step 2 to room temperature, repeatedly washing with dilute hydrochloric acid and ultrapure water, and drying to obtain black powder biochar; Step 4, placing the black powdered biochar in step 3 in ultrapure water for ultrasonic dispersion, then uniformly mixing it with FeCl3•6H2O and MnCl2•4H2O in a molar ratio of 2:1, adjusting the pH to alkaline, and performing a high temperature and high pressure hydrothermal reaction; Step 5, washing the mixture after the reaction in step 4 with ultrapure water and ethanol in sequence, and vacuum drying to obtain a porous biochar-based MnFe2O4 composite; In the step 4, the ultrasonic dispersion time is 20 minutes, the pH is adjusted to 12 with a sodium hydroxide solution, and the high-temperature and high-pressure hydrothermal reaction is carried out in a high-temperature and high-pressure autoclave, the reaction temperature is 180° C., and the reaction time is 6 hours.
2. The use of a porous biochar-based MnFe2O4 composite in degrading tetracycline in wastewater according to claim 1, characterized in that: In the step 1, drying is performed in an oven at 100° C. for 12 hours, crushing is performed using a pulverizer, and sieving is performed using a 20-mesh sieve.
3. The use of a porous biochar-based MnFe2O4 composite in degrading tetracycline in wastewater according to claim 1, characterized in that: In the step 2, the co-pyrolysis reaction is carried out in a tubular furnace, the reaction atmosphere is nitrogen, the temperature is 700° C., the heating rate is 8° C. / min, and the time is 1 h.
4. The use of a porous biochar-based MnFe2O4 composite in degrading tetracycline in wastewater according to claim 1, characterized in that: In the step 5, the drying temperature is 100° C. and the drying time is 18 hours.